One-component adhesive and preparation method thereof

By using epoxy resin and modified epoxy resin in single-component adhesives combined with fumed silica, calcium carbonate and other additives, a dense network structure is formed, which solves the problem of insufficient performance of existing adhesives under high temperature conditions and achieves Improved high temperature stability and shear strength, suitable for various industrial fields.

CN114774041BActive Publication Date: 2024-10-11ZHENJIANG LEADER COMPOSITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110569276.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-25
Publication Date
2024-10-11
Estimated Expiration
2041-05-25

AI Technical Summary

Technical Problem

Existing single-component adhesives in automobile and other fields, especially when bonding metal materials and polymer materials on their surfaces, have poor high temperature resistance and oil resistance, and cannot meet the needs of use under special high temperature conditions.

Method used

Epoxy resin and modified epoxy resin are used as the main components, and by adding additives such as fumed silica, calcium carbonate, and mica powder, the formula and preparation process are optimized to form a dense three-dimensional network structure to improve toughness and shear. Strength, solving the problem of internal moisture and external dryness.

Benefits of technology

Significantly improves the adhesive's high temperature resistance, impact resistance and shear strength, ensuring stability at 150°C, and is suitable for automobiles, packaging, new energy and construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of adhesives, and more specifically relates to a novel one-component adhesive and a preparation method thereof. A novel one-component adhesive, the preparation raw materials of which include at least epoxy resin and / or modified epoxy resin; and also include 0.1-1.5 parts of fumed silica. The novel one-component adhesive and the preparation method thereof provided by the present invention have high temperature resistance and impact resistance; the novel one-component adhesive provided by the present invention solves the problem of "wet inside and dry outside" that occurs during the gluing process, ensures the stability of its application on the surface of materials such as metals, and can ensure that the shear strength does not change after being placed at 150°C for 1 month.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of adhesives, and more specifically relates to a one-component adhesive and a preparation method thereof. Background Art

[0002] Adhesive refers to a material with good adhesive properties that can form a thin film between two surfaces and firmly bond them together. It is generally formulated from adhesives, curing agents, toughening agents, diluents and modifiers. Most Chinese adhesive companies were established in the 1980s and 1990s, and started late. However, at this stage, Chinese companies have great development potential in the adhesive industry. Under the background of China's current economic transformation and upgrading, a number of rapidly developing emerging industries have been spawned. For example, there are many good development opportunities for adhesives in the fields of automobiles, packaging, new energy, and construction.

[0003] There are many types of one-component adhesives on the market, but they generally have poor high temperature resistance, oil resistance, and thermal shock resistance. In order to solve the existing problems of one-component adhesives in the automotive field, especially the high temperature resistance and oil resistance of adhesives when bonding metal materials and polymer materials, it is necessary to further optimize and improve the formulation and preparation process of adhesives in the existing technology. This is of great significance to improving the application scope and application value of one-component adhesives. Summary of the invention

[0004] In order to solve the above technical problems, the first aspect of the present invention provides a one-component adhesive, the preparation raw materials of which at least include epoxy resin and / or modified epoxy resin; and also include 0.1-1.5 parts of fumed silica.

[0005] As a preferred technical solution, the weight ratio of the epoxy resin to the modified epoxy resin is 1:(0.5-1.2).

[0006] As a preferred technical solution, the weight ratio of the epoxy resin to the modified epoxy resin is 1:(0.9-1.1).

[0007] As a preferred technical solution, the preparation raw materials also include auxiliary agents; the auxiliary agents are selected from one or more of defoaming agents, curing agents, coupling agents, fillers, and black pastes.

[0008] As a preferred technical solution, the filler is selected from one or more of calcium carbonate, mica powder, talcum powder, and barium carbonate.

[0009] As a preferred technical solution, the weight of the calcium carbonate is 10-60wt% of the weight of the epoxy resin and / or modified epoxy resin.

[0010] As a preferred technical solution, the curing agent is selected from at least one of dicyandiamide, polyamines, and benzoxazine.

[0011] As a preferred technical solution, the polyamine is selected from aromatic amines.

[0012] A second aspect of the present invention provides a method for preparing a one-component adhesive, comprising the following steps:

[0013] 1) Add epoxy resin and / or modified epoxy resin and additives into a stirring kettle, stir and disperse for 15-20 minutes, control the temperature at 15-25°C, and discharge;

[0014] 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature below 25°C;

[0015] 3) Stir the ground material again, control the temperature at 15-25℃, perform vacuum degassing, control the vacuum degree, degas for 20-40min, and then discharge the material.

[0016] As a preferred technical solution, the vacuum degree in step 3) is -0.098~-0.1MPa.

[0017] Beneficial effects: The adhesive prepared by the present invention has the following advantages compared with the prior art:

[0018] 1. The one-component adhesive and the preparation method thereof provided by the present invention have high temperature resistance and impact resistance;

[0019] 2. The one-component adhesive and the preparation method thereof provided by the present invention are simple to operate, have strong storage stability and high economic benefits;

[0020] 3. The one-component adhesive provided by the present invention has high shear strength during use and good bonding performance to metal materials, and has great application prospects in the fields of automobiles, packaging, new energy, construction, etc.;

[0021] 4. The one-component adhesive provided by the present invention solves the problem of "wet inside and dry outside" that occurs during the gluing process, ensures its stability when applied on the surface of materials such as metals, and can ensure that the shear strength does not change after being placed at 150°C for 1 month. DETAILED DESCRIPTION

[0022] The content of the present invention can be more easily understood by selecting the following detailed description of the preferred implementation method of the present invention and the embodiments included. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definition in this specification shall prevail.

[0023] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0024] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0025] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0026] Singular forms include plural references unless the context clearly indicates otherwise. "Optional" or "either" means that the subsequently described event or incident may or may not occur, and that the description includes instances where the event occurs and instances where it does not.

[0027] Approximate terms in the specification and claims are used to modify quantities, indicating that the present invention is not limited to the specific quantity, but also includes acceptable and modified parts close to the quantity without causing changes in the relevant basic functions. Accordingly, the use of "about", "approximately", etc. to modify a numerical value means that the present invention is not limited to the exact numerical value. In some examples, the approximate terms may correspond to the accuracy of the instrument for measuring the numerical value. In the specification and claims of this application, range limitations can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0028] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.

[0029] In order to solve the above problems, the first aspect of the present invention provides a one-component adhesive, the preparation raw materials of which at least include epoxy resin and / or modified epoxy resin; and also include 0.1-1.5 parts of fumed silica.

[0030] In some preferred embodiments, the fumed silica is hydrophobic fumed silica.

[0031] Hydrophobic fumed silica was purchased from Weifang Hengshuo Nanomaterials Co., Ltd.

[0032] In some preferred embodiments, the preparation raw materials include at least epoxy resin and modified epoxy resin.

[0033] The epoxy resin described in the present application is not particularly limited, including but not limited to at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, brominated bisphenol A epoxy resin, p-phenol type glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ether type epoxy resin, and glycidyl amine type epoxy resin.

[0034] In some preferred embodiments, the weight ratio of the epoxy resin to the modified epoxy resin is 1:(0.5-1.2).

[0035] In some preferred embodiments, the weight ratio of the epoxy resin to the modified epoxy resin is 1:(0.9-1.1).

[0036] In some preferred embodiments, the epoxy resin is selected from bisphenol A epoxy resin.

[0037] In some preferred embodiments, the modified epoxy resin is a polyurethane modified epoxy resin.

[0038] There is no particular restriction on the manufacturer of the bisphenol A epoxy resin. For example, it can be purchased from Guangxi Zhe Chuang Chemical Co., Ltd., model E51.

[0039] Polyurethane modified epoxy resin, model EPU-303, was purchased from Luohe High-tech Materials (Shanghai) Co., Ltd.

[0040] During the experiment, the applicant found that in this system, adding epoxy resin to prepare adhesive can improve the high temperature resistance of the adhesive, but the applicant found that when using only one epoxy resin, the adhesive is brittle and cannot meet the requirements of using the adhesive under special conditions such as high temperature. In order to further improve the toughness and tensile shear strength of the adhesive, the applicant has found through a large number of creative experiments that adding epoxy resin and polyurethane modified epoxy resin to this system can further improve the toughness of the adhesive while improving the high temperature stability of the adhesive. The applicant speculates that the possible reason is: under the premise of the presence of epoxy resin, reactive active groups can be provided in the system. When compounded with polyurethane modified epoxy resin, further cross-linking will occur in the system to form a dense three-dimensional network structure. When subjected to external high temperature, the high-frequency movement of the molecular chain is limited due to the constraints of the dense network structure, thereby improving the high temperature stability and toughness of the adhesive.

[0041] In addition, the applicant unexpectedly discovered that when the weight ratio of epoxy resin to polyurethane modified epoxy resin is 1: (0.9-1.1), the tensile shear strength of the adhesive can be improved. The applicant speculates that the possible reason is that as the amount of polyurethane modified epoxy resin added changes, the strength of the interaction between molecules varies greatly. In the range of 1: (0.9-1.1) for the weight ratio of epoxy resin to polyurethane modified epoxy resin, as the content of polyurethane modified epoxy resin increases, the free active groups in the system increase, which can cooperate with the epoxy resin in the system to introduce more branching points on the polyurethane chain segment. When stretched by external force, the force can be evenly dispersed, avoiding the concentration of local stress and improving the tensile shear strength. However, the applicant found that when the added polyurethane content is greater than the scope of protection of this application, it will lead to excessive crosslinking density between molecules, resulting in enhanced rigidity of the molecules and a significant decrease in impact resistance.

[0042] In some preferred embodiments, the preparation raw materials further include auxiliary agents; the auxiliary agents are selected from one or more of defoaming agents, curing agents, coupling agents, fillers, and black pastes.

[0043] In some preferred embodiments, the preparation raw materials further include a defoamer, a curing agent, a coupling agent, a filler, and a black paste.

[0044] In the present application, the black slurry can be made by yourself or purchased; there is no special restriction on the manufacturer, and the preparation method can refer to the following steps:

[0045] Mix carbon black and 128 base resin in a weight ratio of 1:1.8 and grind to obtain the product.

[0046] The carbon black is commonly available on the market, and the 128 base resin is purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0047] In some preferred embodiments, the filler is selected from one or more of calcium carbonate, mica powder, talcum powder, and barium carbonate.

[0048] In some preferred embodiments, the filler is selected from calcium carbonate and mica powder.

[0049] In some preferred embodiments, the weight ratio of calcium carbonate to mica powder is 26:(2-3).

[0050] During the experiment, the applicant found that although the latent curing agent selected for addition improved the stability of the adhesive, the applicant found that the addition of the latent curing agent may cause the adhesive to become "wet inside and dry outside" during use. In order to solve the above-mentioned problem, the applicant found through a lot of creative research that the addition of calcium carbonate and mica powder can solve this problem, especially when the weight ratio of calcium carbonate to mica powder is 26: (2-3), not only will the adhesive not become "wet inside and dry outside", but the shear strength of the adhesive will also be improved. The applicant speculates that this phenomenon may occur. Reasons for the phenomenon: With the addition of calcium carbonate and mica powder into the adhesive, the rheological properties of the adhesive are appropriately adjusted. Under the synergistic effect of silane coupling agents and the like in the system, the stability of calcium carbonate and mica powder in the system is promoted. The addition of mica powder, when its weight ratio is 26: (2-3), can promote the orderly dispersion of calcium carbonate, epoxy resin and curing agent between the mica powder layer structure, promote the transferability between the cured products during the curing process, enhance its curing effect, and avoid the occurrence of "wet inside and dry outside"; thereby improving the shear strength of the adhesive,

[0051] In addition, the applicant has found that when the proportion of added calcium carbonate is greater than the range of the present application, the calcium carbonate particles will agglomerate during the preparation of the adhesive, causing defects inside the adhesive, resulting in reduced shear strength, and limiting the use conditions and scope of the adhesive.

[0052] In some preferred embodiments, the weight of the calcium carbonate is 10-60 wt % of the weight of the epoxy resin and / or modified epoxy resin.

[0053] In some preferred embodiments, the weight of the calcium carbonate is 10-60 wt % of the weight of the epoxy resin and the polyurethane-modified epoxy resin.

[0054] During the experiment, it was found that when the weight of calcium carbonate is 10-60wt% of the total amount of epoxy resin and polyurethane modified epoxy resin, it can promote the stability of its dispersion in the system under the premise of cooperating with mica powder, thereby improving the stability of the adhesive under special conditions. It can ensure that the tensile shear strength does not change after being placed in lubricating oil for 24 hours.

[0055] In some preferred embodiments, the curing agent is selected from at least one of dicyandiamide, polyamines, and benzoxazine.

[0056] In some preferred embodiments, the polyamine is selected from aromatic amines.

[0057] In some preferred embodiments, the aromatic amine is selected from diaminodiphenyl sulfone (CAS: 80-08-0).

[0058] In some preferred embodiments, the weight ratio of polycyanamide, diaminodiphenyl sulfone and benzoxazine is 1:(4-5):1.

[0059] During the experiment, the applicant found that in the preparation process of the one-component adhesive, the type of curing agent selected has an important influence on the stability of the adhesive. Adding dicyandiamide, aromatic amine curing agent, and benzoxazine curing agent to the system can reduce the curing temperature of the one-component curing agent and improve the stability of the adhesive. The applicant found that when diaminodiphenyl sulfone is selected as the aromatic amine curing agent, and the weight ratio of dicyandiamide, diaminodiphenyl sulfone, and benzoxazine is 1: (4-5): 1, the storage stability of the adhesive can be ensured, and the tensile shear strength of the adhesive can be kept at 150°C for 1 month without changing. The applicant speculates that the possible reason is that the sulfone group in the diaminodiphenyl sulfone structure tends to attract electrons on the benzene ring, causing the benzene ring to lack electrons. When dicyandiamide and benzoxazine act synergistically in the system, it can more easily combine with the electron-donating group in the system to form a stable structure, thereby improving the storage stability of the adhesive. In the epoxy resin and modified epoxy resin system, it is ensured that the adhesive can be placed at 150°C for 1 month without changing its tensile shear strength.

[0060] In addition, the applicant has found that if the weight ratio of the diamine curing agent added to the system exceeds the range of the present application, the water resistance of the adhesive will decrease.

[0061] In some preferred embodiments, the raw materials for preparing the one-component adhesive include, by weight: 20-35 parts of epoxy resin, 25-40 parts of modified epoxy resin, 0.1-1 parts of fumed silica, 1-5 parts of black paste, 0.001-0.005 parts of defoaming agent, 0.05-0.5 parts of coupling agent, 5-20 parts of curing agent, and 25-50 parts of filler.

[0062] A second aspect of the present invention provides a method for preparing a one-component adhesive, comprising the following steps:

[0063] 1) Add epoxy resin and / or modified epoxy resin and additives into a stirring kettle, stir and disperse for 15-20 minutes, control the temperature at 15-25°C, and discharge;

[0064] 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature below 25°C;

[0065] 3) Stir the ground material again, control the temperature at 15-25℃, perform vacuum degassing, control the vacuum degree, degas for 20-40min, and then discharge the material.

[0066] In some preferred embodiments, the vacuum degree in step 3) is -0.098 to -0.1 MPa.

[0067] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the above content of the present invention still belong to the scope of protection of the present invention.

[0068] In addition, unless otherwise stated, all raw materials used were commercially available.

[0069] Example

[0070] Example 1

[0071] A one-component adhesive is prepared by raw materials, which are calculated by weight: 20 parts of epoxy resin, 25 parts of modified epoxy resin, 0.1 parts of fumed silica, 1 part of black paste, 0.001 parts of defoaming agent, 0.05 parts of coupling agent, 5 parts of curing agent and 25 parts of filler.

[0072] The epoxy resin is bisphenol A epoxy resin, model E51, purchased from Guangxi Zhechuang Chemical Co., Ltd.

[0073] The modified epoxy resin is a polyurethane modified epoxy resin, model EPU-303, purchased from Luohe High-tech Materials (Shanghai) Co., Ltd.;

[0074] The fumed silica is hydrophobic silica, purchased from Weifang Hengshuo Nanomaterials Co., Ltd.

[0075] The black slurry is homemade in an experiment, and the preparation method is: mix carbon black and 128 base resin in a weight ratio of 1:1.8, grind, and obtain the black slurry.

[0076] The 128 base resin was purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0077] The defoamer, model BYK-016, was purchased from Shanghai Kaiyin Chemical Co., Ltd.

[0078] The coupling agent is selected from KH-560;

[0079] The curing agent is selected from polycyanamide, diaminodiphenyl sulfone and benzoxazine, and the weight ratio thereof is 1:4:1.

[0080] The filler is selected from calcium carbonate and mica powder, and the weight ratio thereof is 26:2.3.

[0081] A method for preparing a one-component adhesive comprises the following steps:

[0082] 1) Add epoxy resin and modified epoxy resin, defoamer and coupling agent into a stirring kettle, stir and disperse for 20 minutes, then add calcium carbonate and mica powder, disperse for 20 minutes, then add fumed silica, disperse for 45 minutes, control the temperature at 20°C, then add curing agent, disperse for 30 minutes, control the temperature at 20°C, and discharge;

[0083] 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature at 20°C;

[0084] 3) Stir the ground material again, control the temperature to 22°C, perform vacuum degassing, control the vacuum degree to -0.099MPa, degas for 30 minutes, and discharge the material.

[0085] Example 2

[0086] A one-component adhesive is prepared by preparing raw materials, which include, by weight: 35 parts of epoxy resin, 40 parts of modified epoxy resin, 1 part of fumed silica, 5 parts of black paste, 0.005 parts of defoaming agent, 0.5 parts of coupling agent, 20 parts of curing agent and 50 parts of filler.

[0087] The epoxy resin is bisphenol A epoxy resin, model E51, purchased from Guangxi Zhechuang Chemical Co., Ltd.

[0088] The modified epoxy resin is a polyurethane modified epoxy resin, model EPU-303, purchased from Luohe High-tech Materials (Shanghai) Co., Ltd.;

[0089] The fumed silica is hydrophobic silica, purchased from Weifang Hengshuo Nanomaterials Co., Ltd.

[0090] The black slurry is homemade in an experiment, and the preparation method is: mix carbon black and 128 base resin in a weight ratio of 1:1.8, grind, and obtain the black slurry.

[0091] The 128 base resin was purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0092] The defoamer, model BYK-016, was purchased from Shanghai Kaiyin Chemical Co., Ltd.

[0093] The coupling agent is selected from KH-560;

[0094] The curing agent is selected from polycyanamide, diaminodiphenyl sulfone, and benzoxazine, and the weight ratio thereof is 1:5:1.

[0095] The filler is selected from calcium carbonate and mica powder, and the weight ratio thereof is 26:3.

[0096] A method for preparing a one-component adhesive comprises the following steps:

[0097] 1) Add epoxy resin and modified epoxy resin, defoamer and coupling agent into a stirring kettle, stir and disperse for 20 minutes, then add calcium carbonate and mica powder, disperse for 20 minutes, then add fumed silica, disperse for 45 minutes, control the temperature at 20°C, then add curing agent, disperse for 30 minutes, control the temperature at 20°C, and discharge;

[0098] 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature at 20°C;

[0099] 3) Stir the ground material again, control the temperature to 22°C, perform vacuum degassing, control the vacuum degree to -0.099MPa, degas for 30 minutes, and discharge the material.

[0100] Example 3

[0101] A one-component adhesive is prepared by preparing raw materials, which, by weight, include: 27 parts of epoxy resin, 29 parts of modified epoxy resin, 0.6 parts of fumed silica, 2.3 parts of black paste, 0.003 parts of defoaming agent, 0.2 parts of coupling agent, 12 parts of curing agent and 28.9 parts of filler.

[0102] The epoxy resin is bisphenol A epoxy resin, model E51, purchased from Guangxi Zhechuang Chemical Co., Ltd.

[0103] The modified epoxy resin is a polyurethane modified epoxy resin, model EPU-303, purchased from Luohe High-tech Materials (Shanghai) Co., Ltd.;

[0104] The fumed silica is hydrophobic silica, purchased from Weifang Hengshuo Nanomaterials Co., Ltd.

[0105] The black slurry is homemade in an experiment, and the preparation method is: mix carbon black and 128 base resin in a weight ratio of 1:1.8, grind, and obtain the black slurry.

[0106] The 128 base resin was purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0107] The defoamer, model BYK-016, was purchased from Shanghai Kaiyin Chemical Co., Ltd.

[0108] The coupling agent is selected from KH-560;

[0109] The curing agent is selected from polycyanamide, diaminodiphenyl sulfone, and benzoxazine, and the weight ratio thereof is 1:4.6:1.

[0110] The filler is selected from calcium carbonate and mica powder, and the weight ratio thereof is 26:2.9.

[0111] A method for preparing a one-component adhesive comprises the following steps:

[0112] 1) Add epoxy resin and modified epoxy resin, defoamer and coupling agent into a stirring kettle, stir and disperse for 20 minutes, then add calcium carbonate and mica powder, disperse for 20 minutes, then add fumed silica, disperse for 45 minutes, control the temperature at 20°C, then add curing agent, disperse for 30 minutes, control the temperature at 20°C, and discharge;

[0113] 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature at 20°C;

[0114] 3) Stir the ground material again, control the temperature to 22°C, perform vacuum degassing, control the vacuum degree to -0.099MPa, degas for 30 minutes, and discharge the material.

[0115] Example 4

[0116] A one-component adhesive, the specific implementation of which is the same as that of Example 3, except that the weight ratio of the epoxy resin to the polyurethane modified resin is 1:2.

[0117] Example 5

[0118] A one-component adhesive, whose specific implementation method is the same as that of Example 3, except that the polyurethane-modified epoxy resin is replaced by a bisphenol A epoxy resin, and the bisphenol A epoxy resin is the same as that in the example.

[0119] Example 6

[0120] A one-component adhesive, the specific implementation of which is the same as that of Example 3, except that the weight ratio of polycyanamide, diaminodiphenyl sulfone and benzoxazine is 1:1:1.

[0121] Example 7

[0122] A one-component adhesive, the specific implementation of which is the same as that of Example 3, except that the weight ratio of polycyanamide, diaminodiphenyl sulfone and benzoxazine is 1:6:1.

[0123] Example 8

[0124] A one-component adhesive, the specific implementation of which is the same as that of Example 3, except that the weight ratio of polycyanamide, diaminodiphenyl sulfone and benzoxazine is 1:1:4.

[0125] Example 9

[0126] A one-component adhesive, the specific implementation of which is the same as that of Example 3, except that the filler does not contain mica powder.

[0127] Example 10

[0128] A one-component adhesive, whose specific implementation is the same as that of Example 3, except that the weight ratio of calcium carbonate to mica powder is 1:1.

[0129] Performance Testing:

[0130] Before testing, bonding is performed first. Before bonding, the bonding area should be cleaned and dried. The adhesive should be evenly applied to the bonding surface. Then the objects should be bonded. The bonded products and the bonding area should be placed horizontally and placed in an oven. The curing conditions are 120℃ / 15min. After the above operations are completed, the performance test should be performed.

[0131] 1. Tensile shear strength test: The adhesives prepared in Examples 1-10 were used for tensile shear strength test. The test method was based on GB / T7124-1986. 45# steel was selected as the tensile test piece. The test results are summarized in the table below.

[0132] 2. Tensile shear strength test at 150°C: Place at 150°C for 1 month, and then test it according to the test method of Test 1 to determine the change in the data compared with Test 1, and report the results in the table below.

[0133] 3. High temperature resistance: The adhesives prepared in Examples 1-10 were placed at 200°C for 30 minutes and then subjected to a tensile shear strength test. The test standard referred to the method of Test 1, and the data decreased compared to Test 1, and the results were statistically reported in the table below.

[0134] 4. Impact resistance test: The test standard refers to GB / T 1732-93, and the test results are statistically shown in the table below.

[0135]

[0136] 5. Oil resistance: The adhesives prepared in Examples 1-3 were used for tensile shear strength test. The test method was based on GB / T7124-1986. After the test, ten pieces were placed in lubricating oil for 24 hours. After being taken out, the tensile shear strength test was performed again. The changes in tensile shear strength were recorded in the table below.

[0137]

[0138] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A one-component adhesive, characterized in that: The preparation raw materials include at least epoxy resin and modified epoxy resin; and also include 0.1-1.5 parts of fumed silica; The weight ratio of the epoxy resin to the modified epoxy resin is 1:(0.9-1.1); The modified epoxy resin is polyurethane modified epoxy resin, model EPU-303; The preparation raw materials also include fillers, and the fillers are selected from calcium carbonate and mica powder, and the weight ratio of calcium carbonate to mica powder is 26: (2-3); The epoxy resin is selected from bisphenol A epoxy resin, model E51; The adhesive further comprises a curing agent; The curing agent is selected from dicyandiamide, diaminodiphenyl sulfone, and benzoxazine, and the weight ratio of dicyandiamide, diaminodiphenyl sulfone, and benzoxazine is 1:(4-5):

1.

2. The one-component adhesive according to claim 1, characterized in that: The preparation raw materials also include auxiliary agents; the auxiliary agents are selected from one or more compounds of defoaming agents, coupling agents, and black paste.

3. The one-component adhesive according to claim 1, characterized in that: The weight of the calcium carbonate is 10-60wt% of the weight of the epoxy resin and the modified epoxy resin.

4. A method for preparing a one-component adhesive according to claim 2, characterized in that: The following steps are involved: 1) Add epoxy resin and modified epoxy resin, curing agent, fumed silica and additives into a stirring kettle, stir and disperse for 15-20 minutes, control the temperature at 15-25°C, and discharge; 2) Grinding the material obtained in step 1) on a three-roll mill, controlling the temperature below 25°C; 3) Stir the ground material again, control the temperature at 15-25℃, perform vacuum degassing, control the vacuum degree, degas for 20-40min, and then discharge the material.

5. The method for preparing a one-component adhesive according to claim 4, characterized in that: The vacuum degree in step 3) is -0.098~-0.1MPa.