Corrosion-resistant low-voltage cable and preparation method thereof
By using specific materials and processes to prepare a corrosion-resistant sheath layer for low-voltage cables, the problems of insufficient heat resistance and poor water resistance of the sheath material under high-temperature conditions are solved, achieving halogen-free flame retardancy and rodent-proof effects, and improving the overall performance of the cable.
Patent Information
- Application Number
- CN202410952506.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing sheath materials of low-voltage cables have insufficient heat resistance under high temperature conditions, and do not have halogen-free flame retardant and waterproof properties, making them susceptible to being chewed, which leads to a decrease in protective performance.
The corrosion-resistant low-voltage cable is manufactured using an inner and outer semi-conductive shielding layer made of ethylene-vinyl acetate copolymer, an insulation layer made of cross-linked polyethylene, and a metal shielding layer made of aluminum conductive metal strip. The sheath layer uses a corrosion-resistant sheath material composed of polyvinyl chloride, flame retardant additives, impact modifiers, coupling agents, etc., and is prepared through a specific process.
It improves the cable's high temperature resistance, flame retardancy, water resistance, and rodent resistance, meets the requirements for halogen-free flame retardancy, and enhances the overall performance of the cable.
Smart Images

Figure CN118919149A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of cables, and in particular, relates to a corrosion-resistant low-voltage cable and a preparation method thereof. Background Art
[0002] Wires and cables are conductors covered with insulation, shielding, and protective layers used to transmit electricity or signal current or signal voltage. Low-voltage cables are a type of wire and cable. They are widely used in low-voltage power distribution systems because of their reliable operation, no need for poles, no need to occupy the ground, and no obstruction of appearance. Polyvinyl chloride is a commonly used sheath material for wires and cables. In actual use, it is found that its high-temperature resistance is insufficient, which is not conducive to the use of cables under high temperature conditions. In order to make the cable sheath material have excellent impact strength, acrylic copolymers are usually used to modify it. However, acrylic copolymers have a certain hydrophilicity, which is not conducive to the waterproof performance of the cable sheath material. In addition, polyvinyl chloride-based sheath materials do not have halogen-free flame retardant properties, which do not meet the green environmental protection and halogen-free flame retardant index requirements of cable materials.
[0003] The sheath layer made of cable sheath material is located on the outer layer of the cable, which is easily eaten by rats, insects and ants, resulting in a decrease in the protective performance of the sheath layer. Adding rodent repellent to the cable sheath material will produce toxic and harmful substances that are not conducive to environmental protection and human health. Therefore, a suitable method is needed to modify the cable sheath material, and improve the comprehensive performance of the cable such as high temperature resistance, rodent resistance, flame retardancy and waterproofness by improving the performance of the sheath material. Summary of the invention
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A corrosion-resistant low-voltage cable, comprising, from the inside out, a wire core, an inner semi-conductive shielding layer, an insulating layer, an outer semi-conductive shielding layer, a metal shielding layer and a sheath layer, wherein the wire core is located in the innermost layer, the outer periphery of the wire core is extruded with the inner semi-conductive shielding layer; the outer periphery of the inner semi-conductive shielding layer is extruded with the insulating layer; the outer periphery of the insulating layer is extruded with the outer semi-conductive shielding layer; the outer periphery of the outer semi-conductive shielding layer is provided with a metal shielding layer; the outer periphery of the metal shielding layer is extruded with the sheath layer;
[0006] The wire core is a plurality of twisted copper wires; the inner semi-conductive shielding layer and the outer semi-conductive shielding layer are both made of ethylene-vinyl acetate copolymer material; the insulating layer is made of cross-linked polyethylene insulating material; the metal shielding layer is obtained by spirally wrapping an aluminum conductive metal tape around the outer semi-conductive shielding layer;
[0007] The sheath layer is made of a corrosion-resistant sheath material, which includes the following raw materials in parts by weight: 50-60 parts of polyvinyl chloride, 40-50 parts of flame retardant additives, 25-35 parts of impact modifiers, 0.8-1.0 parts of coupling agents, 1.5-2 parts of antioxidants, 25-30 parts of plasticizers, 2-4 parts of crosslinking agents, 8-10 parts of accelerators, 1-3 parts of crosslinking additives, 10-15 parts of magnesium oxide, and 5-10 parts of zinc oxide;
[0008] The coupling agent is KH560, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, the plasticizer is epoxidized soybean oil, the crosslinking agent is diisopropylbenzene peroxide, the accelerator is accelerator DM, and the crosslinking aid is triallyl isocyanurate;
[0009] The preparation of the corrosion-resistant low-voltage cable comprises the following steps:
[0010] Step S1: Put polyvinyl chloride and impact modifier into a torque rheometer, mix for 10 minutes, heat to 90°C, add flame retardant, coupling agent, antioxidant, plasticizer, magnesium oxide and zinc oxide into the torque rheometer for mixing, heat to 130°C after 25 minutes, add crosslinking agent, accelerator and crosslinking aid, and continue mixing for 10 minutes to prepare corrosion-resistant sheath material;
[0011] Step S2: use an extruder to extrude and deposit the inner semi-conductive shielding layer on the periphery of the wire core, and then extrude and deposit an insulating layer on the periphery of the inner semi-conductive shielding layer; then extrude and deposit the outer semi-conductive shielding layer on the periphery of the insulating layer; then wrap an aluminum conductive metal belt around the periphery of the outer semi-conductive shielding layer in a spiral form to obtain a metal shielding layer; finally, extrude and deposit a corrosion-resistant sheath material on the periphery of the metal shielding layer to obtain a sheath layer, and anneal after extrusion to obtain a corrosion-resistant low-voltage cable.
[0012] The flame retardant auxiliary agent is prepared by the following steps:
[0013] Step A1: Add cinnamic acid and DOPO into a flask, start stirring, raise the temperature to 125-135°C, and stir at constant temperature for 3-4 hours to obtain a reaction product;
[0014] Furthermore, the dosage ratio of cinnamic acid and DOPO is 0.1 mol:0.1 mol;
[0015] During the reaction of step A1, DOPO adds to the carbon-carbon double bond of cinnamic acid to obtain a reaction product;
[0016] Step A2: Add 3,4-dihydroxycinnamamide, epichlorohydrin and tetraethylammonium chloride into a flask, start stirring, heat to 75-85°C, reflux and stir for 1 hour, slowly add sodium hydroxide solution dropwise, continue to reflux and stir for 2-2.5 hours, cool to room temperature, add benzene into the flask, slowly add sodium hydroxide solution dropwise, reflux and stir for 2-2.5 hours, wash with distilled water, and distill under reduced pressure to obtain an epoxy product;
[0017] Furthermore, the total amount of 3,4-dihydroxycinnamic acid amide, epichlorohydrin, tetraethylammonium chloride, sodium hydroxide solution and benzene are in a ratio of 0.1 mol: 0.2 mol: 0.001-0.002 mol: 85-95 mL: 110-130 mL; the concentration of the sodium hydroxide solution is 0.25-0.30 mol / L, and the volume ratio of the sodium hydroxide solution added twice is 1:1;
[0018] During the reaction of step A2, under the action of tetraethylammonium chloride as a phase transfer catalyst, the phenolic hydroxyl group of 3,4-dihydroxycinnamamide is firstly ring-opened with epichlorohydrin, and the obtained alcoholic hydroxyl group is then ring-closed with chlorine in a sodium hydroxide solution to obtain an epoxy product;
[0019] Step A3: In a nitrogen atmosphere, add the reaction product and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10 hours to obtain a flame retardant additive;
[0020] Further, the usage ratio of the reaction product, toluene, pyridine and epoxy product is 0.1 mol:190-200 mL:0.005-0.006 mol:0.2 mol;
[0021] During the reaction of step A3, the carboxyl group of the reaction product and the epoxy group of the epoxy product open to generate a flame retardant additive;
[0022] The impact modifier is prepared by the following steps:
[0023] Step B1: Add vinyl pentamethyldisiloxane to DMF, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 4-5 hours to obtain epoxy product a;
[0024] Further, the usage ratio of vinyl pentamethyldisiloxane, DMF and 3-chloroperoxybenzoic acid is 0.1 mol:40-50 mL:0.1 mol;
[0025] During the reaction of step B1, the carbon-carbon double bond in vinyl pentamethyldisiloxane is oxidized to an epoxy group to obtain an epoxy product a;
[0026] Step B2: In a nitrogen atmosphere, add perfluoropentanoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product a into the flask, stir and react for 8-10 hours to obtain a hydroxyl product;
[0027] Furthermore, the usage ratio of perfluoropentanoic acid, toluene, pyridine and epoxy product a is 0.1 mol:70-80 mL:0.002-0.003 mol:0.1 mol;
[0028] During the reaction of step B2, the carboxyl group of perfluoropentanoic acid and the epoxy group of the epoxy product a open to generate a hydroxyl product;
[0029] Step B3: Add the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution 1; add methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 2; slowly dropwise add the mixed solution 2 into the mixed solution 1 in a 0°C ice-water bath; after the dropwise addition is completed, raise the temperature to 40°C, stir and react at a constant temperature for 8-10 hours, and distill under reduced pressure to obtain a fluorosilicon product;
[0030] Further, the dosage ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 0.1 mol: 0.01-0.015 mol: 0.1 mol: 80-90 mL; the dosage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 20-30 mL; the dosage ratio of the mixed solution 1 and the mixed solution 2 is 85-95 mL: 25-35 mL;
[0031] During the reaction of step B3, the hydroxyl group of the hydroxyl product reacts with methacryloyl chloride to generate a fluorosilicon product containing a terminal double bond;
[0032] Step B4: adding methyl methacrylate, butyl acrylate, fluorosilicon product, hydroxyethyl methacrylate and acrylic acid into a flask, starting stirring, then adding dibenzoyl peroxide, xylene and butyl acetate, stirring and reacting at 100° C. for 7-9 hours to obtain an impact modifier;
[0033] Further, the usage ratio of methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:30g:10g:10g:5g:1g:150mL:100mL;
[0034] During the reaction of step B4, methyl methacrylate, butyl acrylate, fluorosilicon product, hydroxyethyl methacrylate and acrylic acid are polymerized under the initiation of dibenzoyl peroxide to obtain an impact modifier;
[0035] Beneficial effects of the invention: The invention discloses a corrosion-resistant low-voltage cable, which includes a wire core, an inner semi-conductive shielding layer, an insulating layer, an outer semi-conductive shielding layer, a metal shielding layer and a sheath layer from the inside to the outside, and the sheath layer includes the following raw materials: polyvinyl chloride, a flame retardant additive, an impact modifier, a coupling agent, an antioxidant, a plasticizer, a cross-linking agent, a promoter, a cross-linking aid, magnesium oxide and zinc oxide. Polyvinyl chloride has excellent acid and alkali corrosion resistance and meets the use requirements of corrosion-resistant low-voltage cables. The flame retardant additive is based on DOPO as the basic skeleton, and active hydroxyl and cinnamamide structures are introduced into it; the active hydroxyl and the carboxyl and hydroxyl functional groups in the impact modifier are cross-linked, and the impact modifier has good dispersibility in polyvinyl chloride with large polarity. As the impact modifier is dispersed in the matrix, the flame retardant additive is evenly dispersed in the matrix, avoiding uneven dispersion or migration failure of DOPO and cinnamamide small molecules in the matrix; the DOPO structure can dehydrate and degrade the polymer surface to form a carbon layer when the matrix burns, and the phosphorus-containing derivatives produced at the same time cover the polymer surface, isolate the combustible gas, block the heat transfer, form a physical shield, play a flame retardant and fireproof role, and make the cable have halogen-free flame retardant characteristics; adding cinnamamide to the matrix will not only not produce toxic substances and odors harmful to the human body and pollute the environment, but also can keep away mice for a long time, preventing mice from gnawing on the sheath material and causing the cable sheath to lose its protective effect. Therefore, the flame retardant additive makes the cable have good halogen-free flame retardancy and rodent resistance.
[0036] The synthesized impact modifier is a polysiloxane chain and a long fluorinated alkane chain introduced into an acrylate copolymer; the acrylate copolymer can significantly improve the impact strength of polyvinyl chloride, and the carboxyl and hydroxyl groups in the acrylate copolymer are cross-linked with the hydroxyl groups of the flame retardant additive, increasing the cross-linking network density of the system, and cooperating with the long fluorinated alkane chain with strong hydrophobicity to enhance the waterproofness of the sheath material, thereby significantly improving the waterproofness of the cable; the polysiloxane chain has a high bond energy of Si-OS i and SiC bonds, and requires a high energy to break, which improves the thermal stability of the cable sheath material, so that the cable has good performance under high temperature conditions and improves the high temperature resistance of the cable. Therefore, adding the synthesized impact modifier can improve the waterproofness and high temperature resistance of the cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0038] Figure 1 The figure is a schematic structural diagram of a corrosion-resistant low-voltage cable of the present invention.
[0039] In the accompanying drawings, the components represented by the reference numerals are listed as follows:
[0040] Ⅰ. Wire core; Ⅱ. Inner semi-conductive shielding layer; Ⅲ. Insulation layer; Ⅳ. Outer semi-conductive shielding layer; Ⅴ. Metal shielding layer; Ⅵ. Sheath layer. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] A flame retardant additive is prepared by the following steps:
[0044] Step A1: Add cinnamic acid and DOPO to a flask, start stirring, heat to 125°C, and stir at constant temperature for 3 hours to obtain a reaction product; the amount ratio of cinnamic acid to DOPO is 0.1 mol:0.1 mol;
[0045] Step A2: Add 3,4-dihydroxycinnamamide, epichlorohydrin and tetraethylammonium chloride into a flask, start stirring, heat to 75°C, reflux and stir for 1 hour, slowly drop sodium hydroxide solution, continue to reflux and stir for 2 hours, cool to room temperature, add benzene into the flask, slowly drop sodium hydroxide solution, reflux and stir for 2 hours, wash with distilled water, and distill under reduced pressure to obtain an epoxy product; the total amount of 3,4-dihydroxycinnamamide, epichlorohydrin, tetraethylammonium chloride, sodium hydroxide solution and benzene are in a ratio of 0.1 mol: 0.2 mol: 0.001 mol: 85 mL: 110 mL; the concentration of the sodium hydroxide solution is 0.25 mol / L, and the volume ratio of the sodium hydroxide solution added twice is 1:1;
[0046] Step A3: In a nitrogen atmosphere, add the reaction product and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8 hours to obtain a flame retardant additive; the amount ratio of the reaction product, toluene, pyridine and epoxy product is 0.1 mol:190 mL:0.005 mol:0.2 mol.
[0047] Example 2
[0048] A flame retardant additive is prepared by the following steps:
[0049] Step A1: Add cinnamic acid and DOPO to a flask, start stirring, heat to 130°C, and stir at constant temperature for 3.5 hours to obtain a reaction product; the amount ratio of cinnamic acid to DOPO is 0.1 mol:0.1 mol;
[0050] Step A2: 3,4-dihydroxycinnamamide, epichlorohydrin and tetraethylammonium chloride are added to a flask, stirring is started, the temperature is raised to 80°C, the mixture is refluxed and stirred for 1 hour, sodium hydroxide solution is slowly added dropwise, the mixture is refluxed and stirred for 2.2 hours, the mixture is cooled to room temperature, benzene is added to the flask, sodium hydroxide solution is slowly added dropwise, the mixture is refluxed and stirred for 2.2 hours, the mixture is washed with distilled water and distilled under reduced pressure to obtain an epoxy product; the total amount of 3,4-dihydroxycinnamamide, epichlorohydrin, tetraethylammonium chloride and sodium hydroxide solution and the amount ratio of benzene are 0.1 mol: 0.2 mol: 0.0015 mol: 90 mL: 120 mL; the concentration of the sodium hydroxide solution is 0.27 mol / L, and the volume ratio of the sodium hydroxide solution added twice is 1:1;
[0051] Step A3: In a nitrogen atmosphere, add the reaction product and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 9 hours to obtain a flame retardant additive; the amount ratio of the reaction product, toluene, pyridine and epoxy product is 0.1 mol:195mL:0.005 mol:0.2 mol.
[0052] Example 3
[0053] A flame retardant additive is prepared by the following steps:
[0054] Step A1: Add cinnamic acid and DOPO to a flask, start stirring, heat to 135°C, and stir at constant temperature for 4 hours to obtain a reaction product; the amount ratio of cinnamic acid to DOPO is 0.1 mol:0.1 mol;
[0055] Step A2: 3,4-dihydroxycinnamamide, epichlorohydrin and tetraethylammonium chloride are added to a flask, stirring is started, the temperature is raised to 85°C, the mixture is refluxed and stirred for 1 hour, sodium hydroxide solution is slowly added dropwise, the mixture is refluxed and stirred for 2.5 hours, the mixture is cooled to room temperature, benzene is added to the flask, sodium hydroxide solution is slowly added dropwise, the mixture is refluxed and stirred for 2.5 hours, the mixture is washed with distilled water and distilled under reduced pressure to obtain an epoxy product; the total amount of 3,4-dihydroxycinnamamide, epichlorohydrin, tetraethylammonium chloride and sodium hydroxide solution and the amount ratio of benzene are 0.1 mol:0.2 mol:0.002 mol:95 mL:130 mL; the concentration of the sodium hydroxide solution is 0.30 mol / L, and the volume ratio of the sodium hydroxide solution added twice is 1:1;
[0056] Step A3: In a nitrogen atmosphere, add the reaction product and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 10 hours to obtain a flame retardant additive; the amount ratio of the reaction product, toluene, pyridine and epoxy product is 0.1 mol: 200 mL: 0.006 mol: 0.2 mol.
[0057] Example 4
[0058] An impact modifier is prepared by the following steps:
[0059] Step B1: Add vinyl pentamethyl disiloxane to DMF, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 4 hours to obtain epoxy product a; the amount ratio of vinyl pentamethyl disiloxane, DMF and 3-chloroperoxybenzoic acid is 0.1 mol:40 mL:0.1 mol;
[0060] Step B2: In a nitrogen atmosphere, add perfluoropentanoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product a into the flask, stir and react for 8 hours to obtain a hydroxyl product; the dosage ratio of perfluoropentanoic acid, toluene, pyridine and epoxy product a is 0.1 mol:70 mL:0.002 mol:0.1 mol;
[0061] Step B3: Add the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution 1; add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 into the mixed solution 1 in a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 8 hours, and distill under reduced pressure to obtain a fluorosilicon product; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 0.1 mol: 0.01 mol: 0.1 mol: 80 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 20 mL; the amount ratio of the mixed solution 1 to the mixed solution 2 is 85 mL: 25 mL;
[0062] Step B4: Add methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate and acrylic acid into a flask, start stirring, then add dibenzoyl peroxide, xylene and butyl acetate, and stir the reaction at 100°C for 7 hours to obtain an impact modifier; the amount ratio of methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:30g:10g:10g:5g:1g:150mL:100mL.
[0063] Example 5
[0064] An impact modifier is prepared by the following steps:
[0065] Step B1: Add vinyl pentamethyl disiloxane to DMF, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 4.5 hours to obtain epoxy product a; the amount ratio of vinyl pentamethyl disiloxane, DMF and 3-chloroperoxybenzoic acid is 0.1 mol:45 mL:0.1 mol;
[0066] Step B2: In a nitrogen atmosphere, add perfluoropentanoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product a into the flask, stir and react for 9 hours to obtain a hydroxyl product; the dosage ratio of perfluoropentanoic acid, toluene, pyridine and epoxy product a is 0.1 mol:75 mL:0.002 mol:0.1 mol;
[0067] Step B3: Add the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution 1; add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 into the mixed solution 1 in a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 9 hours, and distill under reduced pressure to obtain a fluorosilicon product; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 0.1 mol: 0.013 mol: 0.1 mol: 85 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 25 mL; the amount ratio of the mixed solution 1 to the mixed solution 2 is 90 mL: 30 mL;
[0068] Step B4: Add methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate and acrylic acid into a flask, start stirring, then add dibenzoyl peroxide, xylene and butyl acetate, and stir the reaction at 100°C for 8 hours to obtain an impact modifier; the amount ratio of methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:30g:10g:10g:5g:1g:150mL:100mL.
[0069] Example 6
[0070] An impact modifier is prepared by the following steps:
[0071] Step B1: Add vinyl pentamethyl disiloxane to DMF, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 5 hours to obtain epoxy product a; the amount ratio of vinyl pentamethyl disiloxane, DMF and 3-chloroperoxybenzoic acid is 0.1 mol:50 mL:0.1 mol;
[0072] Step B2: In a nitrogen atmosphere, add perfluoropentanoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product a into the flask, stir and react for 10 hours to obtain a hydroxyl product; the dosage ratio of perfluoropentanoic acid, toluene, pyridine and epoxy product a is 0.1 mol:80 mL:0.003 mol:0.1 mol;
[0073] Step B3: Add the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution 1; add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution 2, slowly drop the mixed solution 2 into the mixed solution 1 in a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 10 hours, and distill under reduced pressure to obtain a fluorosilicon product; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 0.1 mol: 90 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 30 mL; the amount ratio of the mixed solution 1 to the mixed solution 2 is 95 mL: 35 mL;
[0074] Step B4: Add methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate and acrylic acid into a flask, start stirring, then add dibenzoyl peroxide, xylene and butyl acetate, and stir the reaction at 100°C for 9 hours to obtain an impact modifier; the amount ratio of methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:30g:10g:10g:5g:1g:150mL:100mL.
[0075] Example 7
[0076] like Figure 1 The corrosion-resistant low-voltage cable shown in the figure includes, from the inside to the outside, a core I, an inner semi-conductive shielding layer II, an insulating layer III, an outer semi-conductive shielding layer IV, a metal shielding layer V and a sheath layer VI, the core I is located in the innermost layer, the outer periphery of the core I is extruded with an inner semi-conductive shielding layer II; the outer periphery of the inner semi-conductive shielding layer II is extruded with an insulating layer III; the outer periphery of the insulating layer III is extruded with an outer semi-conductive shielding layer IV; the outer periphery of the outer semi-conductive shielding layer IV is provided with a metal shielding layer V; the outer periphery of the metal shielding layer V is extruded with a sheath layer VI; the core I is a plurality of twisted copper wires, the inner semi-conductive shielding layer II and the outer semi-conductive shielding layer IV are both made of ethylene-vinyl acetate copolymer material, the insulating layer III is made of cross-linked polyethylene insulating material, and the metal shielding layer V is obtained by spirally wrapping an aluminum conductive metal tape around the outer semi-conductive shielding layer IV;
[0077] The sheath layer VI is made of a corrosion-resistant sheath material, which includes the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 40 parts of flame retardant additives, 25 parts of impact modifiers, 0.8 parts of coupling agents, 1.5 parts of antioxidants, 25 parts of plasticizers, 2 parts of crosslinking agents, 8 parts of accelerators, 1 part of crosslinking aids, 10 parts of magnesium oxide, and 5 parts of zinc oxide; the coupling agent is KH560, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, the plasticizer is epoxy soybean oil, the crosslinking agent is diisopropyl peroxide, the accelerator is accelerator DM, and the crosslinking aid is triallyl isocyanurate;
[0078] The preparation of the corrosion-resistant low-voltage cable comprises the following steps:
[0079] Step S1: Put polyvinyl chloride and the impact modifier obtained in Example 4 into a torque rheometer, mix for 10 minutes, heat to 90° C., then add the flame retardant additive, coupling agent, antioxidant, plasticizer, magnesium oxide and zinc oxide obtained in Example 1 into the torque rheometer for mixing, after 25 minutes, heat to 130° C., add a crosslinking agent, accelerator and crosslinking aid, and continue mixing for 10 minutes to prepare a corrosion-resistant sheath material;
[0080] Step S2: use an extruder to extrude and deposit the inner semi-conductive shielding layer on the periphery of the wire core, and then extrude and deposit an insulating layer on the periphery of the inner semi-conductive shielding layer; then extrude and deposit the outer semi-conductive shielding layer on the periphery of the insulating layer; then wrap an aluminum conductive metal belt around the periphery of the outer semi-conductive shielding layer in a spiral form to obtain a metal shielding layer; finally, extrude and deposit a corrosion-resistant sheath material on the periphery of the metal shielding layer to obtain a sheath layer, and anneal after extrusion to obtain a corrosion-resistant low-voltage cable.
[0081] Example 8
[0082] like Figure 1 The corrosion-resistant low-voltage cable shown in the figure includes, from the inside to the outside, a core I, an inner semi-conductive shielding layer II, an insulating layer III, an outer semi-conductive shielding layer IV, a metal shielding layer V and a sheath layer VI, the core I is located in the innermost layer, the outer periphery of the core I is extruded with an inner semi-conductive shielding layer II; the outer periphery of the inner semi-conductive shielding layer II is extruded with an insulating layer III; the outer periphery of the insulating layer III is extruded with an outer semi-conductive shielding layer IV; the outer periphery of the outer semi-conductive shielding layer IV is provided with a metal shielding layer V; the outer periphery of the metal shielding layer V is extruded with a sheath layer VI; the core I is a plurality of twisted copper wires, the inner semi-conductive shielding layer II and the outer semi-conductive shielding layer IV are both made of ethylene-vinyl acetate copolymer material, the insulating layer III is made of cross-linked polyethylene insulating material, and the metal shielding layer V is obtained by spirally wrapping an aluminum conductive metal tape around the outer semi-conductive shielding layer IV;
[0083] The sheath layer VI is made of a corrosion-resistant sheath material, which includes the following raw materials in parts by weight: 55 parts of polyvinyl chloride, 45 parts of flame retardant additives, 30 parts of impact modifiers, 0.9 parts of coupling agents, 1.7 parts of antioxidants, 27 parts of plasticizers, 3 parts of crosslinking agents, 9 parts of accelerators, 2 parts of crosslinking aids, 12 parts of magnesium oxide, and 7 parts of zinc oxide; the coupling agent is KH560, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, the plasticizer is epoxy soybean oil, the crosslinking agent is diisopropyl peroxide, the accelerator is accelerator DM, and the crosslinking aid is triallyl isocyanurate;
[0084] The preparation of the corrosion-resistant low-voltage cable comprises the following steps:
[0085] Step S1: Put polyvinyl chloride and the impact modifier obtained in Example 5 into a torque rheometer, mix for 10 minutes, heat to 90° C., then add the flame retardant additive, coupling agent, antioxidant, plasticizer, magnesium oxide and zinc oxide obtained in Example 2 into the torque rheometer for mixing, after 25 minutes, heat to 130° C., add a crosslinking agent, accelerator and crosslinking aid, and continue mixing for 10 minutes to prepare a corrosion-resistant sheath material;
[0086] Step S2: use an extruder to extrude and deposit the inner semi-conductive shielding layer on the periphery of the wire core, and then extrude and deposit an insulating layer on the periphery of the inner semi-conductive shielding layer; then extrude and deposit the outer semi-conductive shielding layer on the periphery of the insulating layer; then wrap an aluminum conductive metal belt around the periphery of the outer semi-conductive shielding layer in a spiral form to obtain a metal shielding layer; finally, extrude and deposit a corrosion-resistant sheath material on the periphery of the metal shielding layer to obtain a sheath layer, and anneal after extrusion to obtain a corrosion-resistant low-voltage cable.
[0087] Example 9
[0088] like Figure 1 The corrosion-resistant low-voltage cable shown in the figure includes, from the inside to the outside, a core I, an inner semi-conductive shielding layer II, an insulating layer III, an outer semi-conductive shielding layer IV, a metal shielding layer V and a sheath layer VI, the core I is located in the innermost layer, the outer periphery of the core I is extruded with an inner semi-conductive shielding layer II; the outer periphery of the inner semi-conductive shielding layer II is extruded with an insulating layer III; the outer periphery of the insulating layer III is extruded with an outer semi-conductive shielding layer IV; the outer periphery of the outer semi-conductive shielding layer IV is provided with a metal shielding layer V; the outer periphery of the metal shielding layer V is extruded with a sheath layer VI; the core I is a plurality of twisted copper wires, the inner semi-conductive shielding layer II and the outer semi-conductive shielding layer IV are both made of ethylene-vinyl acetate copolymer material, the insulating layer III is made of cross-linked polyethylene insulating material, and the metal shielding layer V is obtained by spirally wrapping an aluminum conductive metal tape around the outer semi-conductive shielding layer IV;
[0089] The sheath layer VI is made of a corrosion-resistant sheath material, which includes the following raw materials in parts by weight: 60 parts of polyvinyl chloride, 50 parts of flame retardant additives, 35 parts of impact modifiers, 1.0 parts of coupling agents, 2 parts of antioxidants, 30 parts of plasticizers, 4 parts of cross-linking agents, 10 parts of accelerators, 3 parts of cross-linking aids, 15 parts of magnesium oxide, and 10 parts of zinc oxide; the coupling agent is KH560, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, the plasticizer is epoxy soybean oil, the cross-linking agent is diisopropyl peroxide, the accelerator is accelerator DM, and the cross-linking aid is triallyl isocyanurate;
[0090] The preparation of the corrosion-resistant low-voltage cable comprises the following steps:
[0091] Step S1: Put polyvinyl chloride and the impact modifier obtained in Example 6 into a torque rheometer, mix for 10 minutes, heat to 90° C., then add the flame retardant additive, coupling agent, antioxidant, plasticizer, magnesium oxide and zinc oxide obtained in Example 3 into the torque rheometer for mixing, after 25 minutes, heat to 130° C., add a crosslinking agent, accelerator and crosslinking aid, and continue mixing for 10 minutes to prepare a corrosion-resistant sheath material;
[0092] Step S2: use an extruder to extrude and deposit the inner semi-conductive shielding layer on the periphery of the wire core, and then extrude and deposit an insulating layer on the periphery of the inner semi-conductive shielding layer; then extrude and deposit the outer semi-conductive shielding layer on the periphery of the insulating layer; then wrap an aluminum conductive metal belt around the periphery of the outer semi-conductive shielding layer in a spiral form to obtain a metal shielding layer; finally, extrude and deposit a corrosion-resistant sheath material on the periphery of the metal shielding layer to obtain a sheath layer, and anneal after extrusion to obtain a corrosion-resistant low-voltage cable.
[0093] Comparative Example 1
[0094] Compared with Example 9, the flame retardant additive was replaced with DOPO, and the rest was exactly the same as Example 9 to prepare a corrosion-resistant low-voltage cable.
[0095] Comparative Example 2
[0096] Compared with Example 9, the impact modifier is replaced with an acrylic copolymer, and the rest is exactly the same as Example 9 to obtain a corrosion-resistant low-voltage cable; the preparation process of the acrylic copolymer is as follows: methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate and acrylic acid are added to a flask, stirring is started, and then dibenzoyl peroxide, xylene and butyl acetate are added, and the reaction is stirred at 100°C for 9 hours to obtain an acrylic copolymer; the amount ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:40g:10g:5g:1g:150mL:100mL.
[0097] The corrosion-resistant low-voltage cable prepared by the present invention is further tested for its effect, and the test results are as follows.
[0098] In order to test the corrosion-resistant low-voltage cable prepared by the present invention, the performance test of the sheath material of the low-voltage cable obtained in Examples 7-9 and Comparative Examples 1-2 was carried out, and the 200°C thermal stability time was measured according to GB / T2951.32-2008 "General Test Methods for Insulation and Sheath Materials of Electric Cables and Optical Cables"; the oxygen index was tested according to GB / T2406.1-2008 "Determination of Combustion Behavior by Oxygen Index Method for Plastics"; and the oxygen index was tested according to GB / T34016-2017 "General Rules for Rat-proof and Ant-proof Wires and Cables". Test rodent-proof performance; Waterproof performance test method: Take 150.0g of the corrosion-resistant low-voltage cable samples obtained from Examples 7-9 and Comparative Examples 1-2 and immerse them in water (water temperature 15°C), seal both ends of the sample and extend 300mm out of the water surface. After soaking for one week, measure the weight after soaking and remove the sheath layer after soaking to observe whether there is moisture on the outer surface; use an impact testing machine to test the impact strength according to GB / T1843-2008 "Determination of impact strength of plastic cantilever beam"; the results are recorded in Table 1;
[0099] Table 1:
[0100]
[0101]
[0102] According to the data in Table 1, the sheath material of the corrosion-resistant low-voltage cable prepared by the present invention has good high temperature resistance, flame retardancy, waterproofness, rodent resistance and impact strength; Comparative Example 1 is compared with Example 9, and the flame retardant additive of active hydroxyl and cinnamamide is introduced into the DOPO skeleton, so that the sheath material has good flame retardancy and good rodent resistance, thereby improving the flame retardancy and rodent resistance of the corrosion-resistant cable, and the active hydroxyl is cross-linked with the impact modifier, which is also beneficial to the improvement of the waterproofness of the cable; Comparative Example 2 is compared with Example 9, and an acrylic copolymer containing polysiloxane and a long chain of fluorinated alkane is used as an impact modifier, and the waterproofness and high temperature resistance of the sheath material are improved, thereby improving the waterproofness and high temperature resistance of the cable.
[0103] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A corrosion-resistant low-voltage cable, characterized in that: From the inside to the outside, it includes a wire core Ⅰ, an inner semi-conductive shielding layer Ⅱ, an insulating layer Ⅲ, an outer semi-conductive shielding layer Ⅳ, a metal shielding layer Ⅴ and a sheath layer Ⅵ. The wire core Ⅰ is located in the innermost layer. The outer periphery of the wire core Ⅰ is extruded with an inner semi-conductive shielding layer Ⅱ; the outer periphery of the inner semi-conductive shielding layer Ⅱ is extruded with an insulating layer Ⅲ; the outer periphery of the insulating layer Ⅲ is extruded with an outer semi-conductive shielding layer Ⅳ; the outer periphery of the outer semi-conductive shielding layer Ⅳ is provided with a metal shielding layer Ⅴ; the outer periphery of the metal shielding layer Ⅴ is extruded with a sheath layer Ⅵ The sheath layer VI is made of a corrosion-resistant sheath material, which includes the following raw materials in parts by weight: 50-60 parts of polyvinyl chloride, 40-50 parts of flame retardant additives, 25-35 parts of impact modifiers, 0.8-1.0 parts of coupling agents, 1.5-2 parts of antioxidants, 25-30 parts of plasticizers, 2-4 parts of crosslinking agents, 8-10 parts of accelerators, 1-3 parts of crosslinking additives, 10-15 parts of magnesium oxide, and 5-10 parts of zinc oxide. The flame retardant auxiliary agent is prepared by the following steps: Step A1: Add cinnamic acid and DOPO into a flask, start stirring, raise the temperature to 125-135°C, and stir at constant temperature for 3-4 hours to obtain a reaction product; Step A2: Add 3,4-dihydroxycinnamamide, epichlorohydrin and tetraethylammonium chloride into a flask, start stirring, heat to 75-85°C, reflux and stir for 1 hour, slowly add sodium hydroxide solution dropwise, continue to reflux and stir for 2-2.5 hours, cool to room temperature, add benzene into the flask, slowly add sodium hydroxide solution dropwise, reflux and stir for 2-2.5 hours, wash with distilled water, and distill under reduced pressure to obtain epoxy product 2; Step A3: In a nitrogen atmosphere, add the reaction product and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10 hours to obtain a flame retardant additive.
2. A corrosion-resistant low-voltage cable according to claim 1, characterized in that: In step A1, the usage ratio of cinnamic acid and DOPO is 0.1 mol:0.1 mol.
3. The corrosion-resistant low-voltage cable according to claim 1, characterized in that: In step A2, the total amount of 3,4-dihydroxycinnamic acid amide, epichlorohydrin, tetraethylammonium chloride, sodium hydroxide solution and benzene are used in a ratio of 0.1 mol: 0.2 mol: 0.001-0.002 mol: 85-95 mL: 110-130 mL; the concentration of the sodium hydroxide solution is 0.25-0.30 mol / L, and the volume ratio of the sodium hydroxide solutions added twice is 1:
1.
4. The corrosion-resistant low-voltage cable according to claim 1, characterized in that: In step A3, the usage ratio of the reaction product, toluene, pyridine and epoxy product is 0.1 mol:190-200 mL:0.005-0.006 mol:0.2 mol.
5. The corrosion-resistant low-voltage cable according to claim 1, characterized in that: The impact modifier is prepared by the following steps: Step B1: Add vinyl pentamethyldisiloxane to DMF, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 4-5 hours to obtain epoxy product a; Step B2: In a nitrogen atmosphere, add perfluoropentanoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product a into the flask, stir and react for 8-10 hours to obtain a hydroxyl product; Step B3: Add the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution 1; add methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 2; slowly dropwise add the mixed solution 2 into the mixed solution 1 in a 0°C ice-water bath; after the dropwise addition is completed, raise the temperature to 40°C, stir and react at a constant temperature for 8-10 hours, and distill under reduced pressure to obtain a fluorosilicon product; Step B4: Add methyl methacrylate, butyl acrylate, fluorosilicon product, hydroxyethyl methacrylate and acrylic acid into a flask, start stirring, then add dibenzoyl peroxide, xylene and butyl acetate, stir and react at 100° C. for 7-9 hours to obtain an impact modifier.
6. A corrosion-resistant low-voltage cable according to claim 5, characterized in that: In step B1, the usage ratio of vinyl pentamethyldisiloxane, DMF and 3-chloroperoxybenzoic acid is 0.1 mol: 40-50 mL: 0.1 mol; in step B2, the usage ratio of perfluoropentanoic acid, toluene, pyridine and epoxy product a is 0.1 mol: 70-80 mL: 0.002-0.003 mol: 0.1 mol.
7. The corrosion-resistant low-voltage cable according to claim 5, characterized in that: In step B3, the usage ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 0.1 mol: 0.01-0.015 mol: 0.1 mol: 80-90 mL; the usage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 20-30 mL; the usage ratio of mixed solution 1 and mixed solution 2 is 85-95 mL: 25-35 mL.
8. The corrosion-resistant low-voltage cable according to claim 5, characterized in that: In step B4, the usage ratio of methyl methacrylate, butyl acrylate, fluorosilicone product, hydroxyethyl methacrylate, acrylic acid, dibenzoyl peroxide, xylene and butyl acetate is 45g:30g:10g:10g:5g:1g:150mL:100mL.
9. The corrosion-resistant low-voltage cable according to claim 1, characterized in that: The wire core I is a plurality of twisted copper wires, the inner semi-conductive shielding layer II and the outer semi-conductive shielding layer IV are both made of ethylene-vinyl acetate copolymer material, the insulating layer III is made of cross-linked polyethylene insulating material, and the metal shielding layer V is an aluminum conductive metal belt spirally wound around the outer semi-conductive shielding layer IV; the coupling agent is KH560, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, the plasticizer is epoxy soybean oil, the cross-linking agent is diisopropyl peroxide, the accelerator is accelerator DM, and the cross-linking aid is triallyl isocyanurate.
10. The method for preparing a corrosion-resistant low-voltage cable according to claim 1, characterized in that: The steps include: Step S1: Put polyvinyl chloride and impact modifier into a torque rheometer, mix for 10 minutes, heat to 90°C, add flame retardant, coupling agent, antioxidant, plasticizer, magnesium oxide and zinc oxide into the torque rheometer for mixing, heat to 130°C after 25 minutes, add crosslinking agent, accelerator and crosslinking aid, and continue mixing for 10 minutes to prepare corrosion-resistant sheath material; Step S2: Use an extruder to extrude and deposit the inner semi-conductive shielding layer on the periphery of the wire core, and then extrude and deposit the insulating layer on the periphery of the inner semi-conductive shielding layer; then extrude and deposit the outer semi-conductive shielding layer on the periphery of the insulating layer; then wrap an aluminum conductive metal belt around the periphery of the outer semi-conductive shielding layer in a spiral form to obtain a metal shielding layer; finally, extrude and deposit a corrosion-resistant sheath material on the periphery of the metal shielding layer to obtain a sheath layer, and anneal after extrusion to obtain a corrosion-resistant low-voltage cable.
Citation Information
Patent Citations
Impact-resistant flame-retardant fire-resistant cable and production process thereof
CN115746481A
Flexible mineral insulation isolation type flame-retardant B1-level rat-proof and termite-proof fireproof cable
CN117524569A
Impact-resistant modified polyacrylic resin and preparation process thereof
CN118271770A
Perpendicular for earthing pole water conservancy diversion cable of dark well type
CN207765197U
Halogen-free flame retardant compositions with improved tensile properties
WO2017151256A1
Cited By
Wear-resistant and impact-resistant composite PVC (polyvinyl chloride) material and preparation method thereof
CN119591998A
Medium-voltage power cable and manufacturing method thereof
CN121011391A
Low-voltage cable oil-resistant and corrosion-resistant sheath material and preparation method thereof
CN122790327A