A composite deodorizing masterbatch and its application

Through the use of composite deodorant masterbatch, combined with porous polymer and component B with microporous-mesoporous-macroporous structure, the problem of insufficient adsorption capacity of existing deodorants for longer chain alkane molecules is solved. Efficient removal of volatile components and improvement of material properties are achieved.

CN114773638BActive Publication Date: 2024-10-29ANHUI XINGBEIDA NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110712932.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-25
Publication Date
2024-10-29
Estimated Expiration
2041-06-25

AI Technical Summary

Technical Problem

Existing deodorants are difficult to effectively remove unpleasant odors and irritating small-molecule organic compounds during the preparation process of polymer materials. In particular, they have poor adsorption capacity for alkane molecules with longer chain lengths, which affects air pollution and human health.

Method used

A composite deodorizing masterbatch is used, including component A and component B. Component A is composed of porous polymers and low boiling point components, and component B is composed of PEO-PPO-PEO, ethyl orthosilicate, 13X molecular sieve and It is composed of diatomaceous earth, which forms a microporous-mesoporous-macroporous network structure through specific proportions and modification treatments. It can be used with a vacuum device to improve the deodorizing effect.

Benefits of technology

It significantly improves the adsorption effect on volatile small molecules and larger molecular weight alkanes, reduces odor and volatile content, enhances the mechanical properties of the material, avoids closed pores and void collapse, and improves the odor removal effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003134367110000141
    Figure BDA0003134367110000141
  • Figure BDA0003134367110000151
    Figure BDA0003134367110000151
Patent Text Reader

Abstract

The present invention relates to the technical field of plastic deodorization, and in particular to a composite deodorization masterbatch and its application. The composite deodorization masterbatch comprises component A and component B, wherein the raw materials of component A comprise porous polymer and low boiling point component; the raw materials of component B comprise PEO-PPO-PEO, tetraethyl orthosilicate, 13X molecular sieve, and diatomaceous earth. The raw materials of the porous polymer comprise, by weight, 80-100 parts of pore opener, 80-100 parts of polymer resin, 5-7 parts of inorganic auxiliary agent, and 0.6-0.8 parts of surfactant. In the present invention, the processing process of the plastics using component A and component B is used for deodorization, the low boiling point component in component A can react with some volatile small molecules in the resin and then be taken away from the system, and component B can effectively adsorb some volatile molecules with larger molecular weight in the resin, and component B prepared by specific raw materials can better adsorb volatile molecules with larger molecular weight, especially alkanes and alkenes with longer carbon chains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic deodorization, and in particular to a composite deodorization masterbatch and application thereof. Background Art

[0002] With the development of polymer materials, especially the use of some medium and high polymer materials in car interiors has increased significantly, but these polymer materials will produce a very unpleasant odor during the preparation or modification process. After preparation, the polymer materials will also release some small molecular organic compounds, causing some unpleasant irritation and air pollution problems. These small molecular organic compounds will also affect human health. Therefore, people will add some deodorants when preparing this type of polymer materials, but these deodorants cannot achieve a good deodorizing effect.

[0003] Patent CN108192203B discloses a two-component deodorant, wherein the first deodorant is a foamed polyethylene masterbatch loaded with a liquid extractant having a boiling point of 80-100°C or a volatilization temperature of 90-180°C; the second deodorant described is a porous adsorbent loaded with a reactive deodorant. Although two components of the deodorant are used, the removal effect is average, mainly because the molecular sieve used has a poor adsorption capacity and is difficult to adsorb some alkane molecules with longer chain lengths. Summary of the invention

[0004] In order to better understand the technical content of the present invention, the following detailed description of the preferred implementation method of the present invention is provided.

[0005] In order to solve the above technical problems, the first aspect of the present invention provides a composite deodorizing masterbatch, including component A and component B, wherein the raw materials of component A include porous polymer and low boiling point component; the raw materials of component B include PEO-PPO-PEO, tetraethyl orthosilicate, 13X molecular sieve and diatomaceous earth.

[0006] In one embodiment, the weight ratio of the porous polymer to the low boiling point component is 1:(5-20); preferably 1:(8-15); and more preferably 1:12.

[0007] In one embodiment, the raw materials of the porous polymer include, by weight, 80-100 parts of a pore opener, 80-100 parts of a polymer resin, 5-7 parts of an inorganic auxiliary agent, and 0.6-0.8 parts of a surfactant.

[0008] In a preferred embodiment, the raw materials of the porous polymer include, by weight, 90 parts of a pore opener, 90 parts of a polymer resin, 6 parts of an inorganic auxiliary agent, and 0.7 parts of a surfactant.

[0009] In one embodiment, the polymer resin is selected from at least one of polyethylene, polypropylene, polystyrene, polycarbonate, polyurethane, and polytetrafluoroethylene, preferably polypropylene.

[0010] In one embodiment, the polypropylene comprises random polypropylene.

[0011] In a preferred embodiment, the melt flow rate of the random polypropylene at 230° C. and 2.16 kg is 0.1-0.5 g / 10 min, more preferably 0.15-0.3 g / 10 min, and even more preferably 0.2 g / 10 min.

[0012] In one embodiment, the random polypropylene is Hyosung R200P.

[0013] In a preferred embodiment, the polypropylene further comprises high melt strength polypropylene; the weight of the high melt strength polypropylene is 10-20% of the weight of the polypropylene, preferably 15%.

[0014] In a preferred embodiment, the high melt strength polypropylene has a melt flow rate of 20-30 g / 10 min at 230° C. and 2.16 kg, more preferably 26 g / 10 min.

[0015] In one embodiment, the high melt strength polypropylene is purchased from Shanghai Secco with a brand number of k7926.

[0016] In the present invention, the porous polymer prepared by the synergistic effect of a specific amount of high melt strength polypropylene and a specific random polypropylene has better voids. The synergistic effect of the two has higher tensile ductility and more uniform and stable pores can be obtained during the pore opening process.

[0017] In one embodiment, the inorganic auxiliary agent is selected from at least one of attapulgite, montmorillonite, oxide whiskers and bernettite.

[0018] In a preferred embodiment, the inorganic additives are attapulgite and oxide whiskers.

[0019] In one embodiment, the weight ratio of the attapulgite to the oxide whiskers is (4.3-8):1; preferably (5.2-6):1; and more preferably 5.4:1.

[0020] In one embodiment, the attapulgite is used after being modified, and the modification method is: ultrasonicating the attapulgite in acetic acid for 20-40 minutes, then adding a silane coupling agent and ultrasonicating for 40-50 minutes, and then filtering and drying to obtain the obtained product.

[0021] In one embodiment, the weight ratio of the attapulgite to the silane coupling agent is 100:(1.2-3); preferably 100:(1.5-2); and more preferably 100:1.8.

[0022] In one embodiment, the average particle size of the attapulgite is 200-600 mesh; preferably 300-400 mesh; more preferably 325 mesh.

[0023] In one embodiment, the attapulgite is purchased from Lingshou County Lingxin Mineral Products Processing Plant.

[0024] In one embodiment, the oxide whiskers are selected from at least one of magnesium oxide whiskers, silicon oxide whiskers, and zinc oxide whiskers.

[0025] In a preferred embodiment, the oxide whiskers are zinc oxide whiskers.

[0026] In a preferred embodiment, the zinc oxide whisker is used after being modified, and the modification method is: ultrasonically treating the zinc oxide whisker in an aqueous solution with a pH value of 5 for 20-40 minutes, then adding a silane coupling agent and ultrasonically treating the whisker for 40-50 minutes, filtering, drying, and activating at 110-130° C. for 10-15 hours to obtain the obtained product.

[0027] In one embodiment, the weight ratio of the zinc oxide whisker to the silane coupling agent is 100:(3.5-6); preferably 100:(4-5); and more preferably 100:4.5.

[0028] In one embodiment, the zinc oxide whiskers have an average diameter of 0.5-1 um and a length of 10-20 um.

[0029] In a preferred embodiment, the zinc oxide whiskers have an average diameter of 0.8 μm and a length of 15 μm.

[0030] In one embodiment, the zinc oxide whiskers are purchased from Hangzhou Jikang New Materials Co., Ltd.

[0031] The silane coupling agent used in the modified attapulgite and zinc oxide whiskers is the same.

[0032] In one embodiment, the silane coupling agent includes a silane coupling agent containing an epoxy group, including but not limited to KH560 silane coupling agent.

[0033] In order to increase the pore-making effect, the applicant added a certain amount of high melt strength polypropylene to the system, but found that the addition of high melt strength polypropylene would produce closed-cell phenomenon. The applicant unexpectedly found that the use of a specific amount of zinc oxide whiskers in the present invention can solve the defects caused by high melt strength polypropylene. This may be because the zinc oxide whiskers can be inserted into the polymer resin matrix from four directions, can resist decomposition and external forces, thereby avoiding the occurrence of closed-cell phenomenon; at the same time, it may be because the zinc oxide whiskers can support the matrix resin well from four directions. When the low boiling point component is injected under a lower pressure, the void collapse phenomenon will not occur. The low boiling point component can be better injected into the void. When using component A, the low boiling point component can better produce azeotropy with the volatile system and be taken away from the system, thereby reducing the odor.

[0034] In one embodiment, the surfactant is an anionic surfactant and / or a cationic surfactant.

[0035] In a preferred embodiment, the surfactant is an anionic surfactant and a cationic surfactant.

[0036] In one embodiment, the weight ratio of the anionic surfactant to the cationic surfactant is (1.5-3):1; preferably (1.8-2.3):1; and more preferably 2:1.

[0037] In one embodiment, the anionic surfactant is selected from at least one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium hexadecyl sulfate, and sodium octadecyl sulfate, preferably sodium hexadecyl sulfate.

[0038] In one embodiment, the cationic surfactant is at least one of hexadecyltrimethylammonium bromide, octadecyldimethylbenzylquaternary ammonium chloride, and dodecyltrimethylammonium bromide, preferably dodecyltrimethylammonium bromide.

[0039] The pores of some existing polypropylene materials are not very uniform. In the present invention, a uniform porous polymer can be obtained. The addition of a small amount of surfactant in the system may also be one of the reasons for obtaining uniform porosity. On the one hand, it may be because the surfactant can better disperse the attapulgite and zinc oxide whiskers modified by the silane coupling agent to be epoxy group to form a good dispersion system, and then continuously nucleate the attapulgite and zinc oxide whiskers in the system to form uniform and dense bubbles. Then the surfactant can reduce the surface tension of the foam, which is more conducive to the formation of uniform pores. On the other hand, it may be because the addition of specific anionic and cationic surfactants can reduce the crystallinity and particle size of polypropylene, thereby increasing its surface area and pore volume.

[0040] In one embodiment, the pore opening agent is composed of water, n-pentane, isopentane, and isopropanol.

[0041] In one embodiment, the weight ratio of water, pentane and isopropanol is 20:(6-9):(2-3)(0.5-0.8); preferably 20:8:2.5:0.6.

[0042] In one embodiment, the low boiling point component comprises water.

[0043] In a preferred embodiment, the low boiling point component further includes an organic solvent with a boiling point below 200°C.

[0044] The type of organic solvent and the ratio of organic solvent to water can be selected as required.

[0045] In a preferred embodiment, the organic solvent is 2-methyl-2-butanol.

[0046] In a preferred embodiment, the water accounts for (20-30)% by weight of the low boiling point components, preferably 27.5%.

[0047] The deodorizing masterbatch of the present invention is mainly used for deodorizing in the production or modification process of PP. The applicant has found through a large number of experiments that the use of a specific proportion of water and 2-methyl-2-butanol as low-boiling point components in the present invention can better remove the volatile components in PP. This may be because the specific proportion of water and 2-methyl-2-butanol can produce a co-boiling with the volatile components in PP, especially can produce an azeotropic reaction with 2,4-dimethylheptane, and remove some volatile components.

[0048] In one embodiment, the method for preparing the porous polymer comprises the following steps:

[0049] (1) mixing the polymer resin and the inorganic additive in a high-speed mixer and transferring the mixture into a twin-screw extruder to melt and granulate at 210-230° C. to obtain granules A;

[0050] (2) mixing granular material A with a pore-opening agent and a surfactant, stirring the mixture at 100° C. for 6-7 hours, and then cooling the mixture to obtain a mixture B;

[0051] (3) The solid obtained after filtering the mixed material B is dried with an electric blower, and then heated at 175-180° C. for 40-50 seconds to open the pores, thereby obtaining a porous polymer.

[0052] After the porous polymer is prepared, component A is prepared by taking corresponding weight portions of the porous polymer and the low boiling point component.

[0053] In one embodiment, the preparation method of component A is: placing a porous polymer in a container at -1 MPa, and then injecting a low boiling point component into the container to obtain component A.

[0054] In a preferred embodiment, the raw materials of component B include, by weight, 1-4 parts of PEO-PPO-PEO, 10-20 parts of tetraethyl orthosilicate, 50-80 parts of 13X molecular sieve, and 75-90 parts of diatomaceous earth.

[0055] In a more preferred embodiment, the raw materials of component B include, by weight, 2-3 parts of PEO-PPO-PEO, 12-15 parts of tetraethyl orthosilicate, 60-68 parts of 13X molecular sieve, and 80-86 parts of diatomaceous earth.

[0056] In a more preferred embodiment, the raw materials of component B include, by weight, 2.5 parts of PEO-PPO-PEO, 14 parts of tetraethyl orthosilicate, 63 parts of 13X molecular sieve, and 83 parts of diatomaceous earth.

[0057] PEO-PPO-PEO is a triblock copolymer of polyethylene oxide-polypropylene oxide-polyethylene oxide.

[0058] The source of the PEO-PPO-PEO is not limited, and the purchasing manufacturers include but are not limited to Shanghai Yanxin Materials Co., Ltd.

[0059] In one embodiment, the 13X molecular sieve is a 13X activated molecular sieve.

[0060] In one embodiment, the average particle size of the 13X active molecular sieve is 300-400 mesh, preferably 325 mesh.

[0061] In one embodiment, the 13X active molecule is purchased from Zhengzhou Tianxiang Inorganic Materials Co., Ltd.

[0062] In one embodiment, the specific surface area of ​​the diatomaceous earth is 50-60m 2 / g, pore volume is 0.6-0.8cm3 / g, and pore radius is 2000-4000nm.

[0063] In one embodiment, the diatomaceous earth is purchased from Changbai Korean Autonomous County Tianbao Diatomaceous Earth Functional Products Co., Ltd.

[0064] In one embodiment, diatomaceous earth is modified before use, and the modification method is: calcining the diatomaceous earth at 400-500°C for 1-1.5h, adding it to a 50-60% hydrochloric acid aqueous solution after cooling it to room temperature, soaking it for 6-8h, and then drying it to constant weight.

[0065] In one embodiment, the preparation method of component B comprises the following steps:

[0066] (1) stirring the modified diatomaceous earth and molecular sieve in an ethanol solution for 4-6 hours, and then standing for 30-35 hours to obtain material A;

[0067] (2) discarding the supernatant of material A to obtain material B;

[0068] (3) drying material B to constant weight to obtain material C;

[0069] (4) Grinding material C and passing it through a 400-600 mesh sieve to obtain material D;

[0070] (5) dissolving tetraethyl orthosilicate in water to obtain solution E, wherein the concentration of solution E is 0.01-0.02 mol / L;

[0071] (6) PEO-PPO-PEO was added to solution E and mixed evenly, and hydrochloric acid was added dropwise to adjust the pH value to 5-6 to obtain solution F;

[0072] (7) Add material D to solution F, stir for 8-9 hours, and evaporate the water to obtain solid G;

[0073] (8) The solid G is dried at 120-130°C for 8-10 h and then transferred to a muffle furnace at 500-600°C for drying for 7-8 h to obtain component B.

[0074] The use of component A in the present invention can effectively remove some volatile components in the PP production process, but it is poor for some longer-chain alkanes. The applicant has found that the use of component B in the present application can effectively adsorb longer-chain alkanes. This may be because diatomaceous earth has a larger pore size, and 13X molecular sieve has a mesoporous structure. Then, micropores and mesopores are generated through the joint action of PEO-PPO-PEO and tetraethyl orthosilicate, so that component B has a micropore-mesopore-macroporous interpenetrating network structure, which is not only conducive to the adsorption of volatile components, but also can accelerate the diffusion and transportation of volatile components in the gaps, achieving a better deodorization and removal of volatile components.

[0075] The second aspect of the present invention provides an application of a composite deodorizing masterbatch, wherein the composite deodorizing masterbatch is used for deodorizing in a thermoplastic plastic preparation process.

[0076] The thermoplastics include but are not limited to polyethylene, polypropylene, polystyrene, and polycarbonate, and are particularly suitable for deodorizing polypropylene plastics.

[0077] When the composite deodorizing masterbatch is used, the addition amount of component A and component B is selected according to the needs. The weight ratio of component A to component B can be 1:1, 1:2, or other weight ratios.

[0078] When using composite deodorizing masterbatch for deodorization, it is necessary to use it in conjunction with a vacuum device. The vacuum device can be turned on during all processing time periods, or it can be turned on during the early processing time periods. You can choose according to your needs.

[0079] The main beneficial effects of the present invention are:

[0080] 1. In the present invention, component A and component B are used together in the plastic processing process to deodorize. The low boiling point component in component A can react with some volatile small molecules in the resin, and then these volatile small molecules are taken out of the system in conjunction with a vacuum device. At the same time, component B can effectively adsorb some volatile molecules with larger molecular weight in the resin. Component B prepared from specific raw materials can better adsorb volatile molecules with larger molecular weight, especially alkanes and alkenes with longer carbon chains;

[0081] 2. Adding high melt strength polypropylene and surfactant increases the uniformity of the pores, and the surfactant can increase the adsorption of component A to the small molecule volatile system to a certain extent;

[0082] 3. The addition of zinc oxide whiskers solves the shortcoming that high melt strength polypropylene may form a closed-cell structure, while increasing the stability of the pores. At the same time, the synergistic effect with attapulgite increases the deodorization effect, which may be because the two can increase the adsorption of component A on the small molecule volatile system to a certain extent, thereby removing some volatile small molecules;

[0083] 4. Component A and component B not only will not affect the performance of resin products, but can also increase the mechanical properties of the resin to a certain extent. DETAILED DESCRIPTION

[0084] Specific embodiments of the present invention are given below, but the present invention is not limited by the embodiments.

[0085] In addition, unless otherwise specified, the raw materials in the present invention can be obtained from commercial sources.

[0086] Example 1

[0087] A composite deodorizing masterbatch, comprising component A and component B;

[0088] The raw materials of component A include porous polymer and low boiling point component; the weight ratio of the porous polymer to the low boiling point component is 1:8; the raw materials of the porous polymer include, by weight, 80 parts of pore opening agent, 80 parts of polymer resin, 5 parts of inorganic auxiliary agent, and 0.6 parts of surfactant;

[0089] The polymer resin is polypropylene; the polypropylene includes random polypropylene; the melt flow rate of the random polypropylene at 230°C and 2.16kg is 0.2g / 10min; the random polypropylene is Korea Hyosung R200P; the polypropylene also includes high melt strength polypropylene; the weight of the high melt strength polypropylene is 10% of the weight of the polypropylene; the melt flow rate of the high melt strength polypropylene at 230°C and 2.16kg is 26g / 10min; the high melt strength polypropylene is purchased from Shanghai Saike, with the brand name k7926;

[0090] The inorganic auxiliary agents are attapulgite and oxide whiskers; the weight ratio of the attapulgite to the oxide whiskers is 5.2:1; the attapulgite is used after being modified, and the modification method is: ultrasonicating the attapulgite in acetic acid for 20 minutes, then adding a silane coupling agent and ultrasonicating for 40 minutes, filtering and drying to obtain the obtained product; the weight ratio of the attapulgite to the silane coupling agent is 100:1.5; the average particle size of the attapulgite is 325 meshes; the attapulgite is purchased from Lingshou County Lingxin Mineral Products Processing Plant; the oxide whiskers are zinc oxide whiskers; the zinc oxide whiskers are modified The modified method is as follows: the zinc oxide whisker is ultrasonically treated in an aqueous solution with a pH value of 5 for 20 minutes, and then a silane coupling agent is added and ultrasonically treated for 40 minutes, filtered, dried, and activated at 110°C for 15 hours; the weight ratio of the zinc oxide whisker to the silane coupling agent is 100:4; the average diameter of the zinc oxide whisker is 0.5um and the length is 10um; the zinc oxide whisker is purchased from Hangzhou Jikang New Materials Co., Ltd.; the silane coupling agent used for the modified attapulgite and the zinc oxide whisker is the same; the silane coupling agent is KH560 silane coupling agent;

[0091] The surfactant is an anionic surfactant and a cationic surfactant; the weight ratio of the anionic surfactant to the cationic surfactant is 1.8:1; the anionic surfactant is sodium hexadecyl sulfate; the cationic surfactant is dodecyltrimethylammonium bromide;

[0092] The pore opening agent is composed of water, n-pentane, isopentane and isopropanol; the weight ratio of water, pentane and isopropanol is 20:6:2:0.5;

[0093] The low boiling point component includes water; the low boiling point component also includes an organic solvent with a boiling point lower than 200°C; the organic solvent is 2-methyl-2-butanol; the water accounts for 20% by weight of the low boiling point component;

[0094] The preparation method of the porous polymer comprises the following steps: (1) mixing a polymer resin and an inorganic additive in a high-speed mixer, and then transferring the mixture into a twin-screw extruder to melt and granulate at 210° C. to obtain a granule A; (2) mixing the granule A with a pore-opening agent and a surfactant, and then stirring the mixture at 100° C. for 6 hours, and then cooling the mixture to obtain a mixed material B; (3) filtering the mixed material B, and drying the solid obtained by using an electric blower, and then heating the mixture at 175° C. for 50 seconds to open the pores, to obtain a porous polymer;

[0095] After the porous polymer is prepared, corresponding weight portions of the porous polymer and the low boiling point component are taken to prepare component A; the preparation method of component A is as follows: the porous polymer is placed in a container at -1MPa, and then the low boiling point component is injected into the container to obtain component A;

[0096] The raw materials of component B include, by weight, 2 parts of PEO-PPO-PEO, 12 parts of tetraethyl orthosilicate, 60 parts of 13X molecular sieve, and 80 parts of diatomaceous earth;

[0097] The PEO-PPO-PEO was purchased from Shanghai Yanxin Materials Co., Ltd.

[0098] The 13X molecular sieve is a 13X active molecular sieve; the average particle size of the 13X active molecular sieve is 325 mesh; the 13X active molecular sieve is purchased from Zhengzhou Tianxiang Inorganic Materials Co., Ltd.;

[0099] The specific surface area of ​​the diatomaceous earth is 50m 2 / g, pore volume of 0.6cm3 / g, pore radius of 2000nm; the diatomite was purchased from Tianbao Diatomite Functional Products Co., Ltd., Changbai Korean Autonomous County; the diatomite was modified and then used, and the modification method was: calcining the diatomite at 400°C for 1h, adding it to a 50% hydrochloric acid aqueous solution after cooling it to room temperature, soaking it for 6h, and then drying it to constant weight;

[0100] The preparation method of component B comprises the following steps: (1) stirring the modified diatomaceous earth and molecular sieve in an ethanol solution for 4-6 hours, and then standing for 30 hours to obtain material A; (2) discarding the supernatant of material A to obtain material B; (3) drying material B to constant weight to obtain material C; (4) grinding material C and passing it through a 400-mesh sieve to obtain material D; (5) dissolving tetraethyl orthosilicate in water to obtain solution E, wherein the solution of solution E is 0.01 mol / L; (6) adding PEO-PPO-PEO to solution E and mixing evenly, and then dropping hydrochloric acid to adjust the pH value to 5 to obtain solution F; (7) adding material D to solution F and stirring for 8 hours, and then evaporating the water to obtain solid G; (8) drying solid G at 120-130° C. for 8 hours, and then transferring it to a muffle furnace at 500° C. and drying it for 8 hours to obtain component B.

[0101] Example 2

[0102] A composite deodorizing masterbatch, comprising component A and component B;

[0103] The raw materials of component A include porous polymer and low boiling point component; the weight ratio of the porous polymer to the low boiling point component is 1:15; the raw materials of the porous polymer include, by weight, 100 parts of pore opening agent, 100 parts of polymer resin, 7 parts of inorganic auxiliary agent, and 0.8 parts of surfactant;

[0104] The polymer resin is polypropylene; the polypropylene includes random polypropylene; the melt flow rate of the random polypropylene at 230°C and 2.16kg is 0.2g / 10min; the random polypropylene is Korea Hyosung R200P; the polypropylene also includes high melt strength polypropylene; the weight of the high melt strength polypropylene is 20% of the weight of the polypropylene; the melt flow rate of the high melt strength polypropylene at 230°C and 2.16kg is 26g / 10min; the high melt strength polypropylene is purchased from Shanghai Secco, with the brand name k7926;

[0105] The inorganic additives are attapulgite and oxide whiskers; the weight ratio of the attapulgite to the oxide whiskers is 6:1; the attapulgite is used after being modified, and the modification method is: ultrasonicating the attapulgite in acetic acid for 40 minutes, then adding a silane coupling agent and ultrasonicating for 50 minutes, filtering and drying to obtain the obtained product; the weight ratio of the attapulgite to the silane coupling agent is 100:2; the average particle size of the attapulgite is 325 meshes; the attapulgite is purchased from Lingshou County Lingxin Mineral Products Processing Plant; the oxide whiskers are zinc oxide whiskers; the zinc oxide whiskers are modified The modified method is as follows: the zinc oxide whisker is ultrasonically treated in an aqueous solution with a pH value of 5 for 40 minutes, and then a silane coupling agent is added and ultrasonically treated for 50 minutes, filtered, dried, and activated at 130°C for 10 hours; the weight ratio of the zinc oxide whisker to the silane coupling agent is 100:5; the average diameter of the zinc oxide whisker is 1um and the length is 20um; the zinc oxide whisker is purchased from Hangzhou Jikang New Materials Co., Ltd.; the silane coupling agent used for the modified attapulgite and the zinc oxide whisker is the same; the silane coupling agent is KH560 silane coupling agent;

[0106] The surfactant is an anionic surfactant and a cationic surfactant; the weight ratio of the anionic surfactant to the cationic surfactant is 2.3:1; the anionic surfactant is sodium hexadecyl sulfate; the cationic surfactant is dodecyltrimethylammonium bromide;

[0107] The pore opening agent is composed of water, n-pentane, isopentane and isopropanol; the weight ratio of water, pentane and isopropanol is 20:9:3:0.8;

[0108] The low boiling point component includes water; the low boiling point component also includes an organic solvent with a boiling point lower than 200°C; the organic solvent is 2-methyl-2-butanol; the water accounts for 30% of the weight of the low boiling point component;

[0109] The preparation method of the porous polymer comprises the following steps: (1) mixing a polymer resin and an inorganic additive in a high-speed mixer, and then transferring the mixture into a twin-screw extruder to melt and granulate at 230° C. to obtain a granule A; (2) mixing the granule A with a pore-opening agent and a surfactant, and stirring the mixture at 100° C. for 7 hours, and then cooling the mixture to obtain a mixed material B; (3) filtering the mixed material B, and drying the solid obtained by using an electric blower, and then heating the mixture at 180° C. for 40 seconds to open the pores, to obtain a porous polymer;

[0110] After the porous polymer is prepared, corresponding weight portions of the porous polymer and the low boiling point component are taken to prepare component A; the preparation method of component A is as follows: the porous polymer is placed in a container at -1MPa, and then the low boiling point component is injected into the container to obtain component A;

[0111] The raw materials of component B include, by weight, 3 parts of PEO-PPO-PEO, 15 parts of tetraethyl orthosilicate, 68 parts of 13X molecular sieve, and 86 parts of diatomaceous earth;

[0112] PEO-PPO-PEO was purchased from Shanghai Yanxin Materials Co., Ltd.;

[0113] The 13X molecular sieve is a 13X active molecular sieve; the average particle size of the 13X active molecular sieve is 325 mesh; the 13X active molecular sieve is purchased from Zhengzhou Tianxiang Inorganic Materials Co., Ltd.;

[0114] The specific surface area of ​​the diatomaceous earth is 60m 2 / g, pore volume of 0.8cm3 / g, pore radius of 4000nm; the diatomite was purchased from Tianbao Diatomite Functional Products Co., Ltd., Changbai Korean Autonomous County; the diatomite was modified and then used, and the modification method was: calcining the diatomite at 500°C for 1h, adding it to a 60% hydrochloric acid aqueous solution after cooling it to room temperature, soaking it for 8h, and then drying it to constant weight;

[0115] The preparation method of component B comprises the following steps: (1) stirring the modified diatomaceous earth and molecular sieve in an ethanol solution for 6 hours, and then standing for 35 hours to obtain material A; (2) discarding the supernatant of material A to obtain material B; (3) drying material B to constant weight to obtain material C; (4) grinding material C and passing it through a 600-mesh sieve to obtain material D; (5) dissolving tetraethyl orthosilicate in water to obtain solution E, wherein the solution of solution E is 0.02 mol / L; (6) adding PEO-PPO-PEO to solution E and mixing evenly, then dropping hydrochloric acid to adjust the pH value to 6 to obtain solution F; (7) adding material D to solution F and stirring for 9 hours, then evaporating the water to obtain solid G; (8) drying solid G at 130° C. for 10 hours, and then transferring it to a muffle furnace at 600° C. and drying it for 7 hours to obtain component B.

[0116] Example 3

[0117] A composite deodorizing masterbatch, comprising component A and component B, wherein the raw materials of component A comprise a porous polymer and a low boiling point component; the weight ratio of the porous polymer to the low boiling point component is 1:12; the raw materials of the porous polymer comprise, by weight, 90 parts of a pore opener, 90 parts of a polymer resin, 6 parts of an inorganic auxiliary agent, and 0.7 parts of a surfactant;

[0118] The polymer resin is polypropylene; the polypropylene includes random polypropylene; the melt flow rate of the random polypropylene at 230°C and 2.16kg is 0.2g / 10min; the random polypropylene is Korea Hyosung R200P; the polypropylene also includes high melt strength polypropylene; the weight of the high melt strength polypropylene is 15% of the weight of the polypropylene; the melt flow rate of the high melt strength polypropylene at 230°C and 2.16kg is 26g / 10min; the high melt strength polypropylene is purchased from Shanghai Secco, with the brand name k7926;

[0119] The inorganic auxiliary agents are attapulgite and oxide whiskers; the weight ratio of the attapulgite to the oxide whiskers is 5.4:1; the attapulgite is used after being modified, and the modification method is: ultrasonicating the attapulgite in acetic acid for 30 minutes, then adding a silane coupling agent and ultrasonicating for 45 minutes, filtering and drying to obtain the obtained product; the weight ratio of the attapulgite to the silane coupling agent is 100:1.8; the average particle size of the attapulgite is 325 meshes; the attapulgite is purchased from Lingshou County Lingxin Mineral Products Processing Plant; the oxide whiskers are zinc oxide whiskers; the zinc oxide whiskers are modified The modified method is as follows: the zinc oxide whisker is ultrasonicated in an aqueous solution with a pH value of 5 for 30 minutes, and then a silane coupling agent is added to ultrasonicate for 45 minutes, filtered, dried, and activated at 120°C for 12 hours; the weight ratio of the zinc oxide whisker to the silane coupling agent is 100:4.5; the average diameter of the zinc oxide whisker is 0.8m and the length is 15um; the zinc oxide whisker is purchased from Hangzhou Jikang New Materials Co., Ltd.; the silane coupling agent used for the modified attapulgite and the zinc oxide whisker is the same; the silane coupling agent is KH560 silane coupling agent;

[0120] The surfactant is an anionic surfactant and a cationic surfactant; the weight ratio of the anionic surfactant to the cationic surfactant is 2:1; the anionic surfactant is sodium hexadecyl sulfate; the cationic surfactant is dodecyltrimethylammonium bromide;

[0121] The pore opening agent is composed of water, n-pentane, isopentane and isopropanol; the weight ratio of water, pentane and isopropanol is 20:8:2.5:0.6;

[0122] The low boiling point component includes water; the low boiling point component also includes an organic solvent with a boiling point lower than 200°C; the organic solvent is 2-methyl-2-butanol; the water accounts for 27.5% by weight of the low boiling point component;

[0123] The preparation method of the porous polymer comprises the following steps: (1) mixing a polymer resin and an inorganic additive in a high-speed mixer, and then transferring the mixture into a twin-screw extruder to melt and granulate at 220° C. to obtain a granule A; (2) mixing the granule A with a pore-opening agent and a surfactant, and stirring the mixture at 100° C. for 6.5 hours, and then cooling the mixture to obtain a mixed material B; (3) filtering the mixed material B, and drying the solid obtained by using an electric blower, and then heating the mixture at 176° C. for 45 seconds to open the pores, to obtain a porous polymer;

[0124] After the porous polymer is prepared, corresponding weight portions of the porous polymer and the low boiling point component are taken to prepare component A; the preparation method of component A is as follows: the porous polymer is placed in a container at -1MPa, and then the low boiling point component is injected into the container to obtain component A;

[0125] The raw materials of component B include, by weight, 2.5 parts of PEO-PPO-PEO, 14 parts of tetraethyl orthosilicate, 63 parts of 13X molecular sieve, and 83 parts of diatomaceous earth;

[0126] PEO-PPO-PEO was purchased from Shanghai Yanxin Materials Co., Ltd.;

[0127] The 13X molecular sieve is a 13X active molecular sieve; the average particle size of the 13X active molecular sieve is 325 mesh; the 13X active molecular sieve is purchased from Zhengzhou Tianxiang Inorganic Materials Co., Ltd.;

[0128] The specific surface area of ​​the diatomaceous earth is 55m 2 / g, pore volume of 0.7cm3 / g, pore radius of 3000nm; the diatomite was purchased from Tianbao Diatomite Functional Products Co., Ltd., Changbai Korean Autonomous County; the diatomite was modified and then used, and the modification method was: calcining the diatomite at 450°C for 1.2h, adding it to a 55% hydrochloric acid aqueous solution after cooling it to room temperature, soaking it for 7h, and then drying it to constant weight;

[0129] The preparation method of component B comprises the following steps: (1) stirring the modified diatomaceous earth and molecular sieve in an ethanol solution for 5 hours, and then standing for 32 hours to obtain material A; (2) discarding the supernatant of material A to obtain material B; (3) drying material B to constant weight to obtain material C; (4) grinding material C and passing it through a 500-mesh sieve to obtain material D; (5) dissolving tetraethyl orthosilicate in water to obtain solution E, wherein the solution of solution E is 0.015 mol / L; (6) adding PEO-PPO-PEO to solution E and mixing evenly, and then dropping hydrochloric acid to adjust the pH value to 5 to obtain solution F; (7) adding material D to solution F and stirring for 8.5 hours, and then evaporating the water to obtain solid G; (8) drying solid G at 125° C. for 9 hours, and then transferring it to a muffle furnace at 550° C. for drying for 7.5 hours to obtain component B.

[0130] Example 4

[0131] A composite deodorizing masterbatch, comprising component A and component B, wherein the raw materials of component A comprise a porous polymer and a low boiling point component; the weight ratio of the porous polymer to the low boiling point component is 1:12; the raw materials of the porous polymer comprise, by weight, 90 parts of a pore opener, 90 parts of a polymer resin, 6 parts of an inorganic auxiliary agent, and 0.7 parts of a surfactant;

[0132] The polymer resin is the same as that in Example 3;

[0133] The inorganic auxiliary agent is attapulgite; the attapulgite is used after being modified, and the modification method is: ultrasonicating the attapulgite in acetic acid for 30 minutes, then adding a silane coupling agent and ultrasonicating for 45 minutes, filtering and drying to obtain the obtained product; the weight ratio of the attapulgite to the silane coupling agent is 100:1.8; the average particle size of the attapulgite is 325 meshes; the attapulgite is purchased from Lingshou County Lingxin Mineral Products Processing Plant; the silane coupling agent is KH560 silane coupling agent;

[0134] The surfactant is the same as in Example 3; the pore opener is the same as in Example 3; the low boiling point component is the same as in Example 3; the preparation method of the porous polymer is the same as in Example 3; and the component B is the same as in Example 3.

[0135] Example 5

[0136] A composite deodorizing masterbatch comprises component A and component B, wherein component A is the same as that in Example 3; and component B is the diatomaceous earth in Example 3.

[0137] Example 6

[0138] A composite deodorizing masterbatch comprises component A and component B, wherein component A is the same as that in Example 3; and component B is the 13X molecular sieve in Example 3.

[0139] Performance Testing

[0140] Sample preparation: The composite deodorizing masterbatch prepared in the embodiment was added to a modified PP formula, wherein the modified PP formula is, by weight, 30 parts of homopolymer PP with a weight average molecular weight of 500, 0.8 parts of antioxidant 1010, 0.3 parts of calcium stearate, 1 part of white carbon black, 28 parts of alkali-free glass fiber with a length of 2 mm and a diameter of 12 microns, 0.2 parts of KH550 coupling agent, and composite deodorizing masterbatch (component A 2 parts, component B 4 parts); after the raw materials in the formula are evenly mixed in a high-speed mixer, they are placed in a co-rotating twin-screw extruder for extrusion granulation. A vacuum device is connected during the extrusion process, and the vacuum degree of the vacuum device is -0.8 MPa. After the extruder discharge is cooled for 1 hour, a sample is obtained.

[0141] 1. Odor level test

[0142] The odor level was determined using the odor level test method of VW'S PV 3900E of the German Volkswagen Company. The level description is shown in Table 1.

[0143] Table 1

[0144] level describe 1 Can't feel 2 Feel it, don't disturb 3 Noticeable but not intrusive 4 Disturb 5 Strong plan

[0145] Collect the semi-ziplock bags (the size of the ziplock bags is No. 8, and the weight of the samples in the ziplock bags is the same), and then let 10 experimenters in the laboratory take the materials to smell, and then score them according to the odor level standard and take the average value.

[0146] 2. Volatile content test

[0147] Test method: Place a weighing bottle with a lid in an oven at 110°C for 1 hour, take it out and put it in a desiccator to cool to room temperature, weigh it accurately to 0.0005g, take 5g of the extruded sample and spread it evenly on the bottom of the weighing bottle, then weigh it accurately to 0.0005g, then place it in an oven at 110°C, take it out after 1 hour, put it in a desiccator to cool to room temperature, weigh it accurately to 0.0005g, then place it in an oven at 110°C, take it out after 1 hour, and do the same operation until the sample is constant weight. The difference between two consecutive weighing results is no more than 0.0005g, and then calculate the volatile content. The calculation formula is: Volatile content (%) = (sample weight before heating - sample weight after heating) / sample weight before heating * 100.

[0148] Evaluation criteria: Volatile content less than or equal to 0.2% is Class A; volatile content between 0.2-0.4% is Class B; volatile content greater than or equal to 0.4% is Class C.

[0149] The test results are shown in Table 2:

[0150] Table 2

[0151]

[0152]

Claims

1. A composite deodorizing masterbatch, comprising component A and component B, characterized in that: The raw materials of component A include porous polymer and low boiling point component; the raw materials of component B include, by weight, 1-4 parts of PEO-PPO-PEO, 10-20 parts of tetraethyl orthosilicate, 50-80 parts of 13X molecular sieve, and 75-90 parts of diatomaceous earth; The weight ratio of the porous polymer to the low boiling point component is 1:(5-20); The raw materials of the porous polymer include, by weight, 80-100 parts of a pore opening agent, 80-100 parts of a polymer resin, 5-7 parts of an inorganic auxiliary agent, and 0.6-0.8 parts of a surfactant; The polymer resin is polypropylene; The inorganic auxiliary agent is selected from at least one of attapulgite, montmorillonite, oxide whiskers and bernhardtite; The surfactant is an anionic surfactant and / or a cationic surfactant; The pore opening agent is composed of water, n-pentane, isopentane and isopropanol; The method for preparing the porous polymer comprises the following steps: (1) mixing the polymer resin and the inorganic additive in a high-speed mixer and transferring the mixture into a twin-screw extruder to melt and granulate at 210-230° C. to obtain granules A; (2) mixing granular material A with a pore-opening agent and a surfactant, stirring the mixture at 100° C. for 6-7 hours, and then cooling the mixture to obtain a mixture B; (3) drying the solid obtained after filtering the mixture B with an electric blower, and then heating at 175-180° C. to open the pores for 40-50 seconds to obtain a porous polymer; The low boiling point component includes water and 2-methyl-2-butanol; the water accounts for (20-30)% by weight of the low boiling point component; the preparation method of component A is: placing a porous polymer in a container at -1MPa, and then injecting the low boiling point component into the container to obtain component A; The preparation method of component B comprises the following steps: (1) stirring the modified diatomaceous earth and molecular sieve in an ethanol solution for 4-6 hours, and then standing for 30-35 hours to obtain material A; (2) discarding the supernatant of material A to obtain material B; (3) drying material B to constant weight to obtain material C; (4) Grinding material C and passing it through a 400-600 mesh sieve to obtain material D; (5) dissolving tetraethyl orthosilicate in water to obtain solution E, wherein the concentration of solution E is 0.01-0.02 mol / L; (6) PEO-PPO-PEO was added to solution E and mixed evenly, and hydrochloric acid was added dropwise to adjust the pH value to 5-6 to obtain solution F; (7) Add material D to solution F, stir for 8-9 hours, and evaporate the water to obtain solid G; (8) drying solid G at 120-130° C. for 8-10 h and then transferring it to a muffle furnace at 500-600° C. for drying for 7-8 h to obtain component B; The diatomite is modified before use. The modification method is as follows: calcining the diatomite at 400-500° C. for 1-1.5 hours, cooling it to room temperature, adding it into a 50-60% hydrochloric acid aqueous solution, soaking it for 6-8 hours, and then drying it to constant weight.

2. An application of a composite deodorizing masterbatch according to claim 1, characterized in that: The composite deodorizing masterbatch is used for deodorizing in the process of preparing thermoplastic plastics.

Citation Information

Patent Citations

  • Low-odor glass fiber reinforced polypropylene composite material and its preparation method

    CN108192203B

  • Odor adsorption type functional master batch and preparation method thereof as well as automotive interior polypropylene composite material composed of odor adsorption type functional master batch

    CN108178878A

  • Polypropylene odor adsorption master batch for automobiles and preparation method of master batch

    CN109096598A