An experimental method for testing the crack propagation at the cement sheath interface
By simulating the underground environment in the pressure-bearing sleeve and combining the principle of acoustic variable density logging, the cement sheath interface crack expansion is quantitatively characterized, which solves the problem of cement sheath interface crack expansion testing in the existing technology and improves the efficiency of cement sheath sealing performance evaluation. accuracy.
Patent Information
- Application Number
- CN202210309264.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Existing technology cannot directly conduct quantitative testing of cement sheath interface crack expansion, and theoretical research lacks experimental verification, resulting in inaccurate evaluation of cement sheath sealing performance.
Through the equivalent process of geometric similarity, equal stress and the same process, the underground high-temperature and high-pressure environment is simulated, and the cement sheath interface crack propagation is tested in the pressure-bearing sleeve. Combined with the principle of acoustic variable density logging, the first and second interface cracks of the cement sheath are quantitatively characterized. Extension.
This method achieves direct quantitative characterization of crack growth at the cement sheath interface, analyzes the effects of initial crack length and mechanical properties on crack growth, verifies theoretical research results, and provides reference value for long-term sealing evaluation of cement sheaths.
Smart Images

Figure CN114776278B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas wellbore integrity testing, and more particularly to an experimental method for testing the expansion of cracks at the cement sheath interface of a well cementing device. Background Art
[0002] During the oil and gas cementing process, cement will be filled in the annular space between the casing and the wellbore. The cement ring formed after solidification has the function of supporting the well wall, protecting the casing, and isolating the oil, gas and water layers. In the subsequent drilling and production process, complex working loads can easily damage the mechanical integrity of the cement ring. Especially under fracturing conditions, interface cracks will occur at the first and second interfaces of the cement ring. The fracturing fluid will not only enter the formation cracks through the perforations, but also enter the cement ring interface cracks. The cracks generated at the interface are prone to further expansion under the action of high-pressure fracturing fluid. In severe cases, the cement ring will fail to be sealed, causing interlayer crossflow, annular pressure and other problems. Therefore, effectively predicting the extension degree of interface cracks is of vital importance for the long-term isolation of the cement ring and evaluating the isolation capacity of the cement ring.
[0003] The publication date is June 19, 2020, the publication number is CN111307690A, and the invention patent application named "A sealing performance test device and method for cement ring in the annulus of oil and gas wells" is published. It discloses a sealing performance test device and method for cement ring in the annulus of oil and gas wells. The device includes a pressure-bearing cylinder, a top cover and a base. The device is provided with an internal pressure casing, a cement ring and an external pressure cylinder. The device is provided with a heating sleeve, a temperature sensor, a nitrogen inlet interface, a permeability detection module joint, an internal pressure joint, an equivalent crack width detection module joint, annulus pressure conductivity coefficient detection module joint, annulus inlet joint, a flow monitoring meter joint, annular pressure outlet joint, annular pressure control system, annular pressure conductivity coefficient detection module, equivalent crack width detection module, internal pressure control system, nitrogen bottle, permeability detection module, temperature control system, flow monitoring meter, valve, and computer control system. The invention solves the problem of physical equivalence of cement ring load and the problem of quantitative monitoring of cement ring sealing performance. However, it cannot be used for cementing cement ring interface crack expansion experiment.
[0004] In the study of cement sheath interface crack expansion, there is no good experimental device or scheme to directly test it at home and abroad. At present, the research is mainly based on mathematical calculation models and software simulation. Although the theoretical research on cement sheath interface cracks is relatively mature, the theoretical parameters calculated by the model and software lack credibility in characterizing the degree of cement sheath interface crack expansion, and there are still certain differences from the actual evolution of cement sheath interface cracks in the actual well. Therefore, starting from the theoretical method alone is not comprehensive enough and cannot meet the requirements of characterization performance. Theoretical research results often need to be verified by experimental devices. Only by combining theory with experimental testing can the actual development of cement sheath interface crack expansion be effectively promoted and valuable targeted guidance can be provided to the oil field site. Summary of the invention
[0005] In order to overcome the defects and deficiencies in the above-mentioned prior art, the present invention provides an experimental method for testing the crack expansion of the cement ring interface of cementing wells, so as to solve the problem of quantitative monitoring of the interface crack expansion of cement ring under complex loading conditions in underground wells. According to the actual cement ring under fracturing conditions, the present invention is equivalent to the experimental cement ring through three processes of geometric similarity, stress equality and same process, and the size, stress and simulated fracturing load of the experimental cement ring are calculated. When prefabricating the cement ring, the first interface and / or second interface cracks of the cement ring are prefabricated, and then the cement ring assembly is placed in a pressure sleeve to simulate the real underground high temperature and high pressure cement ring loading environment, and combined with the principle of acoustic variable density logging, the expansion of the first and second interface cracks of the cement ring is quantitatively characterized, and the influence of the initial seam length, casing eccentricity and mechanical properties of the cement ring on the expansion of the interface crack can be analyzed, and the theoretical research results can be experimentally verified.
[0006] In order to solve the above problems existing in the prior art, the present invention is implemented through the following technical solutions.
[0007] The present invention provides an experimental method for testing the expansion of cracks at the interface of cement sheath of a well cementing device, the method comprising the following steps:
[0008] S1. Before the experiment begins, the actual cement sheath under the fracturing condition needs to be equivalent to the experimental cement sheath through three processes: geometric similarity, stress equality and same process, and the size, stress and simulated fracturing load on the experimental cement sheath are calculated; the same process means the same fracturing process.
[0009] S2. Prepare corresponding cement slurry according to the experimental requirements and GB / T10238 standard, and inject it into the cement ring curing mold. The cone ring sleeve on the base of the curing mold can preform the first interface and / or second interface cracks of the cement ring at the bottom of the cement ring. Place the curing mold in a high-temperature and high-pressure curing kettle for curing to a set age, and take out the internal pressure casing, simulated surrounding rock casing and cement ring in the curing mold together to form an "internal pressure casing-cement ring-simulated surrounding rock casing" combination;
[0010] The cement ring is a brittle material. If cracks are artificially added after curing, it is easy to damage the internal stress of the cement stone. In the present application, when the cement slurry is still in liquid state, the first interface and / or second interface cracks are preformed by the cone ring sleeve on the base of the curing mold, which can avoid the problem of artificial cracks changing the internal stress of the cement ring after curing.
[0011] S3, placing the assembly obtained in step S2 in a sealed pressure-bearing sleeve, forming a confining pressure annulus between the outer wall of the simulated surrounding rock casing of the assembly and the inner wall of the pressure-bearing sleeve; a certain space is provided between the prefabricated cement ring with one interface and / or two interface cracks and the upper and lower ends of the assembly, and a cement ring bottom annulus and a cement ring top annulus are formed between the top cover and the base of the pressure-bearing sleeve respectively; a casing inner cavity is formed between the internal pressure casing of the assembly and the top cover and the base of the pressure-bearing sleeve.
[0012] S4. An external heater is installed in the confining pressure annulus, an internal heater is installed in the inner cavity of the casing, and the external heater and the internal heater are connected to the temperature control system; the confining pressure annulus, the annulus at the bottom of the cement ring, the annulus at the top of the cement ring and the inner cavity of the casing are connected to the pressure control system; a coupling drive is installed in the inner cavity of the casing, and a sonic wave transmitter, a 3H sonic wave receiver and a 5H sonic wave receiver are installed at the lower end of the coupling drive in sequence; the sonic wave transmitter and the 3H sonic wave receiver are 3Hcm apart, and the sonic wave transmitter and the 5H sonic wave receiver are 5Hcm apart; the coupling drive is installed in the inner cavity of the casing and maintained Vertically center; connect the sound wave generator, 3H sound wave receiver and 5H sound wave receiver to the sound wave signal processing system; establish data connection between the temperature control system, pressure control system and sound wave signal processing system and the computer control system; the 3H sound wave receiver and the 5H sound wave receiver respectively represent the sound wave receiver at a distance of 3 units from the sound wave transmitter and the sound wave receiver at a distance of 5 units from the sound wave transmitter; to ensure that the sound wave receiver can receive the complete waveform; setting up two receivers also ensures that the complete sound wave signal of the combination can be fully received.
[0013] S5. The computer control system controls the pressure control system to simultaneously inject liquid medium into the confining pressure annulus, the annulus at the bottom of the cement ring and the inner cavity of the casing according to the fracturing load data calculated in step S1 to exhaust the air therein; when the inner cavity of the casing and the confining pressure annulus are filled with the liquid medium, the drain valves of the inner cavity of the casing and the confining pressure annulus are closed;
[0014] The computer control system controls the temperature control system, sets the heating time, and uses the internal heater and the external heater to uniformly heat the cement sheath assembly. As the temperature increases, the casing cavity pressure, the cement sheath bottom annulus pressure, and the confining pressure annulus pressure will all increase; at the same time, the computer control system sets the pressure increase time in the pressure control system to be consistent with the heating time, and uniformly and continuously pressurizes the casing cavity, the cement sheath bottom annulus, and the confining pressure annulus. After the heating and pressure increase, the temperature is controlled at the target temperature, and the confining pressure annulus pressure is controlled at the target confining pressure, and they are maintained;
[0015] Among them, heating and pressure increase requires a process and cannot be achieved instantly, so a certain time needs to be set to reach the required target value. The heating time and pressure increase time are kept consistent here because the actual underground cement ring itself is in a certain temperature and pressure environment, so we also need to evenly raise the temperature and pressure environment of the cement ring to the target value during the experiment, so the control time is consistent.
[0016] After the pressure of the confining annulus is stable, the pressure injection of the confining annulus is closed; the casing cavity and the annulus at the bottom of the cement ring are continuously and evenly pressurized until the casing cavity pressure and the annulus pressure at the bottom of the cement ring reach the target internal pressure, and then the casing cavity pressure, the confining annulus pressure and the annulus pressure at the bottom of the cement ring are kept stable for a period of time;
[0017] Among them, the pressure injection of closing the confining pressure annulus is because when we start the experiment, the confining pressure annulus is without pressure. However, the actual downhole cement sheath itself will be subjected to the confining pressure from the formation during the fracturing process. Therefore, the purpose here is actually to proceed in two steps. The first step is to allow the temperature and pressure of the experimental cement sheath to rise to the target value we need, and then maintain this temperature and pressure environment to start the second step, which is to simulate the fracturing process. At this time, the confining pressure needs to be stabilized, and the internal pressure and the ring pressure at the bottom of the cement sheath need to continue to increase (to simulate the fracturing process) to observe whether the cracks at the cement sheath interface expand and to what extent.
[0018] S6. The computer control system controls the start-up of the acoustic signal processing system. The acoustic wave transmitter is used to transmit acoustic wave pulses, which are received by the 3H acoustic wave receiver and the 5H acoustic wave receiver after passing through the internal pressure casing, cement sheath and simulated surrounding rock casing. The 3H acoustic wave receiver and the 5H acoustic wave receiver send the acquired full-wave waveform data to the full-wave waveform data collector of the acoustic signal processing system. Then the full-wave waveform data collector transmits the recorded data to the digital oscilloscope. After processing by the digital oscilloscope, it is sent to the instantaneous waveform collector. After that, the waveform data is converted into the cement sheath interface bonding strength signal through the instantaneous waveform converter to determine whether cracks are generated here.
[0019] S7. The computer control system controls the coupling drive action to drive the acoustic wave transmitter, 3H acoustic wave receiver and 5H acoustic wave receiver to move at a uniform speed along the axial direction of the internal pressure casing, measure multiple sections of continuous crack signals that change with time, and finally transmit them to the computer control system to generate the cement sheath first interface and / or second interface crack extension length curve.
[0020] Furthermore, the computer control system starts the acoustic signal processing system and uses the pressure control system to monitor the annular pressure at the top of the cement sheath; once the cement sheath fails, the liquid medium will enter the annular space at the top of the cement sheath to generate hydraulic pressure, and the sensor will record the pressure value and transmit it to the pressure control system, and finally transmit it to the computer control system to generate a cement sheath top annular pressure curve, so as to determine whether the cement sheath interface has failed.
[0021] Furthermore, after the test is completed, the computer control system saves the experimental data, turns off the acoustic signal processing system and the temperature control system, and waits until the temperature inside the pressure sleeve drops to room temperature. The pressure control system is then used to remove the pressure in the casing cavity, the annulus at the bottom of the cement ring, and the confining pressure annulus. The pressure control system is then turned off, the corresponding joints and pipelines of each control system are removed, the top cover of the pressure sleeve is removed, the cement ring assembly is taken out, and the experiment is completed.
[0022] Furthermore, the maintenance mold includes an internal pressure sleeve, a simulated surrounding rock sleeve, a mold top cover and a mold base, the internal pressure sleeve is placed in the simulated surrounding rock sleeve, and the upper and lower ends of the internal pressure sleeve are respectively connected to the slots of the mold top cover and the mold base; the mold top cover and the mold base are respectively fixedly connected to the upper and lower ends of the simulated surrounding rock sleeve by fasteners; a cone ring sleeve for prefabricating cement ring interface cracks is provided on the slot of the base, and the cone ring sleeve is any one of three types of cone ring sleeves; the three types of cone ring sleeves are cone ring sleeve I for prefabricating cement ring one interface crack, cone ring sleeve II for prefabricating cement ring two interface cracks and cone ring sleeve III for prefabricating both cement ring one interface crack and two interface cracks.
[0023] The contact surface of the cone ring sleeve that contacts the cement ring is coated with heat-resistant degreasing oil.
[0024] The internal pressure casing is coaxially arranged with the simulated surrounding rock casing and is used for preparing a circular cement ring.
[0025] The internal pressure casing and the simulated surrounding rock casing are eccentrically arranged to prepare an eccentric cement ring.
[0026] The temperature control system is provided with three connection ports, which are respectively connected to the inner coupling temperature sensor, the outer coupling temperature sensor and the computer control system. The inner heater is located in the inner cavity of the casing and is assembled on the base of the pressure sleeve. The outer heater is located in the confining pressure annulus and is assembled on the base of the pressure sleeve. The temperature control system controls the heating power of the inner heater through the inner coupling temperature sensor and the heating power of the outer heater through the outer coupling temperature sensor. The inner heater and the outer heater are heated simultaneously to ensure that the cement sheath is evenly heated.
[0027] The pressure control system is provided with eight connection ports, which are respectively connected to the internal pressure sensor, the internal pressure joint, the cement ring bottom annulus pressure sensor, the cement ring bottom annulus joint, the cement ring top annulus pressure sensor, the confining pressure annulus pressure sensor, the confining pressure annulus joint and the computer control system; wherein the internal pressure sensor is located on the hydraulic pipeline between the internal pressure control valve and the internal pressure joint, and the internal pressure joint is used to inject liquid medium into the inner cavity of the casing; the cement ring bottom annulus pressure sensor is located on the hydraulic pipeline between the cement ring bottom annulus pressure control valve and the cement ring bottom annulus joint, and the cement ring bottom annulus joint is used to inject liquid medium into the cement ring bottom annulus; the confining pressure annulus pressure sensor is located on the hydraulic pipeline between the confining pressure annulus pressure control valve and the confining pressure annulus joint, and the confining pressure annulus joint is used to inject liquid medium into the confining pressure annulus.
[0028] An internal pressure drain valve is arranged at the top cover above the inner cavity of the casing, and a confining pressure annulus drain valve is arranged at the top cover above the confining pressure annulus.
[0029] Compared with the prior art, the beneficial technical effects brought by the present invention are as follows:
[0030] 1. Regarding the research on cement sheath interface cracks, theoretical research is still the main focus, and there is a lack of a device that can directly conduct quantitative testing on it. The present invention can simulate the real underground high-temperature and high-pressure cement sheath working load environment, and combine the principle of acoustic variable density logging to quantitatively characterize the expansion of cement sheath-to-cement interface cracks, analyze the effects of initial crack length, casing eccentricity, and cement sheath mechanical properties on interface crack expansion, and experimentally verify the theoretical research results.
[0031] 2. The present invention can indirectly evaluate the damage degree of the cement sheath under complex working conditions such as fracturing by testing the extension degree of the crack at the cement sheath-two interface. The measured physical parameters can also be integrated into the software interface of the computer processing system, which is convenient for operators to directly observe. The instrument is easy to install, disassemble and operate, and is also easy to process and manufacture.
[0032] 3. The present invention provides a cement sheath interface crack expansion test and provides a cement sheath assembly curing mold containing corresponding prefabricated cracks, so as to more accurately test the expansion degree of the cement sheath interface crack, and provide reference value for the long-term sealing evaluation of the cement sheath under complex working conditions.
[0033] 4. The maintenance mold in the present invention can simulate different types of combined structures with initial seam lengths according to the actual fracturing working environment of the downhole cement ring. The maintenance mold is simple in design, easy to process and convenient to use.
[0034] 5. The contact surface of the cone ring sleeve and the cement ring is coated with heat-resistant degreasing oil to facilitate the separation of the cone ring sleeve and the cement ring to form the initial seam length. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a structural schematic diagram of an experimental device for testing the expansion of cracks at the interface of cement sheath of a well cementing according to the present invention;
[0036] Figure 2 It is a schematic diagram of the structure of the combined body curing mold containing the first and second interface cracks of the cement sheath under the condition of the vertical well section provided by the present invention;
[0037] Figure 3 It is a schematic diagram of the structure of the combined body curing mold containing cement sheath-interface cracks under the condition of vertical well section provided by the present invention;
[0038] Figure 4 It is a schematic diagram of the structure of the combined body curing mold containing cement sheath second interface cracks under the condition of vertical well section provided by the present invention;
[0039] Figure 5 It is a schematic diagram of the structure of the combined body curing mold containing the first and second interface cracks of the cement sheath under the condition of the eccentric well section provided by the present invention;
[0040] Figure 6 It is a schematic diagram of the structure of the combined body curing mold containing cement sheath-interface cracks under the condition of an eccentric well section provided by the present invention;
[0041] Figure 7 It is a schematic diagram of the structure of the combined body curing mold containing cement sheath second interface cracks under the condition of an eccentric well section provided by the present invention;
[0042] Figure 8 It is a schematic diagram of the test results of the cement sheath interface crack with an initial crack length of l1 provided by the present invention;
[0043] Fig. 9 It is a schematic diagram of the test results of the cement sheath interface crack with an initial crack length of l2 provided by the present invention;
[0044] Fig.10It is a schematic diagram of the test results of the cement sheath interface crack with an initial crack length of l3 provided by the present invention;
[0045] Figure numerals: 1, top cover, 2, base, 3, pressure sleeve, 4, internal pressure casing, 5, cement ring, 6, simulated surrounding rock casing, 7, acoustic wave transmitter, 8, 3H acoustic wave receiver, 9, 5H acoustic wave receiver, 10, coupling drive, 11, acoustic wave signal transmission joint, 12, acoustic wave signal processing system, 13, internal heater, 14, internal coupling temperature sensor, 15, external heater, 16, external coupling temperature sensor, 17, temperature control system, 18, internal pressure control valve, 19, internal pressure sensor, 20, internal pressure joint, 21, internal pressure drain valve, 22, cement ring bottom annulus pressure force control valve, 23. cement ring bottom annulus pressure sensor, 24. cement ring bottom annulus joint, 25. cement ring top annulus pressure sensor, 26. confining pressure annulus pressure control valve, 27. confining pressure annulus pressure sensor, 28. confining pressure annulus joint, 29. confining pressure annulus drain valve, 30. pressure control system, 31. computer control system, 32. mold top cover, 33. mold base, 34. cone ring sleeve I, 35. cone ring sleeve II, 36. cone ring sleeve III, 37. confining pressure annulus, 38. cement ring bottom annulus, 39. cement ring top annulus, 40. casing cavity. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] As a preferred embodiment of the present invention, refer to the attached specification Figure 1As shown, this embodiment discloses an experimental device suitable for the experimental method for testing the interface crack extension of cement sheath in cementing wells according to the present invention, and the experimental device includes a top cover 1, a base 2, a pressure sleeve 3, an internal pressure casing 4, a cement sheath 5, a simulated surrounding rock casing 6, an acoustic wave transmitter 7, a 3H acoustic wave receiver 8, a 5H acoustic wave receiver 9, a coupling drive 10, an acoustic wave signal transmission joint 11, an acoustic wave signal processing system 12, an internal heater 13, an internal coupling temperature sensor 14, an external heater 15, an external coupling temperature sensor 16, a temperature control system 17, an internal pressure control valve 18, an internal pressure sensor 19, an internal pressure joint 20, an internal pressure drain valve 21, an annular space pressure control valve 22 at the bottom of the cement sheath, an annular space pressure sensor 23 at the bottom of the cement sheath, an annular space joint 24 at the bottom of the cement sheath, an annular space pressure sensor 25 at the top of the cement sheath, a confining pressure annular space pressure control valve 26, a confining pressure annular space pressure sensor 27, a confining pressure annular space joint 28, a confining pressure annular space drain valve 29, a pressure control system 30 and a computer control system 31.
[0049] The top cover 1 is tightly connected to the pressure sleeve 3 through the upper thread, and the base 2 is tightly connected to the pressure sleeve 3 through the lower thread. The internal pressure casing 4, cement ring 5 and simulated surrounding rock casing 6 form a simulated wellbore assembly, the cement ring has an inner diameter of D1cm, an outer diameter of D2cm, and a length of L1cm. The bottom of the cement ring contains prefabricated initial cracks at the first interface and / or the second interface, the purpose is to simulate the cracks generated at the first interface and / or the second interface of the cement ring during the fracturing and perforating process, the first interface crack width of the cement ring is D3cm, the crack length is L2cm, the second interface crack width of the cement ring is D4cm, the crack length is L3cm, and D2>D1≥D3+D4, L1≥L2+L3 are satisfied.
[0050] The acoustic signal processing system 12 is provided with two connection ports, one end of which is connected to the coupling drive 10 through the acoustic signal transmission connector 11, and the other end is connected to the computer control system 31; the lower end of the coupling drive is connected to the acoustic wave transmitter 7, the 3H acoustic wave receiver 8 and the 5H acoustic wave receiver 9 in sequence, the acoustic wave transmitter is 3Hcm away from the 3H acoustic wave receiver, and the acoustic wave transmitter is 5Hcm away from the 5H acoustic wave receiver; the coupling drive is placed in the inner cavity of the casing and kept vertically centered, and the coupling drive can be raised and lowered at a uniform speed, thereby controlling the absolute positions of the acoustic wave transmitter and the receiver, and realizing the purpose of continuous monitoring of the one-two interface cracks of the cement sheath.
[0051] The acoustic signal processing system 12 includes a full-wave waveform data collector, a digital oscilloscope, an instantaneous waveform collector, and an instantaneous waveform converter. Its working method adopts the principle of acoustic variable density logging. The principle of testing the extension length of the cement sheath one-two interface crack is roughly as follows: the acoustic wave transmitter 7 transmits an acoustic wave pulse, which is received by a 3H acoustic wave receiver 8 and a 5H acoustic wave receiver 9 after passing through the casing, the cement sheath and the simulated surrounding rock casing. The full-wave waveform data obtained by the receiver is sent to the full-wave waveform data collector through the acoustic wave signal transmission connector. Then the collector transmits the recorded data to the digital oscilloscope, which is processed by the digital oscilloscope and sent to the instantaneous waveform collector. After that, the waveform data is converted into a cement sheath interface bonding strength signal through the instantaneous waveform converter to determine whether a crack is generated here. When the acoustic wave transmitter and the receiver move along the axial direction of the casing, two sections of continuous crack signals that change with time are measured, and finally transmitted to the computer control system 31 to generate a cement sheath one-two interface crack extension length curve.
[0052] The temperature control system 17 is provided with three connection ports, which are respectively connected to the inner coupling temperature sensor 14, the outer coupling temperature sensor 16 and the computer control system 31; the inner heater 13 is located in the inner cavity of the casing and is placed on the base of the kettle body, and the outer heater 15 is located in the confining pressure annulus and is placed on the base of the kettle body. The temperature control system controls the heating power of the inner heater through the inner coupling temperature sensor, and controls the heating power of the outer heater through the outer coupling temperature sensor. The simultaneous heating inside and outside ensures that the cement ring is evenly heated.
[0053] The internal pressure drain valve 21 is located at the top cover above the inner cavity of the casing, and the confining pressure annulus drain valve 29 is located at the top cover above the confining pressure annulus.
[0054] The pressure control system 30 is provided with eight connection ports, which are respectively connected to the internal pressure sensor 19, the internal pressure joint 20, the cement ring bottom annulus pressure sensor 23, the cement ring bottom annulus joint 24, the cement ring top annulus pressure sensor 25, the confining pressure annulus pressure sensor 27, the confining pressure annulus joint 28 and the computer control system 31; wherein the internal pressure sensor is located on the hydraulic pipeline between the internal pressure control valve 18 and the internal pressure joint, the cement ring bottom annulus pressure sensor is located on the hydraulic pipeline between the cement ring bottom annulus pressure control valve 22 and the cement ring bottom annulus joint, and the confining pressure annulus pressure sensor is located on the hydraulic pipeline between the confining pressure annulus pressure control valve 26 and the confining pressure annulus joint. The cement ring top annulus pressure sensor is mainly used to determine whether the cement ring has a channeling failure. Once the cement ring has a channeling failure, the top of the cement ring will enter the liquid medium to generate hydraulic pressure, and the sensor will record the pressure value and transmit it to the pressure control system, and finally transmit it to the computer control system to generate the cement ring top annulus pressure curve.
[0055] Example 2
[0056] As another preferred embodiment of the present invention, refer to the attached specification Figure 1 As shown, this embodiment discloses an experimental method for testing the expansion of cracks at the cement sheath interface of a well cementing device, the method comprising the following steps:
[0057] S1. Before the experiment begins, the actual cement sheath under the fracturing condition needs to be equivalent to the experimental cement sheath through three processes: geometric similarity, stress equality, and same process, and the size, stress, and simulated fracturing condition load on the experimental cement sheath need to be calculated;
[0058] S2. According to the experimental requirements and GB / T10238 standard, the corresponding cement slurry is prepared and injected into the cement ring curing mold. The cone ring sleeve on the base of the curing mold can preform the first interface and / or second interface cracks of the cement ring at the bottom of the cement ring. The curing mold is placed in a high-temperature and high-pressure curing kettle for curing to a set age. The internal pressure casing 4, the simulated surrounding rock casing 6 and the cement ring in the curing mold are taken out together to form an "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" combination.
[0059] S3, placing the assembly obtained in step S2 in a sealed pressure-bearing sleeve 3, forming a confining pressure annulus 37 between the outer wall of the simulated surrounding rock casing 6 of the assembly and the inner wall of the pressure-bearing sleeve 3; a certain space is provided between the prefabricated cement ring with one interface and / or two interface cracks and the upper and lower ends of the assembly, and a cement ring bottom annulus 38 and a cement ring top annulus 39 are formed between the top cover 1 and the base 2 of the pressure-bearing sleeve 3 respectively; a casing inner cavity 40 is formed between the internal pressure casing 4 of the assembly and the top cover 1 and the base 2 of the pressure-bearing sleeve 3;
[0060] S4, an external heater 15 is arranged in the confining pressure annulus 37, an internal heater 13 is arranged in the casing inner cavity 40, and the external heater 15 and the internal heater 13 are connected to the temperature control system 17; the confining pressure annulus 37, the cement ring bottom annulus 38, the cement ring top annulus 39 and the casing inner cavity 40 are connected to the pressure control system 30; the coupling drive 10 is assembled in the casing inner cavity 40, and the acoustic wave transmitter 7, the 3H acoustic wave receiver 8 and the 5H acoustic wave receiver 9 are assembled at the lower end of the coupling drive 10 in sequence; wherein the acoustic wave transmitter 7 and the 3H acoustic wave receiver 8 are 3Hcm apart, and the acoustic wave transmitter 7 and the 5H acoustic wave receiver 9 are 5Hcm apart; the coupling drive 10 is assembled in the casing inner cavity 40 and kept vertically centered; the acoustic wave generator, the 3H acoustic wave receiver 8 and the 5H acoustic wave receiver 9 are connected to the acoustic wave signal processing system 12; the temperature control system 17, the pressure control system 30 and the acoustic wave signal processing system 12 are data connected to the computer control system 31;
[0061] S5, the computer control system 31 controls the pressure control system 30 to simultaneously inject liquid medium into the confining pressure annulus 37, the cement ring bottom annulus 38 and the casing lumen 40 according to the fracturing load data calculated in step S1, and exhaust the air therein; when the casing lumen 40 and the confining pressure annulus 37 are filled with liquid medium, the drain valves of the casing lumen 40 and the confining pressure annulus 37 are closed;
[0062] The computer control system 31 controls the temperature control system 17, sets the heating time, and uses the inner heater 13 and the outer heater 15 to uniformly heat the cement sheath assembly. As the temperature increases, the pressure of the casing cavity 40, the pressure of the cement sheath bottom annulus 38, and the pressure of the confining pressure annulus 37 will all increase; at the same time, the computer control system 31 sets the pressure increase time in the pressure control system 30 to be consistent with the heating time, and uniformly and continuously pressurizes the casing cavity 40, the cement sheath bottom annulus 38, and the confining pressure annulus 37. After the heating and pressure increase are completed, the temperature is controlled at the target temperature, and the pressure of the confining pressure annulus 37 is controlled at the target confining pressure, and they are maintained;
[0063] After the pressure of the confining pressure annulus 37 is stabilized, the pressure injection of the confining pressure annulus 37 is closed; the casing inner cavity 40 and the annulus 38 at the bottom of the cement ring are continuously and uniformly pressurized until the pressure of the casing inner cavity 40 and the annulus 38 at the bottom of the cement ring rise to the target inner pressure, and then the pressure of the casing inner cavity 40, the pressure of the confining pressure annulus 37 and the pressure of the annulus 38 at the bottom of the cement ring are kept stable for a period of time;
[0064] S6, the computer control system 31 controls the acoustic signal processing system 12 to start, and uses the acoustic transmitter 7 to transmit the acoustic pulse, which is received by the 3H acoustic receiver 8 and the 5H acoustic receiver 9 after passing through the internal pressure casing 4, the cement sheath and the simulated surrounding rock casing 6. The 3H acoustic receiver 8 and the 5H acoustic receiver 9 send the full-wave waveform data they obtain to the full-wave waveform data collector of the acoustic signal processing system 12, and then the full-wave waveform data collector transmits the recorded data to the digital oscilloscope, which is sent to the instantaneous waveform collector after processing, and then the waveform data is converted into the cement sheath interface bonding strength signal through the instantaneous waveform converter to determine whether cracks are generated here;
[0065] S7, the computer control system 31 controls the coupling drive 10 to move, driving the acoustic wave transmitter 7, the 3H acoustic wave receiver 8 and the 5H acoustic wave receiver 9 to move at a uniform speed along the axial direction of the internal pressure casing 4, measuring multiple sections of continuous crack signals that change with time, and finally transmitting them to the computer control system 31 to generate a cement sheath first interface and / or second interface crack extension length curve.
[0066] Example 3
[0067] As another preferred embodiment of the present invention, refer to the attached specification Figure 2-7As shown, this embodiment is an explanation of the implementation method of the curing mold in Example 1 and Example 2.
[0068] The maintenance mold includes an internal pressure sleeve 4, a simulated surrounding rock sleeve 6, a mold top cover 32 and a mold base 33. The internal pressure sleeve is placed in the simulated surrounding rock sleeve 6, and the upper and lower ends of the internal pressure sleeve are respectively connected to the slots of the mold top cover 32 and the mold base 33; the mold top cover 32 and the mold base 33 are respectively fixedly connected to the upper and lower ends of the simulated surrounding rock sleeve 6 by fasteners; a cone ring sleeve for prefabricating cement sheath interface cracks is provided on the slot of the base 2, and the cone ring sleeve is any one of three types of cone ring sleeves; the three types of cone ring sleeves are cone ring sleeve I 34 for prefabricating cement sheath one interface crack, cone ring sleeve II 35 for prefabricating cement sheath two interface cracks and cone ring sleeve III 36 for prefabricating both cement sheath one interface crack and two interface cracks.
[0069] As an implementation method of this embodiment, Figure 2 As shown, it is a combined body maintenance mold structure containing cement ring one and two interface cracks under vertical well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33, and the contact surface between the clamping cone ring sleeve III 36 and the cement ring is coated with smooth and uniform temperature-resistant degreasing oil, and the clamping cone ring sleeve III 36 of corresponding size is tightly fitted with the cement ring one and two interfaces; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve, and then bolted. The mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve III 36 are disassembled, and at this time, the "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length at the cement ring one-two interface is obtained.
[0070] As another implementation method of this embodiment, Figure 3As shown, it is a combined body curing mold structure containing cement sheath-interface cracks under vertical well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33, and the contact surface between the clamping cone ring sleeve Ⅰ34 and the cement sheath is coated with smooth and uniform temperature-resistant degreasing oil, and the clamping cone ring sleeve Ⅰ34 of corresponding size is closely fitted with the cement sheath-interface; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve, and then the internal pressure casing 4 and the simulated surrounding rock casing 6 are fixed by bolts. The mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve I 34 are disassembled, and at this time, an "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length at the cement ring interface is obtained.
[0071] As another implementation method of this embodiment, Figure 4 As shown, it is a combined body curing mold structure containing cement ring II interface cracks under vertical well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33, and the contact surface of the clamping cone ring sleeve II 35 and the cement ring is coated with smooth and uniform temperature-resistant degreasing oil, and the clamping cone ring sleeve II 35 of corresponding size is closely fitted with the cement ring II interface; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve, and then bolted The mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve II 35 are disassembled, and at this time, the "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length at the cement ring interface is obtained.
[0072] As another implementation method of this embodiment, Figure 5As shown, it is a combined body maintenance mold structure containing cement ring one and two interface cracks under eccentric well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33. The internal pressure casing 4 and the simulated surrounding rock casing 6 are eccentrically arranged. The contact surface between the clamping cone ring sleeve III 36 and the cement ring is coated with smooth and uniform heat-resistant degreasing oil. At the same time, the clamping cone ring sleeve III 36 of corresponding size is closely fitted with the cement ring one and two interfaces; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve. In the meantime, the mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together by bolts, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve III 36 are disassembled, and at this time, the "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length at the first and second interfaces of the cement rings is obtained.
[0073] As another implementation method of this embodiment, Figure 6 As shown, it is a combined body curing mold structure containing cement sheath-interface cracks under eccentric well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33. The internal pressure casing 4 and the simulated surrounding rock casing 6 are eccentrically arranged. The contact surface between the clamping cone ring sleeve Ⅰ34 and the cement sheath is coated with smooth and uniform heat-resistant degreasing oil. At the same time, the clamping cone ring sleeve Ⅰ34 of corresponding size is tightly fitted with the cement sheath-interface; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve. Then, the mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together by bolts, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve I 34 are disassembled, and at this time, a cement ring-interface "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length is obtained.
[0074] As another implementation method of this embodiment, Figure 7As shown, it is a combined body curing mold structure containing cement ring interface cracks under eccentric well section conditions. Specifically, the internal pressure casing 4 and the simulated surrounding rock casing 6 are installed on the groove of the mold base 33. The internal pressure casing 4 and the simulated surrounding rock casing 6 are eccentrically arranged. The contact surface between the clamping cone ring sleeve II 35 and the cement ring is coated with smooth and uniform heat-resistant degreasing oil. At the same time, the clamping cone ring sleeve II 35 of corresponding size is tightly fitted with the cement ring interface II; the corresponding cement slurry is prepared according to GB / T10238 and poured into the annular space between the internal pressure casing 4 and the mold sleeve. Then, the mold top cover 32 and the simulated surrounding rock casing 6 are tightly connected together by bolts, and then the entire assembled mold is placed in a high-temperature and high-pressure curing kettle, the target temperature and curing age are set, and curing begins; after the curing is completed, the curing kettle heating program is turned off, and when the temperature drops to room temperature, the entire assembled mold is taken out, the bolts are loosened, the mold top cover 32 and the mold base 33 and the cone ring sleeve II 35 are disassembled, and at this time, the "internal pressure casing 4-cement ring-simulated surrounding rock casing 6" assembly with an initial seam length at the cement ring II interface is obtained.
[0075] Example 4
[0076] As another preferred embodiment of the present invention, this embodiment is a supplementary implementation of Embodiment 2. Specifically, while the computer control system starts the acoustic signal processing system, it uses the pressure control system to monitor the pressure of the annulus at the top of the cement ring; once the cement ring fails to flow through, the liquid medium will enter the annulus at the top of the cement ring to generate hydraulic pressure, and the sensor will record the pressure value and transmit it to the pressure control system, and finally transmit it to the computer control system to generate a cement ring top annulus pressure curve, so as to determine whether the cement ring interface has failed to flow through.
[0077] Example 5
[0078] As another preferred embodiment of the present invention, this embodiment is a supplementary implementation of Embodiment 2. Specifically, after the test is completed, the computer control system saves the experimental data, turns off the acoustic signal processing system and the temperature control system, and waits until the temperature in the pressure sleeve drops to room temperature. The pressure in the casing cavity, the annulus at the bottom of the cement ring and the confining pressure annulus are removed by using the pressure control system. Then, the pressure control system is turned off, the corresponding joints and pipelines of each control system are removed, the top cover of the pressure sleeve is closed, the cement ring assembly is taken out, and the experiment is completed.
[0079] Example 6
[0080] As another preferred embodiment of the present invention, refer to the attached specification Figure 8 , 9 As shown in Figure 10, the implementation process of the cement sheath interface crack test with initial crack lengths of l1, l2, and l3 is as follows:
[0081] S1. Before the experiment begins, the actual cement sheath under the fracturing condition needs to be equivalent to the experimental cement sheath through three processes: geometric similarity, stress equality, and the same process, and the size, stress, and simulated fracturing load of the experimental cement sheath are calculated; the specific experimental cement sheath internal pressure is 90MPa, and the confining pressure is 50MPa;
[0082] S2. Prepare corresponding cement slurry according to the experimental requirements and GB / T10238 standard, and inject it into the cement ring curing mold. The cone ring sleeve on the base of the curing mold can preform the first interface and / or second interface cracks of the cement ring at the bottom of the cement ring. Place the curing mold in a high-temperature and high-pressure curing kettle for curing for 7 days, and take out the internal pressure casing, simulated surrounding rock casing and cement ring in the curing mold together to form an "internal pressure casing-cement ring-simulated surrounding rock casing" combination (such as Figure 2 shown);
[0083] Referring to the above steps S1 and S2, three "internal pressure casing-cement sheath-simulated surrounding rock casing" assemblies are formed, and the initial seam lengths of the first and second interfaces of the cement sheath in the three assemblies are l1, l2 and l3 respectively;
[0084] S3, placing the three assemblies obtained in step S2 in a sealed pressure-bearing sleeve respectively, forming a confining pressure annulus between the outer wall of the simulated surrounding rock casing of the assembly and the inner wall of the pressure-bearing sleeve; a certain space is provided between the prefabricated cement ring with one interface and / or two interface cracks and the upper and lower ends of the assembly, and a cement ring bottom annulus and a cement ring top annulus are formed between the top cover and the base of the pressure-bearing sleeve respectively; a casing inner cavity is formed between the internal pressure casing of the assembly and the top cover and the base of the pressure-bearing sleeve;
[0085] S4, an external heater is arranged in the confining pressure annulus, an internal heater is arranged in the inner cavity of the casing, and the external heater and the internal heater are connected to the temperature control system; the confining pressure annulus, the annulus at the bottom of the cement ring, the annulus at the top of the cement ring and the inner cavity of the casing are connected to the pressure control system; a coupling drive is assembled in the inner cavity of the casing, and a sound wave transmitter, a 3H sound wave receiver and a 5H sound wave receiver are assembled at the lower end of the coupling drive in sequence; wherein the sound wave transmitter and the 3H sound wave receiver are 3Hcm apart, and the sound wave transmitter and the 5H sound wave receiver are 5Hcm apart; the coupling drive is assembled in the inner cavity of the casing and kept vertically centered; the sound wave generator, the 3H sound wave receiver and the 5H sound wave receiver are connected to the sound wave signal processing system; the temperature control system, the pressure control system and the sound wave signal processing system are data connected to the computer control system;
[0086] S5. The computer control system controls the pressure control system to simultaneously inject liquid medium into the confining pressure annulus, the annulus at the bottom of the cement ring and the inner cavity of the casing according to the fracturing load data calculated in step S1 to exhaust the air therein; when the inner cavity of the casing and the confining pressure annulus are filled with the liquid medium, the drain valves of the inner cavity of the casing and the confining pressure annulus are closed;
[0087] The computer control system controls the temperature control system, sets the heating time to 60 minutes, and uses the internal heater and the external heater to uniformly heat the cement sheath assembly. As the temperature increases, the casing cavity pressure, the cement sheath bottom annulus pressure, and the confining pressure annulus pressure will all increase; at the same time, the computer control system sets the pressure increase time to be consistent with the heating time in the pressure control system, and uniformly and continuously pressurizes the casing cavity, the cement sheath bottom annulus, and the confining pressure annulus. After the heating and pressure increase, the temperature is controlled at the target temperature of 120°C, and the confining pressure annulus pressure is controlled at the target confining pressure of 50MPa, and they are maintained;
[0088] After the confining annulus pressure is stable, close the pressure injection of the confining annulus; continue to uniformly and continuously pressurize the casing cavity and the annulus at the bottom of the cement ring until the casing cavity pressure and the annulus pressure at the bottom of the cement ring rise to the target internal pressure of 90MPa, and then keep the casing cavity pressure, confining annulus pressure and the annulus pressure at the bottom of the cement ring stable for a period of time;
[0089] The computer control system starts the acoustic signal processing system, and uses the acoustic transmitter to transmit acoustic pulses, which are received by the 3H acoustic receiver and the 5H acoustic receiver after passing through the internal pressure casing, cement sheath and simulated surrounding rock casing. The 3H acoustic receiver and the 5H acoustic receiver send the acquired full-wave waveform data to the full-wave waveform data collector of the acoustic signal processing system, and then the full-wave waveform data collector transmits the recorded data to the digital oscilloscope, which is processed by the digital oscilloscope and sent to the instantaneous waveform collector. After that, the waveform data is converted into the cement sheath interface bonding strength signal through the instantaneous waveform converter to determine whether cracks are generated here.
[0090] S7, the computer control system controls the coupling drive action, drives the acoustic wave transmitter, 3H acoustic wave receiver and 5H acoustic wave receiver to move at a uniform speed along the axial direction of the internal pressure casing, measures multiple sections of continuous crack signals that change with time, and finally transmits them to the computer control system to generate a cement sheath first interface and / or second interface crack extension length curve;
[0091] S8. While the computer control system starts the acoustic signal processing system, it uses the pressure control system to monitor the annular pressure at the top of the cement ring. Once the cement ring fails, the liquid medium will enter the annular space at the top of the cement ring to generate hydraulic pressure. The sensor will record the pressure value and transmit it to the pressure control system. Finally, it will be sent to the computer control system to generate a cement ring pressure curve at the top of the cement ring, so as to determine whether the cement ring interface has failed.
[0092] The experimental results are shown in Table 1 below:
[0093]
[0094] Table 1 shows the effect of initial crack length on the extension length of cement sheath interface crack
[0095] The above three combinations use the same cement slurry formula, and the experimental formula is: 100% G-grade high-resistance cement + 35% quartz sand + 1.5% anti-channeling agent + 3.5% fluid loss reducer + 0.2% dispersant + 0.2% retarder + 44% water.
[0096] Experimental results analysis:
[0097] 1) One: Test chart based on experimental results ( Figure 8 ) It can be seen that the crack extension length of the second interface of the cement sheath is greater than that of the first interface, and the two interfaces have not failed through. This shows that the cement sheath under this system can resist the failure of interface cracks through failure when the initial crack length is l1.
[0098] 2) Two: Test chart based on experimental results ( Fig. 9 ) It can be seen that when the initial crack length of the cement sheath is l2 (l2>l1), the crack extension lengths of the first and second interfaces of the cement sheath increase, and the crack extension length of the second interface of the cement sheath is greater than that of the first interface, and the two interfaces still do not fail through. This shows that the cement sheath under this system can still resist the failure of interface cracks through when the initial crack length is l2, but the degree of damage to the cement sheath increases.
[0099] 3) Three: Test chart based on experimental results ( Fig.10 ) It can be seen that when the initial crack length of the cement sheath is l3 (l3>l2), the crack extension length of the second interface of the cement sheath is less than the crack extension length of the first interface, and the first interface of the cement sheath fails through. This means that when the initial crack length is greater than a certain critical value, the cement sheath interface will fail through through. From the test curve, it can be seen that the crack of the second interface of the cement sheath has tortuously expanded, thereby increasing the crack extension of the first interface until interface failure occurs.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit it;
[0101] The present invention has been described in detail with reference to the aforementioned embodiments. Those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An experimental method for testing the expansion of cracks at the cement sheath interface, characterized in that: The experimental method includes the following steps: S1. Before the experiment begins, the actual cement sheath under the fracturing condition needs to be equivalent to the experimental cement sheath (5) through three processes: geometric similarity, stress equality, and process equality, and the size, stress, and simulated fracturing condition load of the experimental cement sheath (5) are calculated; S2. Prepare corresponding cement slurry according to GB / T10238 standard and inject it into the cement ring (5) curing mold. The cone ring sleeve on the base of the curing mold can preform the first interface and / or second interface cracks of the cement ring at the bottom of the cement ring (5). Place the curing mold in a high-temperature and high-pressure curing kettle and cure it to a set age. Take out the internal pressure casing (4), the simulated surrounding rock casing (6) and the cement ring (5) in the curing mold together to form an "internal pressure casing-cement ring-simulated surrounding rock casing" combination. S3, placing the assembly obtained in step S2 in a sealed pressure-bearing sleeve (3), forming a confining pressure annulus (37) between the outer wall of the simulated surrounding rock casing (6) of the assembly and the inner wall of the pressure-bearing sleeve (3); a certain space is provided between the prefabricated cement ring (5) with a single interface and / or a double interface crack and the upper and lower ends of the assembly, and a cement ring bottom annulus (38) and a cement ring top annulus (39) are formed between the top cover (1) and the base (2) of the pressure-bearing sleeve (3); and a casing inner cavity (40) is formed between the internal pressure casing (4) of the assembly and the top cover (1) and the base (2) of the pressure-bearing sleeve (3); S4. An external heater (15) is provided in the confining pressure annulus (37), an internal heater (13) is provided in the inner cavity (40) of the casing, and the external heater (15) and the internal heater (13) are connected to the temperature control system (17); the confining pressure annulus (37), the annulus at the bottom of the cement ring (38), the annulus at the top of the cement ring (39) and the inner cavity (40) of the casing are connected to the pressure control system (30); a coupling drive (10) is installed in the inner cavity (40) of the casing, and an acoustic wave transmitter (7), a 3H acoustic wave receiver (8) and a 5H acoustic wave receiver are installed at the lower end of the coupling drive (10) in sequence. receiver (9); wherein a 3H acoustic wave receiver represents an acoustic wave receiver at a distance of 3 units from the acoustic wave transmitter, and a 5H acoustic wave receiver represents an acoustic wave receiver at a distance of 5 units from the acoustic wave transmitter; the coupling drive (10) is assembled in the inner cavity (40) of the casing and kept vertically centered; the acoustic wave generator, the 3H acoustic wave receiver (8) and the 5H acoustic wave receiver (9) are connected to the acoustic wave signal processing system (12); the temperature control system (17), the pressure control system (30) and the acoustic wave signal processing system (12) are data connected to the computer control system (31); S5, the computer control system (31) controls the pressure control system (30) to simultaneously inject liquid medium into the confining pressure annulus (37), the cement ring bottom annulus (38) and the casing lumen (40) based on the simulated fracturing load data calculated in step S1, and to exhaust the air in the confining pressure annulus (37), the cement ring bottom annulus (38) and the casing lumen (40); when the casing lumen (40) and the confining pressure annulus (37) are filled with liquid medium, the drain valves of the casing lumen (40) and the confining pressure annulus (37) are closed; The computer control system (31) controls the temperature control system (17), sets the heating time, and uses the inner heater (13) and the outer heater (15) to uniformly heat the cement sheath (5) assembly. As the temperature increases, the pressure of the casing lumen (40), the pressure of the cement sheath bottom annulus (38), and the pressure of the confining pressure annulus (37) all increase. At the same time, the computer control system (31) sets the pressure increase time in the pressure control system (30) to be consistent with the heating time, and uniformly and continuously pressurizes the casing lumen (40), the cement sheath bottom annulus (38), and the confining pressure annulus (37). After the heating and pressure increase are completed, the temperature is controlled to be at a target temperature, and the pressure of the confining pressure annulus (37) is controlled to be at a target confining pressure, and the pressure is maintained; After the pressure of the confining pressure annulus (37) is stabilized, the pressure injection of the confining pressure annulus (37) is closed; the casing inner cavity (40) and the cement ring bottom annulus (38) are continuously and uniformly pressurized until the pressure of the casing inner cavity (40) and the cement ring bottom annulus (38) rise to the target inner pressure, and then the casing inner cavity (40), the confining pressure annulus (37) and the cement ring bottom annulus (38) are kept stable for a period of time; S6, the computer control system (31) controls the acoustic signal processing system (12) to start, and uses the acoustic transmitter (7) to transmit acoustic pulses, which are received by the 3H acoustic receiver (8) and the 5H acoustic receiver (9) after passing through the internal pressure casing (4), the cement sheath (5) and the simulated surrounding rock casing (6). The 3H acoustic receiver (8) and the 5H acoustic receiver (9) send the acquired full-wave waveform data to the full-wave waveform data collector of the acoustic signal processing system (12), and then the full-wave waveform data collector transmits the recorded data to the digital oscilloscope, which processes the data and sends it to the instantaneous waveform collector, and then the waveform data is converted into the cement sheath (5) interface bonding strength signal through the instantaneous waveform converter to determine whether cracks are generated here; S7, the computer control system (31) controls the coupling drive (10) to move, driving the acoustic wave transmitter (7), the 3H acoustic wave receiver (8) and the 5H acoustic wave receiver (9) to move at a uniform speed along the axial direction of the internal pressure casing (4), measuring multiple sections of continuous crack signals that change with time, and finally transmitting them to the computer control system (31) to generate a first interface and / or second interface crack extension length curve of the cement sheath (5); The computer control system (31) starts the acoustic signal processing system (12) and uses the pressure control system (30) to monitor the pressure of the annulus (39) at the top of the cement sheath; once the cement sheath (5) fails to flow through, the liquid medium will enter the annulus (39) at the top of the cement sheath to generate hydraulic pressure, and the sensor will record the pressure value and transmit it to the pressure control system (30), and finally transmit it to the computer control system (31) to generate a pressure curve of the annulus (39) at the top of the cement sheath, so as to judge whether the cement sheath (5) interface has failed to flow through.
2. An experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 1, characterized in that: After the test is completed, the computer control system (31) saves the experimental data, closes the acoustic signal processing system (12) and the temperature control system (17), and waits until the temperature in the pressure sleeve (3) drops to room temperature. The pressure in the casing cavity (40), the annulus at the bottom of the cement ring (38) and the confining pressure annulus (37) are removed by using the pressure control system (30). The pressure control system (30) is then closed, the corresponding joints and pipelines of each control system are removed, the top cover (1) of the pressure sleeve (3) is removed, and the cement ring (5) assembly is taken out, and the experiment is completed.
3. The experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 1, characterized in that: The maintenance mold comprises an internal pressure sleeve (4), a simulated surrounding rock sleeve (6), a mold top cover (32) and a mold base (33); the internal pressure sleeve is placed in the simulated surrounding rock sleeve (6), and the upper end and lower end of the internal pressure sleeve are respectively connected to the clamping grooves of the mold top cover (32) and the mold base (33); the mold top cover (32) and the mold base (33) are respectively fixedly connected to the upper end and the lower end of the simulated surrounding rock sleeve (6) by fasteners; a clamping cone ring sleeve for prefabricating interface cracks of a cement ring (5) is provided on the clamping groove of the base (2), and the clamping cone ring sleeve is any one of three types of clamping cone ring sleeves; the three types of clamping cone ring sleeves are respectively a clamping cone ring sleeve I (34) for prefabricating one interface crack of the cement ring (5), a clamping cone ring sleeve II (35) for prefabricating two interface cracks of the cement ring (5), and a clamping cone ring sleeve III (36) for prefabricating both one interface crack and two interface cracks of the cement ring (5).
4. An experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 3, characterized in that: The contact surface of the cone ring sleeve that contacts the cement ring (5) is coated with heat-resistant degreasing oil.
5. The experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 3, characterized in that: The internal pressure casing (4) is coaxially arranged with the simulated surrounding rock casing (6) and is used to produce a circular cement ring (5).
6. An experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 3, characterized in that: The internal pressure casing (4) and the simulated surrounding rock casing (6) are eccentrically arranged and are used to produce an eccentric cement ring (5).
7. An experimental method for testing the propagation of cracks at the cement sheath interface of a well cementing device according to claim 1, 2, 4, 5 or 6, characterized in that: The temperature control system (17) is provided with three connection ports, which are respectively connected to an inner coupling temperature sensor (14), an outer coupling temperature sensor (16) and a computer control system (31); the inner heater (13) is located in the inner cavity (40) of the casing and is mounted on the base (2) of the pressure-bearing sleeve (3); and the outer heater (15) is located in the confining pressure annulus (37) and is mounted on the base (2) of the pressure-bearing sleeve (3); The temperature control system (17) controls the heating power of the inner heater (13) through the inner coupling temperature sensor (14), and controls the heating power of the outer heater (15) through the outer coupling temperature sensor (16). The inner heater (13) and the outer heater (15) are heated simultaneously to ensure that the cement ring (5) is evenly heated.
8. An experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 1, 2, 4, 5 or 6, characterized in that: The pressure control system (30) is provided with eight connection ports, which are respectively connected to an internal pressure sensor (19), an internal pressure joint (20), an annular pressure sensor (23) at the bottom of the cement ring, an annular pressure joint (24) at the bottom of the cement ring, an annular pressure sensor (25) at the top of the cement ring, a confining pressure annular pressure sensor (27), a confining pressure annular joint (28) and a computer control system (31); wherein the internal pressure sensor (19) is located on the hydraulic pipeline between the internal pressure control valve (18) and the internal pressure joint (20), and the internal pressure joint (20) is used to A liquid medium is injected into the inner cavity (40) of the casing; a cement ring bottom annulus pressure sensor (23) is located on a hydraulic pipeline between a cement ring bottom annulus pressure control valve (22) and a cement ring bottom annulus joint (24); and the cement ring bottom annulus joint (24) is used to inject the liquid medium into the cement ring bottom annulus (38); and a confining pressure annulus pressure sensor (27) is located on a hydraulic pipeline between a confining pressure annulus pressure control valve (26) and a confining pressure annulus joint (28); and the confining pressure annulus joint (28) is used to inject the liquid medium into the confining pressure annulus (37).
9. An experimental method for testing the expansion of cement sheath interface cracks as claimed in claim 8, characterized in that: An internal pressure drain valve (21) is provided at the top cover (1) above the inner cavity (40) of the casing, and a confining pressure annulus drain valve (29) is provided at the top cover (1) above the confining pressure annulus (37).
Citation Information
Patent Citations
Device and method for testing packing performance of annulus cement sheath of oil and wellbore
CN111307690A
Cement sheath structural integrity mechanics experiment device
CN103498662A
Oil-gas well cement sheath seal characteristic simulation test device and test method
CN104153760A