Through the formula and process of polycarbonate and hollow glass beads, the problem of glare and high-cost light diffusion agent of the lampshade is solved, the low-cost production of high-transmittance and high-haze lampshades is achieved, and the usage and cost are significantly reduced.

CN114773821BActive Publication Date: 2024-10-18ZHENGZHOU HOLLOWLITE MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210344783.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-10-18
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The existing lampshade materials cause the light to be too dazzling, and the cost of high-transmittance light diffusing agents is high, making it difficult to achieve high-transmittance and high-haze effects at low cost.

Method used

Using a formula of polycarbonate, hollow glass beads, antioxidants, and anti-yellowing agents, a high-transmittance and high-haze lampshade is prepared through mechanical mixing and extrusion granulation processes, taking advantage of the low density and hollow structure of hollow glass beads. Improve light diffusion effect.

Benefits of technology

It achieves light diffusion and haze effects similar to those of organic light diffusing agents at a lower cost. The dosage of hollow glass beads is only 1/3-1/5 of that of organic light diffusing agents, which significantly reduces the cost and improves the quality of the lampshade. Transparency and haze.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114773821B_ABST
    Figure CN114773821B_ABST
Patent Text Reader

Abstract

The invention discloses a formula and a processing technology of a high-transmittance and high-fog lampshade. The formula and the processing technology of the lampshade include the following raw material components in mass proportion: 96-98 parts of polycarbonate, 0.2-1.5 parts of hollow glass microspheres, 0.2-1.0 parts of antioxidants, and 0.2-1.5 parts of anti-yellowing agents. The formula comprises the following steps: weighing a certain amount of polycarbonate, antioxidants and anti-yellowing agents for mechanical mixing; weighing a certain amount of hollow glass microspheres for pretreatment and drying; setting the temperature of an extruder to 260-290 DEG C, adding the evenly mixed polycarbonate antioxidant and anti-yellowing agent to a main feeding port of the extruder; adding the treated hollow glass microspheres to a side feeding port of the extruder, adjusting the feeding parameters, controlling the addition amount to 0.2-1.5%, and performing extrusion granulation; drying the extruded particles at 100 DEG C for 4 hours, setting the temperature of an injection molding machine to 260-290 DEG C, and performing injection molding of a lampshade product with the dried particles. The light diffusion effect is stronger, and the light diffusion and haze effects similar to those of organic light diffusers can be achieved at a lower cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lampshade production, and in particular to a formula and processing technology of a high-light-transmittance and high-fog lampshade. Background Art

[0002] Today's lamps are not only used for lighting, but also a work of art. However, the space for upgrading the bulb itself is limited, and this effect is generally achieved through lampshades. In the past, lampshades were simply made of PC, PMMA, PS, or other types of raw materials. Some at most added some color powder to the raw materials of the lampshade to slightly improve the softness of the light inside the lampshade, but the brightness dropped a lot. And many lamps in the lampshade are incandescent bulbs. Even if the color powder is not added to the raw materials of the lampshade, it will not give people very dazzling light and make people uncomfortable. With the progress of society and the improvement of living requirements, energy demand is increasing. However, the resources available to us humans on the earth are getting less and less. Therefore, energy conservation and environmental protection are topics of common concern to mankind. In the field of lighting, such as daily lighting, factory production, and highway lighting, energy consumption is also huge. The introduction of LED lamps is a revolution in the field of lighting. LED lamps, also known as light-emitting diodes, can be used for lighting, with low energy consumption and high brightness, but the light is strong and dazzling, making it impossible for people to look directly, and it is impossible to get a soft visual effect. The introduction of light diffuser products has solved these problems very well.

[0003] At present, the light diffusers with the largest usage in the market include organic silicone balls, silicon dioxide, acrylic balls, etc. They can be divided into inorganic and organic types based on material classification. Inorganic light diffusers affect light transmittance, and the material transmittance is generally less than 50%. Organic light diffusers have good transmittance and can generally reach ≥70%, but due to high requirements on particle size, they are expensive. Lampshades have become a necessary supporting product for lamps, and their market capacity is huge. According to rough statistics, the domestic use of light diffusers can reach 10,000 tons a year. If a light diffuser with low price and excellent effect can be found, it will promote the rapid development of the lampshade market. Summary of the invention

[0004] To overcome the above defects, the purpose of the present invention is to provide a formula and processing technology for a high-transmittance and high-fog lampshade, which has a stronger light diffusion effect and achieves light diffusion and haze effects similar to those of organic light diffusers at a lower cost.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A formula for a high-transmittance and high-fog lampshade comprises the following raw material components in mass proportion: 96-98 parts of polycarbonate, 0.2-1.5 parts of hollow glass microspheres, 0.2-1.0 parts of antioxidants, and 0.2-1.5 parts of anti-yellowing agents.

[0007] Optionally, the polycarbonate may be selected from models including SABIC1003R, APEC1803 or Ningbo Dafeng 10R; the hollow glass microspheres may be selected from particle sizes including 30 μm, 15 μm or 10 μm; the antioxidant may be selected from models including B215, 1010 or 245; and the anti-yellowing agent may be selected from models including H-203, B11 or 9042.

[0008] A processing technology for a high-light-transmittance and high-fog lampshade comprises the following steps:

[0009] Weigh a certain amount of polycarbonate, antioxidant and anti-yellowing agent and mix them mechanically;

[0010] Weigh a certain amount of hollow glass microspheres for pretreatment and drying;

[0011] Set the extruder temperature to 260-290°C, and add the evenly mixed polycarbonate antioxidant and anti-yellowing agent into the main feed port of the extruder;

[0012] Add the processed hollow glass microbeads into the side feeding port of the extruder, adjust the feeding parameters, control the addition amount to 0.2-1.5%, and perform extrusion granulation;

[0013] The extruded particles were dried at 100°C for 4 hours;

[0014] The temperature of the injection molding machine is set at 260-290°C, and the dried particles are used to injection mold lampshade products.

[0015] Optionally, the step of weighing a certain amount of hollow glass microspheres for pretreatment and drying includes:

[0016] A certain amount of hollow glass microspheres is placed in a stirring tank;

[0017] Add appropriate amount of pure water;

[0018] The temperature was raised to 100°C and heated with stirring.

[0019] Optional, include the following steps:

[0020] Weigh 98 parts of Ningbo Dafeng polycarbonate, weigh 0.5 parts of antioxidant B215, weigh 0.5 parts of anti-yellowing agent H-203, and mechanically mix to obtain a mixture;

[0021] Weigh 1 portion of hollow glass microspheres with a particle size of 15 μm, place in a stirring kettle at 100° C., and stir at a constant speed for 30 minutes to obtain pretreated hollow glass microspheres;

[0022] Set the extruder temperature to 275°C, the main machine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min;

[0023] Add the mixed material from the main feeding port, add the pre-treated hollow glass microspheres from the side feeding port, granulate, and prepare the masterbatch;

[0024] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0025] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0026] The positive beneficial effects of the present invention are:

[0027] The hollow glass microspheres used in the present application have lower cost, lower density, and a smaller added mass fraction. Moreover, they are hollow and have a stronger light diffusion effect. To achieve the same light diffusion effect, the amount used is only 1 / 3-1 / 5 of the currently used organic light diffusers. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic block diagram of a method for processing a high-light-transmittance and high-fog lampshade provided by the present invention;

[0029] Figure 2 It is a schematic diagram comparing the light scattering effect of a hollow glass microsphere provided by the present invention with that of a solid transparent sphere. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with some specific implementation methods.

[0031] A formula for a high-transmittance and high-fog lampshade comprises the following raw material components in mass proportion: 96-98 parts of polycarbonate, 0.2-1.5 parts of hollow glass microspheres, 0.2-1.0 parts of antioxidants, and 0.2-1.5 parts of anti-yellowing agents.

[0032] The polycarbonate includes SABIC1003R, APEC1803 or Ningbo Dafeng 10R, and the high light transmittance type is selected; the hollow glass microspheres include 30μm, 15μm or 10μm in particle size; the antioxidant includes B215, 1010 or 245; the anti-yellowing agent includes H-203, B11 or 9042. While reducing the cost, the light transmittance and haze of the lampshade can be effectively guaranteed.

[0033] Example 1

[0034] like Figure 1 As shown, a processing technology for a high light transmittance and high fog lampshade includes the following steps:

[0035] S1. Weigh a certain amount of polycarbonate, antioxidant and anti-yellowing agent and mix them mechanically;

[0036] S2, weighing a certain amount of hollow glass microspheres for pretreatment and drying;

[0037] S3, setting the extruder temperature to 260-290°C, adding the evenly mixed polycarbonate antioxidant and anti-yellowing agent to the main feeding port of the extruder;

[0038] S4, adding the processed hollow glass microbeads into the side feeding port of the extruder, adjusting the feeding parameters, controlling the addition amount to 0.2-1.5%, and performing extrusion granulation;

[0039] S5, drying the extruded particles at 100° C. for 4 hours;

[0040] S6. Set the temperature of the injection molding machine to 260-290°C, and use the dried particles to injection mold lampshade products.

[0041] The side feeding method of hollow glass microspheres can ensure that the hollow glass microspheres with a small amount of added content are evenly dispersed in the resin matrix.

[0042] Specifically, the steps of weighing a certain amount of hollow glass microspheres for pretreatment and drying include:

[0043] S21, placing a certain amount of hollow glass microspheres into a stirring tank;

[0044] S22, add appropriate amount of pure water;

[0045] S23, raising the temperature to 100°C and heating with stirring.

[0046] Before adding hollow glass microspheres, pretreatment is required. The purpose of this process is to remove impurities on the surface of the microspheres so as not to affect their light transmittance.

[0047] like Figure 2 As shown, it can be seen that the incident light in the solid transparent sphere can be projected out after two refractions and reflections, while the incident light in the hollow glass microsphere can be projected out after four refractions and reflections. Its light divergence ability is stronger, that is, the haze effect of the lampshade is better.

[0048] Example 2

[0049] A processing technology for a high-transmittance and high-fog lampshade, characterized by comprising the steps of:

[0050] S11, weighing 98 parts of Ningbo Dafeng polycarbonate, weighing 0.5 parts of antioxidant B215, weighing 0.5 parts of anti-yellowing agent H-203, and mechanically mixing to obtain a mixture;

[0051] S21, weighing 1 portion of hollow glass microspheres with a particle size of 15 μm, placing in a stirring kettle at 100° C., and stirring at a constant speed for 30 min to obtain pretreated hollow glass microspheres;

[0052] S31, set the extruder temperature to 275°C, the main engine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min;

[0053] S41, adding a mixed material from the main feeding port, adding pretreated hollow glass microspheres from the side feeding port, granulating, and preparing a masterbatch;

[0054] S51, placing the masterbatch in a blast drying oven at 100° C. for drying;

[0055] S61, set the injection molding machine temperature to 280°C, the injection pressure to 110 bar, add the masterbatch and perform sample injection molding.

[0056] Comparative Example 1

[0057] Weigh 97 parts of Ningbo Dafeng polycarbonate, 0.5 parts of antioxidant B215, 0.5 parts of anti-yellowing agent H-203, and 2 parts of silicone balls, and mix them mechanically to obtain a mixture;

[0058] Set the extruder temperature to 275°C, the main machine speed to 100r / min, and the main feed speed to 9r / min;

[0059] Add the mixed material from the main feeding port, granulate it and prepare the masterbatch;

[0060] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0061] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0062] Comparative Example 2

[0063] Weigh 97 parts of Ningbo Dafeng polycarbonate, 0.5 parts of antioxidant B215, 0.5 parts of anti-yellowing agent H-203, and 2 parts of calcium carbonate, and mechanically mix to obtain a mixture;

[0064] Set the extruder temperature to 275°C, the main machine speed to 100r / min, and the main feed speed to 9r / min;

[0065] Add the mixed material from the main feeding port, granulate it and prepare the masterbatch;

[0066] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0067] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0068] Comparative Example 3

[0069] Weigh 96 parts of Ningbo Dafeng polycarbonate, weigh 0.5 parts of antioxidant B215, weigh 0.5 parts of anti-yellowing agent H-203, and mechanically mix to obtain a mixture;

[0070] Weigh 1 portion of hollow glass microspheres with a particle size of 15 μm, place in a stirring kettle at 100° C., and stir at a constant speed for 30 minutes to obtain pretreated hollow glass microspheres;

[0071] Set the extruder temperature to 275°C, the main machine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min;

[0072] Add the mixed material from the main feeding port, add the pre-treated hollow glass microspheres from the side feeding port, granulate, and prepare the masterbatch;

[0073] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0074] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0075] Comparative Example 4

[0076] Weigh 98 parts of Ningbo Dafeng polycarbonate, 0.2 parts of antioxidant B215, and 0.5 parts of anti-yellowing agent H-203, and mechanically mix them to obtain a mixture;

[0077] Weigh 1 portion of hollow glass microspheres with a particle size of 15 μm, place in a stirring kettle at 100° C., and stir at a constant speed for 30 minutes to obtain pretreated hollow glass microspheres;

[0078] Set the extruder temperature to 275°C, the main machine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min;

[0079] Add the mixed material from the main feeding port, add the pre-treated hollow glass microspheres from the side feeding port, granulate, and prepare the masterbatch;

[0080] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0081] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0082] Comparative Example 5

[0083] Weigh 98 parts of Ningbo Dafeng polycarbonate, weigh 0.5 parts of antioxidant B215, weigh 1 part of anti-yellowing agent H-203, and mechanically mix to obtain a mixture;

[0084] Weigh 1 portion of hollow glass microspheres with a particle size of 15 μm, place in a stirring kettle at 100° C., and stir at a constant speed for 30 minutes to obtain pretreated hollow glass microspheres;

[0085] Set the extruder temperature to 275°C, the main machine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min;

[0086] Add the mixed material from the main feeding port, add the pre-treated hollow glass microspheres from the side feeding port, granulate, and prepare the masterbatch;

[0087] The masterbatch was placed in a blast drying oven at 100°C for drying;

[0088] The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

[0089] Table 1

[0090] Transmittance Haze Example 2 78% 88% Comparative Example 1 82% 86% Comparative Example 2 42% 90% Comparative Example 3 79% 85% Comparative Example 4 75% 89% Comparative Example 5 76% 90%

[0091] Referring to Table 1, the lampshade prepared in Example 2 of the present application has a more obvious improvement in haze compared to the lampshade prepared in Comparative Example 1 using silicone balls. Although the light transmittance is insufficient, it has obvious advantages in cost. Organic light diffusers such as silicone balls are generally priced at more than 100,000 yuan per ton or even higher in the market, while the hollow glass microspheres used in the present technology have a market price of 30,000 to 70,000 yuan per ton, and the hollow microspheres have a low density, a smaller mass fraction added, and are hollow, so their light diffusion effect is stronger. To achieve the same light diffusion effect, their usage is only 1 / 3 to 1 / 5 of the currently used organic light diffusers; compared to Comparative Example 2, which uses calcium carbonate, an inorganic light diffuser, although it has a significant effect on improving the haze of the material, it greatly reduces the light transmittance of the material, making it less than 50%, which will lose most of the energy of the bulb and waste energy; the light diffusers of Comparative Examples 3-5 all use hollow glass microspheres, and use different mass fractions of polycarbonate, antioxidants and anti-yellowing agents, respectively. The comprehensive considerations of light transmittance, haze and cost are not as good as those of Example 2 of the present application.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A high light transmittance and high fog lampshade, characterized in that: The invention comprises the following raw material components in the following mass proportions: 96-98 parts of polycarbonate, 0.2-1.5 parts of hollow glass microspheres, 0.2-1.0 parts of antioxidants, and 0.2-1.5 parts of anti-yellowing agents; The polycarbonate is selected from SABIC1003R, APEC1803 or Ningbo Dafeng 10R; the hollow glass microspheres are selected from 30 μm, 15 μm or 10 μm in particle size; the antioxidant is selected from B215, 1010 or 245; the anti-yellowing agent is selected from H-203, B11 or 9042; the hollow glass microspheres are pretreated and dried, and the steps include: Put hollow glass microspheres into a stirring tank; Add appropriate amount of pure water; The temperature was raised to 100°C and heated with stirring.

2. A processing technology for a high light transmittance and high fog lampshade as claimed in claim 1, characterized in that: Includes steps: Weigh 96-98 parts of polycarbonate, 0.2-1.0 parts of antioxidant and 0.2-1.5 parts of anti-yellowing agent and mix them mechanically; Weigh 0.2-1.5 parts of hollow glass microspheres for pretreatment and drying; Set the extruder temperature to 260-290°C, and add the evenly mixed polycarbonate antioxidant and anti-yellowing agent into the main feed port of the extruder; Add the processed hollow glass microbeads into the side feeding port of the extruder, adjust the feeding parameters, control the addition amount to 0.2-1.5%, and perform extrusion granulation; The extruded particles were dried at 100°C for 4 hours; Set the temperature of the injection molding machine to 260-290°C and use the dried particles to mold lampshade products; The step of weighing 0.2-1.5 parts of hollow glass microspheres for pretreatment and drying comprises: Place 0.2-1.5 parts of hollow glass microspheres into a stirring kettle; Add appropriate amount of pure water; The temperature was raised to 100°C and heated with stirring.

3. The processing technology of a high light transmittance and high fog lampshade as claimed in claim 2, characterized in that: Includes steps: Weigh 98 parts of Ningbo Dafeng polycarbonate, weigh 0.5 parts of antioxidant B215, weigh 0.5 parts of anti-yellowing agent H-203, and mechanically mix to obtain a mixture; Weigh 1 portion of hollow glass microspheres with a particle size of 15 μm, place in a stirring kettle at 100° C., and stir at a constant speed for 30 minutes to obtain pretreated hollow glass microspheres; Set the extruder temperature to 275°C, the main machine speed to 100r / min, the main feed speed to 9r / min, and the side feed speed to 1.0r / min; Add the mixed material from the main feeding port, add the pre-treated hollow glass microspheres from the side feeding port, granulate, and prepare the masterbatch; The masterbatch was placed in a blast drying oven at 100°C for drying; The injection molding machine temperature was set to 280°C, the injection pressure to 110 bar, and the masterbatch was added for sample injection molding.

Citation Information

Patent Citations

  • Filled polycarbonate compositions with modified resilience

    CN101541873A