LCD display protection board
By using a laminated resin board in the liquid crystal display protection board to adjust its optical characteristics and cure the coating, the problem of de-identification in the prior art is solved, and more uniform optical performance and higher heat resistance are achieved.
Patent Information
- Application Number
- CN202080085280.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-11
- Filing Date
- 2020-12-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-12-09
AI Technical Summary
The existing liquid crystal display protection plate is prone to rainbow patterns, black screens and coloring when viewed through the polarization filter, resulting in a reduced visual recognition and making it difficult to obtain an optically uniform protective plate.
The resin plates in the phase difference adjustment layer and the base layer are laminated. By adjusting the photoelastic coefficient and orientation birefringence characteristics, the in-plane retardation value (Re value) of the resin plate is controlled to be in the range of 50 to 330 nm, and the resin plate is placed on the resin plate. The surface forms a cured coating to optimize optical properties.
It effectively suppresses rainbow patterns, black screens and coloring phenomena when observed through polarization filters, improves the visual recognition of the liquid crystal display, and maintains the heat resistance and adhesion of the protective plate in a humid and hot environment.
Smart Images

Figure CN114787698B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a protective plate for a liquid crystal display. Background Art
[0002] In a liquid crystal display or a touch panel display in which a liquid crystal display and a touch panel are combined, a protective plate is sometimes provided on the front side thereof to prevent scratches on the surface, etc. In this specification, this protective plate is referred to as a "liquid crystal display protective plate".
[0003] The liquid crystal display protection plate includes a resin plate composed of at least one thermoplastic resin layer and a cured coating film formed on at least one surface of the resin plate as needed.
[0004] For example, Patent Document 1 discloses a scratch-resistant resin plate suitable for a display window protection plate of a portable information terminal, comprising a methacrylic resin plate and a cured coating formed on at least one surface thereof (claims 1, 2, 7, paragraph 0010, etc.). Patent Document 2 discloses a polycarbonate resin laminate for a liquid crystal display cover, comprising a laminate having a methacrylic resin layer laminated on one surface of a polycarbonate resin layer and a cured coating formed on the methacrylic resin layer of the laminate (claim 1, paragraph 0008, etc.).
[0005] The LCD protection plate is provided on the front side of the LCD (viewer side), and the viewer views the LCD screen through the protection plate. Here, the LCD protection plate hardly changes the polarization of the light emitted from the LCD, so when the screen is viewed through a polarizing filter such as polarized sunglasses, the screen may become darker and the image visibility may decrease (black screen phenomenon) depending on the angle between the polarization axis of the emitted light and the transmission axis of the polarizing filter.
[0006] Therefore, a liquid crystal display protection plate capable of suppressing the reduction of image visibility when viewing the screen of a liquid crystal display through a polarizing filter has been studied. For example, Patent Document 3 discloses a liquid crystal display protection plate having an in-plane retardation value (also referred to as "Re value") of 85 to 300 nm, which is composed of a scratch-resistant resin plate having a cured coating formed on at least one surface of the resin plate (claim 1).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2004-299199
[0010] Patent Document 2: Japanese Patent Application Publication No. 2006-103169
[0011] Patent Document 3: Japanese Patent Application Publication No. 2010-085978 Summary of the invention
[0012] Problems to be solved by the invention
[0013] In Patent Document 3, the resin plate is preferably a laminated plate in which a methacrylic resin layer is laminated on at least one surface of a polycarbonate resin layer (claim 6). In this laminated plate, for example, by adjusting the molding conditions according to the thickness of the resin plate, the birefringence of the polycarbonate resin layer can be adjusted, and the Re value of the liquid crystal display protective plate can be adjusted to a suitable range (paragraph 0036, etc.).
[0014] The relationship between stress and birefringence and the relationship between orientation birefringence, stress birefringence and photoelastic coefficient are shown in the figure. Figure 6 .
[0015] The absolute value of the photoelastic coefficient of the polycarbonate resin used in Patent Document 3 is 90×10 -12 / Pa, which is very large, and the Re value will change due to slight stress. Therefore, when using polycarbonate resin, it is difficult to obtain an optically uniform LCD protection plate. For example, when observing the LCD protection plate on the LCD screen through a polarizing filter, rainbow patterns may be observed due to fluctuations in the Re value.
[0016] On the other hand, the absolute value of the photoelastic coefficient of the methacrylic resin used in Patent Document 1 is as low as 3.2×10 -12 / Pa, Re value is not easily changed by stress. Therefore, when using methacrylic resin, an optically uniform LCD protective plate can be obtained. However, the absolute value of the orientation birefringence of methacrylic resin is as low as 4.0×10 -4 Therefore, although it depends on the thickness, the Re value of the obtained LCD protective plate is about 20nm and tends to decrease. Therefore, when the LCD protective plate located on the LCD screen is observed through a polarizing filter, the screen may become black depending on the angle between the polarization axis of the outgoing light and the transmission axis of the polarizing filter, and the visibility of the image may be reduced.
[0017] In general, when the Re value of the liquid crystal display protective plate is larger than the appropriate range, the difference in transmittance of each wavelength in the visible light region becomes larger when viewed through a polarizing filter, and various colors may be seen, resulting in reduced visibility (coloration phenomenon).
[0018] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a liquid crystal display protection plate capable of suppressing a reduction in visibility such as rainbow, black screen, and coloration when the liquid crystal display protection plate located on a liquid crystal screen is observed through a polarizing filter.
[0019] Methods used to solve problems
[0020] The present invention provides the following liquid crystal display protection plates [1] to [7].
[0021] [1] A liquid crystal display protective plate comprising a resin plate having a base material layer laminated on both sides of a phase difference adjustment layer,
[0022] The above-mentioned phase difference adjustment layer has a photoelastic coefficient (C A ) has an absolute value of 10.0×10 -12 / Pa or less and the orientation birefringence (Δn A ) has an absolute value of 10.0×10 -4 ~100.0×10 -4 The transparent thermoplastic resin (A), the oriented birefringence (Δn A ) is obtained by uniaxially stretching a test piece having a width of 20 mm, a length of 40 mm, and a thickness of 1 mm at a temperature 10° C. higher than the glass transition temperature at a rate of 3 mm / min at a stretching ratio of 100% and measuring the in-plane retardation value of the central portion of the test piece,
[0023] The substrate layer has a photoelastic coefficient (C B ) has an absolute value of 10.0×10 -12 / Pa or less and the orientation birefringence (Δn B ) is less than 10.0×10 -4 The transparent thermoplastic resin (B), the oriented birefringence (Δn B ) is obtained by uniaxially stretching a test piece having a width of 20 mm, a length of 40 mm, and a thickness of 1 mm at a temperature 10° C. higher than the glass transition temperature at a rate of 3 mm / min at a stretching ratio of 100% and measuring the in-plane retardation value of the central portion of the test piece,
[0024] The glass transition temperature of the phase difference adjustment layer is Tg A , and the glass transition temperature of the substrate layer is set to Tg B When Tg A <Tg B ,
[0025] The resin plate has an in-plane retardation value of 50 to 330 nm.
[0026] [2] The liquid crystal display protection plate according to [1], wherein the standard deviation of the in-plane retardation value within the range of a width of 17 cm and a length of 22 cm of the resin plate is 15.0 nm or less.
[0027] [3] The liquid crystal display protection plate according to [1] or [2], wherein the glass transition temperature (Tg B ) is above 115°C.
[0028] [4] The liquid crystal display protection plate according to any one of [1] to [3], wherein the thickness of the phase difference adjustment layer is set to T A , and the total thickness of the above-mentioned substrate layer is set as T B When T A <T B .
[0029] [5] The liquid crystal display protective plate according to any one of [1] to [4], wherein the transparent thermoplastic resin (A) contains an aromatic vinyl monomer unit,
[0030] The content of the aromatic vinyl monomer unit in the transparent thermoplastic resin (A) is V [mass %], and the thickness of the phase difference adjustment layer is T A [mm], the following formula (1) is satisfied.
[0031] 6.0≤V×T A ≤30.0…(1)
[0032] [6] The liquid crystal display protection plate according to any one of [1] to [5], further comprising a cured film on at least one surface of the resin plate.
[0033] [7] The liquid crystal display protection plate according to any one of [1] to [6], wherein the resin plate is an extrusion-molded plate.
[0034] Effects of the Invention
[0035] According to the present invention, it is possible to provide a liquid crystal display protection plate capable of suppressing a decrease in visibility such as rainbow, black screen, and coloration when the liquid crystal display protection plate located on a liquid crystal screen is observed through a polarizing filter. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic cross-sectional view of a liquid crystal display protection plate according to a first embodiment of the present invention.
[0037] Figure 2 It is a schematic cross-sectional view of a liquid crystal display protection plate according to a second embodiment of the present invention.
[0038] Figure 3 It is a schematic diagram of the manufacturing apparatus of the extrusion molded plate which is one embodiment of this invention.
[0039] Figure 4 It is a schematic cross-sectional view of a liquid crystal display protection plate used as a comparative example.
[0040] Figure 5 It is a schematic cross-sectional view of a liquid crystal display protection plate used as a comparative example.
[0041] Figure 6 It is a graphic diagram showing the relationship between stress and birefringence and the relationship between orientation birefringence, stress birefringence and photoelastic coefficient. DETAILED DESCRIPTION
[0042] Generally, for a thin film formed body, the terms "film", "sheet" or "plate" are used depending on the thickness, but there is no clear distinction between them. The "resin plate" described in this specification includes both "resin film" and "resin sheet".
[0043] In this specification, the glass transition temperature of a general material is represented by "Tg".
[0044] [LCD display protection plate]
[0045] The invention relates to a liquid crystal display protection plate, which can be suitably used for protecting a liquid crystal display and a touch panel display formed by combining a liquid crystal display and a touch panel.
[0046] The liquid crystal display protective plate of the present invention comprises a resin plate having a base material layer laminated on both sides of a phase difference adjustment layer, and preferably further comprises a cured coating film. The resin plate is preferably an extrusion-molded plate.
[0047] The phase difference adjustment layer contains a transparent thermoplastic resin (A) having specific optical properties, and the base layer contains a transparent thermoplastic resin (B) having specific optical properties. The glass transition temperature of the phase difference adjustment layer is defined as Tg A (°C), and the glass transition temperature of the substrate layer is defined as Tg B (℃), Tg A <Tg B The in-plane retardation value (also referred to as “Re value”) of the resin plate is 50 to 330 nm.
[0048] Figure 1 , Figure 2 The schematic cross-sectional view of the first and second embodiments of the liquid crystal display protection plate of the present invention. In the figure, reference numerals 1 and 2 represent the liquid crystal display protection plate, reference numeral 16 represents the resin plate, reference numeral 21 represents the phase difference adjustment layer, reference numeral 22 represents the substrate layer, and reference numeral 31 represents the cured coating.
[0049] The liquid crystal display protection plate 1 of the first embodiment is composed of a three-layered resin plate 16 in which a base material layer 22 is laminated on both surfaces of a phase difference adjustment layer 21 .
[0050] In the liquid crystal display protection plate 2 of the second embodiment, a cured coating film 31 is formed on at least one surface of a three-layered resin plate 16 in which a base material layer 22 is laminated on both surfaces of a phase difference adjustment layer 21 . Figure 2 In the illustrated example, cured films 31 are formed on both surfaces of the resin plate 16 .
[0051] The structure of the liquid crystal display protection plate is not limited to the illustrated example, and the design can be appropriately changed without departing from the gist of the present invention.
[0052] In the present invention, the phase difference adjustment layer contains a photoelastic coefficient (C A ) has an absolute value of 10.0×10 -12 / Pa or less, orientation birefringence (Δn A ) has an absolute value of 10.0×10 -4 ~100.0×10 -4 The transparent thermoplastic resin (A), the oriented birefringence (Δn A ) is obtained by uniaxially stretching a test piece having a width of 20 mm, a length of 40 mm and a thickness of 1 mm at a temperature 10°C higher than the glass transition temperature at a speed of 3 mm / min at a stretching ratio of 100% and measuring the in-plane retardation value of the central part of the test piece after uniaxial stretching.
[0053] "Delay" refers to the phase difference between light in the direction of the molecular main chain and light in the direction perpendicular to the molecular main chain. It is generally known that polymers can be formed into any shape by heating and melting, but delay occurs due to stress generated during heating and cooling and molecular orientation. It should be noted that in this specification, unless otherwise specified, "delay" means delay in the plane.
[0054] Generally, the Re value of a resin plate is represented by the following formula (i).
[0055] [Re value of resin plate] = [birefringence (ΔN)] × [thickness (d)] (i)
[0056] The birefringence (ΔN) is represented by the following formula (ii).
[0057] [Birefringence] = [stress birefringence] + [orientation birefringence] (ii)
[0058] The stress birefringence and the orientation birefringence are represented by the following formulas (iii) and (iv), respectively.
[0059] [Stress birefringence] = [Photoelastic coefficient (C)] × [Stress] (iii)
[0060] [Orientation birefringence] = [intrinsic birefringence] × [degree of orientation] (iv)
[0061] In formula (iv), the degree of orientation is a value in the range of 0 to 1.0.
[0062] The relationship between stress and birefringence and the relationship between orientation birefringence, stress birefringence and photoelastic coefficient are shown in the figure. Figure 6 .
[0063] In the present invention, using Figure 6 The photoelastic coefficient and the orientation birefringence are schematically shown to determine the optical characteristics of the transparent thermoplastic resin (A) and the transparent thermoplastic resin (B).
[0064] The LCD protective plate of the present invention includes a phase difference adjustment layer containing a transparent thermoplastic resin (A) having the above-mentioned specific optical properties, which can suppress the reduction in visibility such as rainbow patterns and black screens when the LCD protective plate located on the LCD screen is observed through a polarizing filter.
[0065] In this specification, unless otherwise specified, the "Re value of the resin plate" is the average value of the Re values of the birefringent pixels of about 110,000 points within the measurement range of 17 cm in width and 22 cm in length. Unless otherwise specified, the "standard deviation of the Re value of the resin plate" is the standard deviation of the Re values of the birefringent pixels of about 110,000 points within the measurement range of 17 cm in width and 22 cm in length.
[0066] The Re value of the resin plate is 50 to 330 nm, preferably 70 to 250 nm, more preferably 80 to 200 nm, and particularly preferably 90 to 150 nm. When the Re value is less than the above lower limit, when observing the LCD protection plate located on the LCD screen through a polarizing filter, a black screen may occur regardless of the relationship between the polarization axis of the outgoing light and the transmission axis of the polarizing filter. When the Re value exceeds the above upper limit, when viewing through a polarizing filter, the difference in transmittance of each wavelength in the visible light region becomes larger, and various colors may be seen, and visibility is reduced (coloration phenomenon).
[0067] The smaller the standard deviation of the Re value of the resin plate, the less the fluctuation of the Re value, which is preferred. The standard deviation of the Re value is preferably 15 nm or less, more preferably 10 nm or less, further preferably 7 nm or less, particularly preferably 5 nm or less, and most preferably 4 nm or less. When the standard deviation of the Re value is below the above upper limit, when the liquid crystal display protection plate located on the liquid crystal screen is observed through a polarizing filter, the rainbow pattern caused by the fluctuation of the Re value is suppressed, and the visibility is improved.
[0068] The average value and standard deviation of the Re value of the resin plate can be measured by, for example, the method described in the section of [Examples] described later using a retardation measuring instrument "WPA-100-L" manufactured by Filtration Technologies Co., Ltd.
[0069] The overall thickness (d) of the resin plate is not particularly limited, but is preferably 0.2 to 5.0 mm, more preferably 0.5 to 4.0 mm, and particularly preferably 1.0 to 3.5 mm. If it is too thin, the rigidity of the liquid crystal display protective plate may become insufficient, and if it is too thick, it may hinder the weight reduction of the liquid crystal display or the touch panel display including it.
[0070] (Phase difference adjustment layer)
[0071] The resin plate included in the liquid crystal display protective plate of the present invention includes a phase difference adjustment layer. The phase difference adjustment layer is a layer that mainly determines the Re value of the liquid crystal display protective plate and contains a transparent thermoplastic resin (A) having specific optical properties.
[0072] <Transparent thermoplastic resin (A)>
[0073] The photoelastic coefficient (C A ) has an absolute value of 10.0×10 -12 / Pa or less, preferably 8.0×10 -12 / Pa or less, more preferably 6.0×10 -12 / Pa or less, particularly preferably 5.0×10 -12 / Pa or less, and most preferably 4.0×10 -12 / Pa or less. Photoelastic coefficient (C A ) is less than the above upper limit, the stress birefringence caused by the residual stress generated during the molding process such as extrusion molding is small (reference Figure 6 ), the standard deviation of the Re value of the LCD protective plate can be reduced. As a result, when the LCD protective plate located on the LCD screen is observed through a polarizing filter, rainbow patterns caused by fluctuations in the Re value are suppressed, and visibility is improved.
[0074] Orientation birefringence (Δn A ) has an absolute value of 10.0×10 -4 ~100.0×10 -4 , preferably 20.0×10 -4 ~90.0×10 -4 , more preferably 30.0×10 -4 ~70.0×10 -4 , particularly preferably 35.0×10 -4 ~60.0×10 -4 Oriented birefringence (Δn A ) is within the above range, the Re value of the liquid crystal display protection plate can be controlled to an appropriate range.
[0075] Orientation birefringence depends on the degree of orientation of the polymer and is therefore affected by production conditions such as molding conditions and stretching conditions. In this specification, "orientation birefringence" is measured by the method described in the section "Examples" described later unless otherwise specified.
[0076] The transparent thermoplastic resin (A) may be any resin satisfying the photoelastic coefficient (C A ) and orientation birefringence (Δn A ) is not particularly limited.
[0077] In one embodiment, the transparent thermoplastic resin (A) may contain one or more aromatic vinyl monomer units. The aromatic vinyl monomer is not particularly limited, and examples thereof include: styrene (St); core alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-ethylstyrene, and 4-tert-butylstyrene; α-alkyl-substituted styrenes such as α-methylstyrene and 4-methyl-α-methylstyrene, etc. Among them, styrene (St) is preferred from the viewpoint of availability.
[0078] The content of the aromatic vinyl monomer unit in the transparent thermoplastic resin (A) is V [mass %], and the thickness of the phase difference adjustment layer is T A [mm]. Their product (V×T A ) preferably satisfies the following formula (1).
[0079] 6.0≤V×T A ≤30.0…(1)
[0080] The photoelastic coefficient (C A ) is small, and the stress birefringence is substantially zero. When the transparent thermoplastic resin (A) contains aromatic vinyl monomer units such as styrene (St) units, the orientation birefringence (Δn A ) has a tendency to depend on the content V [mass %] of the aromatic vinyl monomer unit in the transparent thermoplastic resin (A). Therefore, V×T A It is strongly correlated with the Re value of the LCD protection plate. A When the above formula (1) is satisfied, the Re value of the liquid crystal display protective plate can be controlled within an appropriate range.
[0081] The transparent thermoplastic resin (A) may be a copolymer having, in addition to the aromatic vinyl monomer unit, other monomer units such as a methacrylate unit such as a methyl methacrylate (MMA) unit, an acid anhydride unit such as a maleic anhydride unit, and an acrylonitrile unit.
[0082] Specific examples of the transparent thermoplastic resin (A) containing an aromatic vinyl monomer unit include methacrylate-styrene copolymers (MS resins); styrene-maleic anhydride copolymers (SMA resins); styrene-methacrylate-maleic anhydride copolymers (SMM resins); acrylonitrile-styrene copolymers (AS resins), etc. These can be used alone or in combination of two or more.
[0083] The content V [mass %] of the aromatic vinyl monomer unit in the transparent thermoplastic resin (A) is not particularly limited, but is preferably 10 to 90 mass %, and more preferably 20 to 80 mass %.
[0084] The transparent thermoplastic resin (A) may satisfy the photoelastic coefficient (C A ) and orientation birefringence (Δn A ), it may be a resin that does not contain an aromatic vinyl monomer unit. As the transparent thermoplastic resin (A) that does not contain an aromatic vinyl monomer unit, there may be mentioned a modified methacrylic resin containing a methacrylate unit such as a methyl methacrylate unit, and at least one unit selected from a glutarimide unit, an N-substituted or unsubstituted maleimide unit, and a lactone ring unit. These may be used alone or in combination.
[0085] The transparent thermoplastic resin (A) may be a material satisfying the photoelastic coefficient (C A ) and orientation birefringence (Δn A ) and the resin containing the aromatic vinyl monomer unit in the range of A ) and orientation birefringence (Δn A ) of a resin (modified methacrylic resin, etc.) that does not contain an aromatic vinyl monomer unit.
[0086] In the present invention, the photoelastic coefficient and / or orientation birefringence of general methacrylic resins (unmodified methacrylic resins) and polycarbonate resins other than the above are outside the specified range of the present invention and are not contained in the transparent thermoplastic resin (A).
[0087] The absolute value of the photoelastic coefficient of polycarbonate resin is 90×10 -12 / Pa, which is very large, and the Re value changes due to slight stress. Therefore, when using polycarbonate resin, it is difficult to obtain an optically uniform LCD protection plate. For example, when observing the LCD protection plate on the LCD screen through a polarizing filter, rainbow patterns may be observed due to fluctuations in the Re value.
[0088] The absolute value of the photoelastic coefficient of methacrylic resin is as low as 3.2×10 -12 / Pa, Re value is not easily changed by stress. Therefore, when using methacrylic resin, an optically uniform LCD protective plate can be obtained. However, the absolute value of the orientation birefringence of methacrylic resin is as low as 4.0×10 -4 Therefore, although it depends on the thickness, the Re value of the obtained LCD protective plate is about 20nm and tends to decrease. Therefore, when the LCD protective plate located on the LCD screen is observed through a polarizing filter, the screen may become black depending on the angle between the polarization axis of the outgoing light and the transmission axis of the polarizing filter, and the visibility of the image may be reduced.
[0089] The thickness of the phase difference adjustment layer (T A ) is not particularly limited, but when the transparent thermoplastic resin (A) contains an aromatic vinyl monomer unit, it is preferably designed so as to satisfy the above formula (1). A It is preferably 0.05 to 3.0 mm, more preferably 0.1 to 1.0 mm, particularly preferably 0.1 to 0.5 mm, and most preferably 0.1 to 0.3 mm.
[0090] The phase difference adjustment layer may contain a small amount of one or more other polymers whose photoelastic coefficient and / or orientation birefringence are outside the provisions of the transparent thermoplastic resin (A). There is no particular limitation on the types of other polymers, and examples thereof include: general unmodified methacrylic resins, polycarbonate resins, polyolefins such as polyethylene and polypropylene, polyamides, polyphenylene sulfide, polyetheretherketone, polyester, polysulfone, polyphenylene ether, polyimide, polyetherimide, polyacetal and other thermoplastic resins; phenolic resins, melamine resins, silicone resins, epoxy resins and other thermosetting resins; and the like.
[0091] Typical unmodified methacrylic resins include, for example, resins containing one or more methacrylate units.
[0092] The content of the transparent thermoplastic resin (A) in the phase difference adjustment layer is preferably relatively high, preferably 90% by mass or more, more preferably 95% by mass or more, and particularly preferably 98% by mass or more. The content of other polymers in the phase difference adjustment layer is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 2% by mass or less.
[0093] The phase difference adjustment layer may contain various additives as needed. As additives, colorants, antioxidants, thermal degradation inhibitors, ultraviolet absorbers, light stabilizers, lubricants, release agents, polymer processing aids, antistatic agents, flame retardants, light diffusers, matting agents, core-shell particles and block copolymers and other rubber components (impact resistance modifiers) and phosphors can be listed. The content of additives can be appropriately set within the range that does not impair the effect of the present invention. Relative to 100 parts by mass of the constituent resin of the phase difference adjustment layer, for example, the content of the antioxidant is preferably 0.01 to 1 parts by mass, the content of the ultraviolet absorber is 0.01 to 3 parts by mass, the content of the light stabilizer is 0.01 to 3 parts by mass, and the content of the lubricant is 0.01 to 3 parts by mass.
[0094] When other polymers and / or additives are added to the phase difference adjusting layer, the timing of addition may be during the polymerization of the transparent thermoplastic resin (A) or after the polymerization.
[0095] The phase difference adjustment layer may be a resin layer comprising a resin composition containing a transparent thermoplastic resin (A) and a known rubber component (impact resistance modifier). As the rubber component, multilayer polymer particles of a core-shell structure, rubber-like polymers and block polymers having a salami structure, etc. may be cited. The rubber component may contain a diene monomer unit and an alkyl acrylate monomer unit, etc. From the perspective of the transparency of the phase difference adjustment layer, the difference between the refractive index of the rubber component and the refractive index of the transparent thermoplastic resin (A) as the main component is preferably smaller.
[0096] The glass transition temperature (Tg A ) As long as Tg is met A <Tg B The temperature is not particularly limited, but is preferably 80 to 160°C, more preferably 90 to 150°C, particularly preferably 95 to 140°C, and most preferably 100 to 130°C.
[0097] It should be noted that the glass transition temperature (Tg A )" is the glass transition temperature of all the constituent materials of the phase difference adjusting layer including one or more transparent thermoplastic resins (A) and, if necessary, one or more optional components.
[0098] (Base material layer)
[0099] The resin plate included in the liquid crystal display protective plate of the present invention includes a base material layer laminated on both surfaces of the above-mentioned retardation adjusting layer and having a glass transition temperature (Tg) higher than that of the retardation adjusting layer.
[0100] The substrate layer is laminated on both sides of the phase difference adjustment layer for the purpose of increasing the overall thickness (d) of the resin plate, improving the rigidity of the resin plate, improving the heat resistance of the surface of the resin plate, etc. The substrate layer is preferably a resin layer that does not affect the Re value of the liquid crystal display protective plate, and is preferably a resin layer containing a transparent thermoplastic resin (B) having a sufficiently small photoelastic coefficient and orientation birefringence.
[0101] The composition and thickness of the base layers laminated on both surfaces of the phase difference adjusting layer may be the same or different as long as the respective base layers are resin layers containing the transparent thermoplastic resin (B) having the above-mentioned optical properties.
[0102] <Transparent thermoplastic resin (B)>
[0103] The photoelastic coefficient (C B ) is preferably smaller, preferably 10.0×10 -12 / Pa or less, more preferably 8.0×10 -12 / Pa or less, more preferably 6.0×10 -12 / Pa or less, particularly preferably 5.0×10 -12 / Pa or less, and most preferably 4.0×10 -12 / Pa or less. Photoelastic coefficient (C B ) is below the upper limit, the stress birefringence caused by the residual stress generated during the molding process such as extrusion molding is sufficiently small (reference Figure 6 ), the standard deviation of the Re value of the resin plate can be reduced. As a result, when the LCD protection plate located on the LCD screen is observed through a polarizing filter, rainbow patterns caused by fluctuations in the Re value are suppressed, and visibility is improved.
[0104] Oriented birefringence (Δn B ) is preferably smaller, preferably less than 10.0×10 -4 , more preferably 8.0×10 -4 Below, more preferably 6.0×10 -4 Below, particularly preferably 4.0×10 -4 Below, the most preferred is 2.0×10 -4 The following is the orientation birefringence (Δn B ) is below the upper limit, the influence on the Re value of the resin plate is sufficiently small (reference Figure 6 ), the Re value of the resin plate can be well controlled within an appropriate range.
[0105] The transparent thermoplastic resin (B) may be any resin satisfying the photoelastic coefficient (C B) and orientation birefringence (Δn B ) is not particularly limited. Specific examples include general unmodified methacrylic resins (PM), modified methacrylic resins modified with glutarimide units, N-substituted or unsubstituted maleimide units, lactone ring units, and cycloolefin polymers (COP). The transparent thermoplastic resin (B) can be used alone or in combination.
[0106] The methacrylic resin (PM) is a homopolymer or copolymer containing structural units derived from one or more methacrylic acid esters. From the viewpoint of transparency, the content of the methacrylic acid ester monomer units in the methacrylic resin (PM) is preferably 50% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, and may be 100% by mass.
[0107] Preferred methacrylates include, for example, methyl methacrylate (MMA), ethyl methacrylate, butyl methacrylate, phenyl methacrylate, benzyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, monocyclic aliphatic hydrocarbon methacrylate, polycyclic aliphatic hydrocarbon methacrylate, etc. From the viewpoint of transparency, the methacrylic resin (PM) preferably contains MMA units, and the content of the MMA units in the methacrylic resin (PM) is preferably 50% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, and may be 100% by mass.
[0108] Methacrylic resin (PM) may contain structural units derived from one or more other monomers other than methacrylate. As other monomers, acrylates such as methyl acrylate (MA), ethyl acrylate, butyl acrylate, cyclohexyl acrylate, phenyl acrylate, benzyl acrylate, 2-ethylhexyl acrylate and 2-hydroxyethyl acrylate can be listed; styrenes; acrylonitrile, methacrylonitrile; maleic anhydride, phenylmaleimide, cyclohexylmaleimide; etc. Among them, MA is preferred from the viewpoint of transparency. For example, the copolymer of MMA and MA has excellent transparency and is therefore preferred. The content of MMA in the copolymer is preferably 80% by mass or more, more preferably 85% by mass or more, particularly preferably 90% by mass or more, and can be 100% by mass.
[0109] Methacrylic resin (PM) is preferably obtained by polymerizing one or more methacrylates containing MMA and other monomers as needed. When using multiple monomers, multiple monomers are usually mixed to prepare a monomer mixture and then polymerized. There is no particular restriction on the polymerization method, and from the viewpoint of productivity, free radical polymerization methods such as bulk polymerization, suspension polymerization, solution polymerization and emulsion polymerization are preferred.
[0110] The substrate layer may contain a methacrylic resin (PM-H) having a high syndiotacticity (rr) (hereinafter sometimes simply referred to as "syndiotacticity (rr) or rr ratio") in terms of triad. Generally, the higher the rr ratio of the methacrylic resin (PM), the higher the glass transition temperature (Tg) and the higher the heat resistance.
[0111] From the improvement of heat resistance (Tg B From the viewpoint of improving the RR ratio, the methacrylic resin (PM-H) preferably has an rr ratio of 58% or more, more preferably 59% or more, further preferably 60% or more, particularly preferably 62% or more, and most preferably 65% or more.
[0112] The upper limit of the rr ratio is not particularly limited, but is preferably 99%, more preferably 85%, further preferably 77%, particularly preferably 76%, and most preferably 75%, from the viewpoint of mechanical properties such as toughness, tear resistance and impact resistance, and film forming properties.
[0113] In the present specification, the syndiotacticity (rr) based on triads is a ratio in which two chains (diad) of a chain of three consecutive structural units (triad) are both racemic.
[0114] It should be noted that the chains (diads) of structural units in polymer molecules with the same stereo configuration are called meso, and those with opposite stereo configurations are called racemo, which are represented by m and r, respectively.
[0115] The syndiotacticity (rr) (%) of the methacrylic resin in terms of triad can be measured in deuterated chloroform at 30°C. 1 The H-NMR spectrum was used to measure the area (X) of the 0.6 to 0.95 ppm region and the area (Y) of the 0.6 to 1.35 ppm region when TMS was set to 0 ppm, and the result was calculated from the formula: (X / Y)×100.
[0116] The methacrylic resin (PM-H) may contain a plurality of methacrylic resins having different rr ratios. For example, the methacrylic resin (PM-H) may contain a first methacrylic resin (H1) having an rr ratio of 65% or more and a second methacrylic resin (H2) having an rr ratio of 45 to 58%. In this case, the content of the first methacrylic resin (H1) is preferably 40 to 70 parts by mass and the content of the second methacrylic resin (H2) is preferably 60 to 30 parts by mass, relative to 100 parts by mass of the total amount of the first methacrylic resin (H1) and the second methacrylic resin (H2). One or more of the first methacrylic resin (H1) and the second methacrylic resin (H2) may be used.
[0117] As described above, by using the first methacrylic resin (H1) having an rr ratio of 65% or more and the second methacrylic resin (H2) having an rr ratio of 45 to 58%, a methacrylic resin (PM-H) having an rr ratio of 58% or more and suitable properties can be stably obtained.
[0118] By using the first methacrylic resin (H1) having an rr ratio of 65% or more, the heat resistance can be further improved, but when the resin is used alone, there is a tendency that mechanical properties such as toughness, tear resistance and impact resistance are reduced, and film forming properties and handling properties are reduced. By using the first methacrylic resin (H1) having an rr ratio of 65% or more and the second methacrylic resin (H2) having an rr ratio of 58% or less in combination, the heat resistance can be improved, and mechanical properties such as toughness, tear resistance and impact resistance, and film forming properties and handling properties can be improved.
[0119] As long as the photoelastic coefficient (C B ) and orientation birefringence (Δn B ), the types of resins exemplified as the transparent thermoplastic resin (B) and as the transparent thermoplastic resin (A) (specifically, MS resin, SMA resin, SMM resin, AS resin, and modified methacrylic resin, etc.) can be used. Depending on the monomer composition or the modification rate, the types of resins exemplified as the transparent thermoplastic resin (A) may be used as the transparent thermoplastic resin (B).
[0120] The photoelastic coefficient and orientation birefringence of the polycarbonate-based resin are outside the prescribed ranges of the present invention, and the polycarbonate-based resin is not contained in the transparent thermoplastic resin (B).
[0121] The absolute value of the photoelastic coefficient of polycarbonate resin is 90×10 -12 / Pa, which is very large, and the Re value changes due to slight stress. Therefore, when using polycarbonate resin, it is difficult to obtain an optically uniform LCD protection plate. For example, when observing the LCD protection plate on the LCD screen through a polarizing filter, rainbow patterns may be observed due to fluctuations in the Re value.
[0122] As described above, the glass transition temperature of the phase difference adjustment layer is set to Tg A (°C), and the glass transition temperature of the substrate layer is defined as Tg B (℃), Tg A <Tg B With this configuration, the heat resistance of the surface of the resin plate can be improved.
[0123] Tg A With Tg B The difference between Tg and A +5≤Tg B , more preferably Tg A +10≤Tg B , particularly preferably Tg A +15≤Tg B .
[0124] The glass transition temperature (Tg B ) As long as Tg is met A <Tg B There is no special restriction. B The upper limit of Tg is preferably 155°C, more preferably 145°C, particularly preferably 135°C, and most preferably 130°C. B The lower limit of is preferably 115°C, more preferably 120°C, particularly preferably 125°C.
[0125] It should be noted that the glass transition temperature (Tg B )" is the glass transition temperature of all constituent materials of the substrate layer including one or more transparent thermoplastic resins (B) and, if necessary, one or more optional components.
[0126] LCD protection plates may be exposed to high temperatures during the manufacturing process.
[0127] A cured coating with low reflectivity for improving scratch resistance (hard coating) and / or visibility can be formed on at least one surface of the resin plate. In the process of forming the cured coating, the resin plate may be exposed to high temperatures. For example, a thermosetting coating material needs to be heated during curing, and a photocurable coating material is heated when irradiated with light. In the case where the coating material contains a solvent, it is sometimes heated in order to dry the solvent. In particular, when a thermosetting coating material is used, the resin plate may be exposed to a higher temperature than when other coating materials are used.
[0128] If the heat resistance of the surface of the resin plate is insufficient, the resin plate may be warped or have its surface roughened due to the heat received during the curing of the thermosetting coating material.
[0129] When the curing temperature of the thermosetting coating material is lowered, the curing time becomes longer and the productivity decreases. Furthermore, the cross-linking reaction does not proceed well, thereby reducing the adhesion between the surface resin of the resin plate and the cured coating, and the cured coating may peel off from the resin plate in a wet heat environment or in a wet heat test.
[0130] In the resin plate included in the liquid crystal display protective plate of the present invention, a base material layer is laminated on both sides of the phase difference adjustment layer. The glass transition temperature of the phase difference adjustment layer is Tg A , and the glass transition temperature of the substrate layer is set to Tg B When Tg A <Tg B . By laminating a substrate layer with a relatively high Tg on both sides of the phase difference adjustment layer, the heat resistance of both sides of the resin plate can be improved. Therefore, even when a thermosetting coating material is used to form a cured coating, warping and surface roughness of the resin plate can be suppressed without lowering the curing temperature. There is no need to lower the curing temperature and the curing is performed at a suitable temperature. Therefore, a cured coating can be formed with good productivity, and the surface resin of the resin plate also has good adhesion to the cured coating.
[0131] The resin plate included in the liquid crystal display protective plate of the present invention is unlikely to warp not only during the formation of a cured coating film but also under a wet heat environment or in a wet heat test.
[0132] When the base material layer contains a methacrylic resin (PM), in addition to the above-mentioned effects, an effect of improving the surface hardness of the resin plate can be obtained, which is preferred.
[0133] The total thickness of the base material layers stacked on both sides of the phase difference adjustment layer is T. B The total thickness of the substrate layer (T B ) is not particularly limited and can be appropriately designed according to the desired thickness and rigidity of the liquid crystal display protection plate. BIt is preferably 0.05 to 4.5 mm, more preferably 0.5 to 4.0 mm, particularly preferably 1.0 to 3.5 mm, and most preferably 1.0 to 3.0 mm.
[0134] The thickness of the phase difference adjustment layer (T A ) and the total thickness of the substrate layer (T B ) is not particularly limited, but is preferably T A <T B In other words, T B / T A > 1. More preferably T B / T A ≥1.2, particularly preferably T B / T A ≥1.5, most preferably T B / T A ≥2.0.
[0135] T A With T B When the above relationship exists, the total thickness of the substrate layer (T B ) relative to the overall thickness (d) of the resin plate is sufficiently large, so that the heat resistance of both sides of the resin plate can be improved more effectively, and warping and surface roughness of the resin plate during the formation of the cured coating, as well as warping in a wet heat environment or in a wet heat test can be more effectively suppressed.
[0136] The substrate layer may contain a small amount of one or more other polymers having photoelastic coefficients and / or orientation birefringence other than those specified for the transparent thermoplastic resin (B). The types of other polymers are not particularly limited, and examples thereof include: other thermoplastic resins such as polycarbonate resins, polyolefins such as polyethylene and polypropylene, polyamides, polyphenylene sulfide, polyetheretherketone, polyester, polysulfone, polyphenylene ether, polyimide, polyetherimide and polyacetal; and thermosetting resins such as phenolic resins, melamine resins, silicone resins and epoxy resins.
[0137] The content of the transparent thermoplastic resin (B) in the substrate layer is preferably relatively high, preferably 90% by mass or more, more preferably 95% by mass or more, and particularly preferably 98% by mass or more. The content of other polymers in the substrate layer is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 2% by mass or less.
[0138] The base material layer may contain various additives as required. Examples of the types of additives and preferred addition amounts are the same as those of the additives that can be used in the phase difference adjustment layer.
[0139] When other polymers and / or additives are added to the base material layer, the timing of addition may be during the polymerization of the transparent thermoplastic resin (B) or after the polymerization.
[0140] The substrate layer may be a resin layer comprising a resin composition containing a transparent thermoplastic resin (B) and a known rubber component (impact resistance modifier). The examples of the rubber component are the same as the rubber component that can be used in the phase difference adjustment layer. From the perspective of the transparency of the substrate layer, the difference between the refractive index of the rubber component and the refractive index of the transparent thermoplastic resin (B) as the main component is preferably smaller.
[0141] (Other resin layers)
[0142] The resin plate included in the liquid crystal display protection plate of the present invention may have other resin layers other than the phase difference adjustment layer and the substrate layer. As the laminated structure of the resin plate, there can be listed: a three-layer structure of substrate layer-phase difference adjustment layer-substrate layer; a four-layer structure of substrate layer-phase difference adjustment layer-substrate layer-other resin layers; a four-layer structure of substrate layer-phase difference adjustment layer-other resin layers-substrate layer, etc.
[0143] (Curing film)
[0144] The LCD protection plate of the present invention may have a cured film formed on at least one surface of a resin plate having a base material layer laminated on both surfaces of a phase difference adjustment layer as required. The LCD protection plate of the present invention may have a cured film on at least one outermost surface.
[0145] The cured film can function as a scratch-resistant layer (hard coat layer) or a low-reflection layer for improving visibility. The cured film can be formed by a known method.
[0146] Examples of the material of the cured film include inorganic, organic, organic-inorganic, and silicone-based materials. From the viewpoint of productivity, organic and organic-inorganic materials are preferred.
[0147] The inorganic cured film can be formed by forming an inorganic material such as SiO 2 , Al 2 O 3 , TiO 2 , or metal oxides such as ZrO 2 by vapor phase film formation such as vacuum deposition and sputtering.
[0148] The organic cured film can be formed by, for example, applying a coating containing a resin such as melamine resin, alkyd resin, polyurethane resin, and acrylic resin and curing it by heating, or applying a coating containing a multifunctional acrylic resin and curing it by ultraviolet light.
[0149] The organic-inorganic cured coating can be formed by, for example, applying an ultraviolet-curable hard coating containing inorganic ultrafine particles such as silica ultrafine particles with photopolymerizable functional groups introduced on the surface and a curable organic component, and then irradiating the hard coating with ultraviolet light to cause the curable organic component to polymerize with the photopolymerizable functional groups of the inorganic ultrafine particles. In this method, a cross-linked coating film in the form of a network in which the inorganic ultrafine particles are dispersed in the organic matrix in a state of chemically bonding with the organic matrix can be obtained.
[0150] The silicone-based cured film can be formed, for example, by polycondensing partial hydrolyzates of carbon-functional alkoxysilane, alkyltrialkoxysilane, tetraalkoxysilane, or the like, or materials containing colloidal silica mixed therewith.
[0151] Among the above methods, examples of the material coating method include dip coating, various roll coatings such as gravure roll coating, flow coating, wire bar coating, knife coating, spray coating, die coating, and bar coating.
[0152] As described above, in particular, when a thermosetting coating material is used, the resin plate may be exposed to a higher temperature than when other coating materials are used. The resin plate included in the liquid crystal display protection plate of the present invention has a structure in which a substrate layer with a relatively high glass transition temperature (Tg) is laminated on both sides of the phase difference adjustment layer, and the heat resistance of both sides is excellent. Therefore, the present invention is particularly useful in the case of forming a cured coating using a thermosetting coating material.
[0153] The thickness of the scratch-resistant (hard-coated) cured film (scratch-resistant layer, hard-coating layer) is preferably 2 to 30 μm, more preferably 5 to 20 μm. If it is too thin, the surface hardness may become insufficient, and if it is too thick, cracks may be generated due to bending in the manufacturing process. The thickness of the low-reflectivity cured film (low-reflectivity layer) is preferably 80 to 200 nm, more preferably 100 to 150 nm. If it is too thin or too thick, the low-reflectivity performance may become insufficient.
[0154] In addition, the LCD protection plate of the present invention may have a known surface treatment layer such as an antiglare layer, an antireflection layer, and an anti-fingerprint layer on the surface as needed.
[0155] [Method for manufacturing liquid crystal display protective plate]
[0156] The method for producing a liquid crystal display protective plate of the present invention comprises a step (X) of preparing a resin plate in which a substrate layer having a relatively high glass transition temperature (Tg) is laminated on both surfaces of a retardation adjustment layer.
[0157] The method for producing a liquid crystal display protective plate of the present invention further comprises a step (Y) of forming a cured film on at least one surface of the obtained resin plate, if necessary.
[0158] (Process (X))
[0159] The resin sheet of the laminated structure can be formed by known methods such as cast molding, injection molding, and extrusion molding, among which co-extrusion molding is preferred.
[0160] Hereinafter, a method for producing a resin plate by co-extrusion molding will be described.
[0161] Figure 3 Schematic diagram of an extrusion molding device including a T-die 11, first to third cooling rolls 12 to 14, and a pair of take-off rolls 15 as one embodiment is shown in FIG.
[0162] The constituent resins of each layer are melt-kneaded using an extruder, and co-extruded in a plate-like form from a T-die 11 having a wide discharge port in the form of a desired laminated structure.
[0163] Examples of the lamination method include a feed block method in which lamination is performed before flowing into a T-die and a multi-manifold method in which lamination is performed inside a T-die. From the viewpoint of improving the smoothness of the interface between layers, the multi-manifold method is preferred.
[0164] The resin sheet of the laminated structure in a molten state co-extruded from the T-die 11 is pressurized and cooled using a plurality of cooling rollers 12 to 14. The pressurized and cooled resin sheet 16 is taken away by a pair of take-off rollers 15. The number of cooling rollers can be appropriately designed. It should be noted that the configuration of the manufacturing device can be appropriately designed and changed within the scope of the present invention.
[0165] In the present invention, the resin plate is formed so that the Re value of the resin plate is 50 to 330 nm.
[0166] In order to control the Re value, it is necessary to control the orientation of the molecules. The orientation of the molecules occurs, for example, due to the stress during molding near the glass transition temperature of the polymer. By optimizing the manufacturing conditions during the extrusion molding process to control the orientation of the molecules, the Re value of the resin plate after extrusion molding can be optimized.
[0167] (Process (Y))
[0168] In step (Y), an inorganic or organic cured film is formed on at least one surface of the resin plate obtained in step (X) by a known method. The method for forming the cured film is as described above, so it is omitted here.
[0169] (Other processes)
[0170] The method for producing a liquid crystal display protective plate of the present invention may include other steps in addition to the above steps (X) and (Y) as necessary.
[0171] For example, between step (X) and step (Y), the following step may be added for the purpose of improving the adhesion of the cured film to the resin plate: the surface of the resin plate obtained in step (X) on which the cured film is formed is subjected to surface roughening treatment such as plasma treatment, sandblasting treatment and solvent treatment; surface oxidation treatment such as corona discharge treatment, chromic acid treatment, ozone irradiation treatment and ultraviolet irradiation treatment.
[0172] As described above, according to the present invention, it is possible to provide a liquid crystal display protection plate capable of suppressing a decrease in visibility such as rainbow, black screen, and coloration when the liquid crystal display protection plate located on a liquid crystal screen is observed through a polarizing filter.
[0173] According to the present invention, it is possible to provide a liquid crystal display protective plate in which the occurrence of warping is suppressed even in a wet heat environment or a wet heat test.
[0174] The liquid crystal display protection plate of the present invention may include a resin plate and a cured coating as required. According to the present invention, a liquid crystal display protection plate including a resin plate and a cured coating can be provided, which can suppress warping and surface roughness of the resin plate without lowering the curing temperature even when a thermosetting coating material is used to form the cured coating, and has good adhesion between the resin plate and the cured coating.
[0175] [use]
[0176] The liquid crystal display protection plate of the present invention is suitable as a protection plate for liquid crystal displays or touch panel displays used in digital information devices such as ATMs, vending machines, televisions, mobile phones (including smart phones), personal computers, tablet personal computers, etc., digital audio players, portable game consoles, copiers, fax machines and car navigation systems of financial institutions such as banks, etc., or used in portable information terminals (PDAs).
[0177] The liquid crystal display protection plate of the present invention is suitable as a protection plate for a liquid crystal display for vehicle use, for example.
[0178] Example
[0179] Examples of the present invention and comparative examples are described.
[0180] [Evaluation items and evaluation methods]
[0181] The evaluation items and evaluation methods are as follows.
[0182] (Content of Aromatic Vinyl Monomer Unit in Transparent Thermoplastic Resin (A))
[0183] The content (V mass %) of the aromatic vinyl monomer unit in the MS resin was measured using a nuclear magnetic resonance apparatus ("GX-270" manufactured by JEOL Ltd.). 1 It was determined by H-NMR method.
[0184] (Glass transition temperature (Tg) of transparent thermoplastic resin)
[0185] The glass transition temperature (Tg) of the transparent thermoplastic resin is measured using a differential scanning calorimeter ("DSC-50", manufactured by Rigaku Corporation). 10 mg of the transparent thermoplastic resin is placed in an aluminum pan and placed in the above-mentioned device. After nitrogen substitution for more than 30 minutes, in a nitrogen gas flow of 10 ml / min, the temperature is first raised from 25°C to 200°C at a rate of 20°C / min, maintained for 10 minutes, and cooled to 25°C (first scan). Next, the temperature is raised to 200°C at a rate of 10°C / min (second scan), and the glass transition temperature (Tg) is calculated by the midpoint method from the results obtained in the second scan. It should be noted that when multiple Tg data are obtained in a resin composition containing two or more resins, the value of the resin from the main component is used as the Tg data.
[0186] (Photoelastic coefficient of transparent thermoplastic resin)
[0187] A transparent thermoplastic resin was press-formed to obtain a 1.0 mm thick resin plate. A test piece with a width of 15 mm and a length of 80 mm was cut from the central portion of the obtained resin plate. The two ends of the test piece in the longitudinal direction were clamped by a pair of chucks. The distance between the chucks was set to 70 mm.
[0188] Tension was applied to the test piece using an "X-axis Air Stage" manufactured by Oji Testing Instruments Co., Ltd. The tension was increased in steps of 10 N from 0 N to 30 N. The tension was monitored using a "Sensor Separate Type Digital Force Gauge ZTS-DPU-100N" manufactured by Imada Co., Ltd.
[0189] The following measurements were performed with respect to the tension applying conditions at each stage from 0 N to 100 N.
[0190] The phase difference value [nm] of the central part of the test piece under tension was measured using "KOBRA-WR" manufactured by Oji Instruments Co., Ltd. at a measurement wavelength of 589.5nm. The test piece was then removed from a pair of chucks and the thickness (d [mm]) of the phase difference measurement portion was measured. The cross-sectional area (S) [m 2 ](=15[mm]×d[mm]×10 -6 ), stress [Pa] (= tension [N] / S [m 2 ]), birefringence (= phase difference value [nm] × 10-6 / d[mm]). A graph was plotted with stress on the horizontal axis and birefringence on the vertical axis, and the slope of the straight line obtained by the least square method was determined as the photoelastic coefficient.
[0191] (Orientation Birefringence of Transparent Thermoplastic Resins)
[0192] A transparent thermoplastic resin is press-formed to obtain a resin plate with a thickness of 1.0 mm. A test piece with a width of 20 mm and a length of 50 mm is cut out from the central part of the obtained resin plate and placed in an autoclave with a heating chamber (manufactured by SHIMADZU). The distance between the chucks is set to 20 mm. After being kept at a temperature 10°C higher than the glass transition temperature (Tg) for 3 minutes, uniaxial stretching is performed at a speed of 3 mm / min. The stretching ratio is set to 100%. Under this condition, the distance between the chucks after stretching becomes 40 mm. The stretched test piece is removed from the above-mentioned device, cooled to 23°C, and the thickness (d) is measured. The Re value of the central part is measured using "KOBRA-WR" manufactured by Prince Instruments Co., Ltd. under the condition of a measuring wavelength of 589.5 nm. The obtained Re value is divided by the thickness (d) of the test piece to calculate the value of oriented birefringence.
[0193] (Average and standard deviation of Re values of liquid crystal display protective plates (resin plates before formation of cured coatings))
[0194] From the center of the LCD protective plate (resin plate before the cured film is formed), a test piece with a width of 21 cm and a length of 30 cm was cut in the direction of the extrusion molding direction (resin flow direction) as the long side direction. A standard lens (FUJINON HF12.5HA-1B) was installed on the "WPA-100-L" manufactured by Futonic Latex Co., Ltd. The height of the lens was adjusted so that the measurement range was 17 cm in width and 22 cm in length. Then, the Re value of the number of birefringent pixels of about 110,000 points was measured, and the average value and standard deviation were obtained.
[0195] (Thickness of each layer)
[0196] The thickness of each layer was measured using a "Universal Projector (V-12B)" manufactured by Nicon Instruments Co., Ltd.
[0197] (Rainbow pattern)
[0198] The LCD protection plate (resin plate before the cured coating is formed) is placed on the LCD so that the transmission axis of the polarizer on the viewing side of the LCD is perpendicular to the extrusion molding direction of the resin plate. A polarizing film is further placed on it, and the polarizing film is rotated at various angles. The appearance at the angle where the rainbow pattern caused by the fluctuation of the Re value is the strongest is visually evaluated according to the following three levels.
[0199] A (excellent): There is no rainbow pattern at all, and the visibility of the liquid crystal display is not reduced.
[0200] B (acceptable): There is a slight rainbow pattern, and the visibility of the liquid crystal display is slightly reduced.
[0201] C (poor): There are noticeable rainbow patterns, and the visibility of the liquid crystal display is greatly reduced.
[0202] (black screen)
[0203] The LCD protective plate (resin plate before the formation of the cured coating) was placed on the LCD so that the transmission axis of the polarizer on the viewing side of the LCD was perpendicular to the extrusion molding direction of the resin plate. A polarizing film was further placed on it and the polarizing film was rotated to various angles. The appearance of the LCD at the angle with the minimum intensity of the transmitted light was visually evaluated using the following three levels.
[0204] A (excellent): The transmitted light intensity is sufficiently high, and characters and the like displayed on the liquid crystal display can be clearly recognized.
[0205] B (acceptable): The transmitted light intensity is slightly low, and the visibility of characters and the like displayed on the liquid crystal display is slightly reduced.
[0206] C (poor): The intensity of transmitted light is almost zero, and the characters displayed on the liquid crystal display cannot be recognized.
[0207] (coloring)
[0208] The LCD protective plate (resin plate before the formation of the cured coating) was placed on the LCD so that the transmission axis of the polarizer on the viewing side of the LCD was perpendicular to the extrusion molding direction of the resin plate. A polarizing film was further placed on it, and the polarizing film was rotated to various angles, and the appearance of the LCD at the angle where the coloring was the largest was visually evaluated according to the following three levels.
[0209] A (excellent): There is no significant coloring, and the visibility of the liquid crystal display is not reduced.
[0210] B (acceptable): Coloring occurs, and visibility on a liquid crystal display is slightly reduced.
[0211] C (poor): There is significant coloring, and visibility on a liquid crystal display is reduced.
[0212] (Pencil hardness)
[0213] Using a tabletop mobile pencil scratch tester (model P) (manufactured by Toyo Seiki Co., Ltd.), the surface of the cured film side of the LCD protective plate including the cured film was scratched while pressing the lead of a pencil at an angle of 45° and a load of 750 g, and the presence or absence of scratches was visually confirmed. The hardness of the lead of the pencil increases in sequence, and the hardness of the lead that is one level softer than when the scratch occurs is adopted as the pencil hardness.
[0214] (Adhesion)
[0215] A 50 mm square test piece was cut out from the LCD protective plate including the cured film. A super UV tester (SUV-W161 manufactured by Iwasaki Electric Co., Ltd.) was used at a blackboard temperature of 83°C, a relative humidity of 50%, and an irradiation energy of 100 mW / cm 2 The test piece was irradiated with ultraviolet light (UV) for 100 hours under the conditions of . Then, the test piece was removed from the test machine and the cured film was cut into 1 mm thick sections using a checkerboard peel test fixture at a temperature of 23°C and a relative humidity of 50% based on JIS-K5600-5-6. 2 100 checkerboards were made. Adhesive tape No. 252 manufactured by Sekisui Chemical Co., Ltd. was pasted on it and pressed evenly on the whole with a scraper. Then, the adhesive tape was torn off in a 180° direction. The number of unpeeled and remaining pieces in the 100 checkerboards was calculated, and the adhesion was evaluated according to the following criteria.
[0216] A (excellent): 100,
[0217] B (pass): 90 to 99
[0218] C (bad): 89 or less.
[0219] (Appearance)
[0220] The liquid crystal display protective plate including the cured film was visually observed from the cured film side, and the appearance was evaluated based on the following criteria.
[0221] A (excellent): There are no wrinkles on the LCD protective plate and no cracks on the cured coating.
[0222] C (bad): There are wrinkles on the LCD protective plate and / or cracks on the cured coating.
[0223] [Material]
[0224] The materials used are described below.
[0225]
[0226] According to the method for producing copolymer (A) described in the section [Examples] of Japanese Patent Application Laid-Open No. 2003-231785, an MS resin (copolymer of methyl methacrylate (MMA) and styrene (St)) was polymerized. The mass ratio of MMA to St put into the autoclave was changed to produce the following three types of MS resins.
[0227] (MS-1) Tg = 116°C, content V of aromatic vinyl monomer units = 10% by mass,
[0228] (MS-2) Tg = 109°C, content of aromatic vinyl monomer unit V = 35% by mass,
[0229] (MS-3) Tg = 100°C, content V of aromatic vinyl monomer units = 90% by mass.
[0230] <Methacrylic resin>
[0231] (PMMA-1) A copolymer of 99.3% by mass of methyl methacrylate (MMA) and 0.7% by mass of methyl acrylate, manufactured by Kuraray Co., Ltd., Tg = 119°C, content of aromatic vinyl monomer units V = 0% by mass, syndiotacticity (rr) = 52%.
[0232] (PMMA-2) Homopolymer of methyl methacrylate (MMA), Tg=130°C, content V of aromatic vinyl monomer units=0 mass %, syndiotacticity (rr)=75%.
[0233] <Polycarbonate resin>
[0234] (PC-1) "SD Polycarboxylic Acid 300 Series" manufactured by Sumika Polycarbonate Co., Ltd., Tg = 150°C, content V of aromatic vinyl monomer units = 0 mass %.
[0235] [Examples 1 to 8]
[0236] (Manufacturing of the first liquid crystal display protection plate)
[0237] The resin for the substrate layer (transparent thermoplastic resin (B)) is melt-extruded using a 50mmφ single-screw extruder (manufactured by Toshiba Machine Co., Ltd.). The resin for the phase difference adjustment layer (transparent thermoplastic resin (A)) is melt-extruded using a 30mmφ single-screw extruder (manufactured by Toshiba Machine Co., Ltd.). These resins in a molten state are stacked via a multi-manifold die, and a three-layer thermoplastic resin stack having a substrate layer stacked on both sides of the phase difference adjustment layer is co-extruded from a T-die. The three-layer resin in a molten state is discharged from the T-die, sandwiched between the first cooling roller and the second cooling roller adjacent to each other, wound onto the second cooling roller, sandwiched between the second cooling roller and the third cooling roller, and wound onto the third cooling roller, thereby cooling. The resin plate obtained after cooling is withdrawn using a pair of withdrawal rollers. In this way, a first liquid crystal display protective plate (without a cured coating, reference figure: Figure 1 ).
[0238] (Manufacturing of the Second Liquid Crystal Display Protection Plate)
[0239] A test piece of 300 mm in length and 210 mm in width was cut out from the first liquid crystal display protection plate. The flow direction of the resin during extrusion molding was set to the length direction of the test piece. Using a thin sheet coater, a silicone-based curable resin composition (SilFORT PHC 587; manufactured by Momentive) was applied as a thermosetting coating material to the surface of one substrate layer of the above-mentioned test piece, and after drying at room temperature for 20 minutes, heat curing was performed under the conditions of the curing temperature and curing time described in Table 2. In this way, a second liquid crystal display protection plate including a cured coating was obtained.
[0240] For each example, the type and properties of the resin used, the thickness of the phase difference adjustment layer, the total thickness of the base material layer, V×T A The evaluation results of the first and second LCD protection plates are shown in Tables 1 and 2.
[0241] [Comparative Examples 1-1 to 1-3, 3, 4]
[0242] A first liquid crystal display protective plate (without a cured coating, reference figure: Figure 4 ). Figure 4 In the figure, reference numeral 101X denotes a liquid crystal display protective plate for comparison, reference numeral 116X denotes a resin plate for comparison, reference numeral 121 denotes a phase difference adjustment layer, and reference numeral 122 denotes a base material layer.
[0243] Using the obtained first liquid crystal display protection plate, a second liquid crystal display protection plate including a cured film was obtained by the same method as in Examples 1 to 8. In these examples, a cured film was formed on one phase difference adjustment layer.
[0244] In addition, in Comparative Examples 1-1 to 1-3, the production conditions of the extrusion-molded plates were common, but the formation conditions of the cured film were changed.
[0245] For each example, the type and properties of the resin used, the thickness of the phase difference adjustment layer, the total thickness of the base material layer, V×T A The formation conditions of the cured coating and the evaluation results of the first and second liquid crystal display protection plates are shown in Tables 1 and 2.
[0246] [Comparative Example 2]
[0247] A first liquid crystal display protective plate (without a cured coating, reference figure: Figure 5 ). Figure 5 In the figure, reference numeral 101Y denotes a liquid crystal display protective plate for comparison, reference numeral 116Y denotes a resin plate for comparison, reference numeral 121 denotes a phase difference adjustment layer, and reference numeral 122 denotes a base material layer.
[0248] Using the obtained first liquid crystal display protection plate, a second liquid crystal display protection plate including a cured film was obtained by the same method as in Examples 1 to 8. In this example, a cured film was formed on the phase difference adjustment layer.
[0249] For each example, the type and properties of the resin used, the thickness of the phase difference adjustment layer, the total thickness of the base material layer, V×T A The formation conditions of the cured coating and the evaluation results of the first and second liquid crystal display protection plates are shown in Tables 1 and 2.
[0250]
[0251]
[0252] [Summary of Results]
[0253] In Examples 1 to 8, a first LCD protective plate including a resin plate with substrate layers laminated on both sides of a phase difference adjustment layer and a second LCD protective plate with a cured coating formed on one substrate layer of the first LCD protective plate were manufactured. The phase difference adjustment layer is a layer containing a photoelastic coefficient (C A ) has an absolute value of 10.0×10 -12 / Pa or less, orientation birefringence (ΔnA ) has an absolute value of 10.0×10 -4 ~100.0×10 -4 The substrate layer is a layer of a transparent thermoplastic resin (A). B ) has an absolute value of 10.0×10 -12 / Pa or less, orientation birefringence (Δn B ) is less than 10.0×10 -4 The glass transition temperature of the phase difference adjustment layer is Tg A , and the glass transition temperature of the substrate layer is set to Tg B When Tg A <Tg B .
[0254] The first LCD protection plates (without cured coating) obtained in Examples 1 to 8 all had an average Re value of 50 to 330 nm within a width of 17 cm and a length of 22 cm, and a standard deviation of 15.0 nm or less within a width of 17 cm and a length of 22 cm.
[0255] In Examples 1 to 8, when the obtained first LCD protection plate was used and the LCD protection plate on the LCD screen was observed through a polarizing filter, rainbow lines, coloration, and black screen were effectively suppressed. In particular, V×T A In Examples 1 to 6 where the value of is 6.0 to 30.0, V×T A Compared with Examples 7 and 8 where the value of was outside the range of 6.0 to 30.0, good results were obtained.
[0256] The second liquid crystal display protection plates (with cured films) obtained in Examples 1 to 8 were all good in surface hardness, adhesion between the resin plate and the cured film, and appearance.
[0257] In Comparative Examples 1-1 to 1-3 and 2 to 4, a first LCD protective plate including a resin plate having a phase difference adjustment layer laminated on both sides or one side of a substrate layer and a second LCD protective plate having a cured coating formed on the phase difference adjustment layer of the first LCD protective plate were manufactured.
[0258] In Comparative Example 1-1, a cured film was formed under the same curing conditions as Examples 1 to 8. In this example, the curing temperature was higher than Tg of the phase difference adjusting layer, and the film material was cured while the phase difference adjusting layer was thermally expanded, so cracks occurred in the cured film.
[0259] In Comparative Example 1-2, the curing temperature was lowered to a temperature lower than the Tg of the phase difference adjusting layer. Although the cured film did not crack, the crosslinking reaction of the film material did not proceed sufficiently, and the surface hardness of the cured film and the adhesion between the resin plate and the cured film decreased.
[0260] In Comparative Example 1-3, the curing temperature was lowered to a temperature lower than Tg of the phase difference adjustment layer to extend the curing time. Although the defects of Comparative Examples 1-1 and 1-2 could be improved, the curing time was long and the productivity was poor.
[0261] In Comparative Example 2, similarly to Comparative Example 1-1, the curing temperature was higher than Tg of the phase difference adjusting layer, and the coating material was cured while the phase difference adjusting layer was thermally expanded, so cracks occurred in the cured coating.
[0262] In Comparative Examples 3 and 4, the photoelastic coefficient (C B ) and orientation birefringence (Δn B ) is a polycarbonate resin outside the scope of the present invention as the resin of the substrate layer. In Comparative Example 4, an oriented birefringence (Δn A ) is a methacrylic resin outside the provisions of the present invention as the resin of the phase difference adjustment layer. The standard deviation of the Re value of the LCD protective plate obtained in these comparative examples is large (the fluctuation of the Re value is large), and rainbow patterns are generated when the LCD protective plate located on the LCD screen is observed through a polarizing filter. In Comparative Example 3, as in Comparative Example 1-1, the curing temperature is higher than the Tg of the phase difference adjustment layer, and the coating material is cured under the state of thermal expansion of the phase difference adjustment layer, so cracks are generated in the cured coating.
[0263] The present invention is not limited to the above-described embodiments and examples, and design changes may be appropriately made without departing from the gist of the present invention.
[0264] This application claims the priority based on Japanese application No. 2019-223420 filed on December 11, 2019, and all the contents disclosed therein are incorporated into this specification.
[0265] Explanation of symbols
[0266] 1, 2 LCD display protection plate
[0267] 11 T-die head
[0268] 12~14 cooling rollers
[0269] 15 Take-off Roller
[0270] 16 Resin board
[0271] 21 Phase difference adjustment layer
[0272] 22 Base material layer
[0273] 31 Curing film
Claims
1. A liquid crystal display protection plate, characterized in that: The resin plate includes a base material layer laminated on both sides of the phase difference adjustment layer. The phase difference adjustment layer has a photoelastic coefficient C A The absolute value of -12 / Pa or less and the orientation birefringence Δn A The absolute value of -4 ~100.0×10 -4 The transparent thermoplastic resin A, the oriented birefringence Δn A The retardation value in the plane of the central part of a test piece of 20 mm in width, 50 mm in length and 1 mm in thickness is obtained by uniaxially stretching a test piece at a temperature 10°C higher than the glass transition temperature at a rate of 3 mm / min and a stretching ratio of 100%. The substrate layer has a photoelastic coefficient C B The absolute value of -12 / Pa or less and the orientation birefringence Δn B The absolute value is less than 10.0×10 -4 The transparent thermoplastic resin B, the oriented birefringence Δn B The retardation value in the plane of the central part of a test piece of 20 mm in width, 50 mm in length and 1 mm in thickness is obtained by uniaxially stretching a test piece at a temperature 10°C higher than the glass transition temperature at a rate of 3 mm / min and a stretching ratio of 100%. Oriented birefringence Δn of transparent thermoplastic resin A A and the oriented birefringence Δn of the transparent thermoplastic resin B B Both are negative, The glass transition temperature of the phase difference adjustment layer is set to Tg A , and the glass transition temperature of the substrate layer is set to Tg B When Tg A <Tg B , The thickness of the phase difference adjustment layer is set to T A , and the total thickness of the substrate layer is set as T B When T B / T A ≥2.0, The resin plate has an in-plane retardation value of 50 to 330 nm.
2. The liquid crystal display protection plate according to claim 1, characterized in that: The standard deviation of the in-plane retardation value of the resin plate within the range of 17 cm in width and 22 cm in length was 15.0 nm or less.
3. The liquid crystal display protection plate according to claim 1 or 2, characterized in that: The glass transition temperature Tg of the substrate layer B Above 115°C.
4. The liquid crystal display protection plate according to claim 1 or 2, characterized in that: The transparent thermoplastic resin A contains an aromatic vinyl monomer unit. The content of the aromatic vinyl monomer unit in the transparent thermoplastic resin A is denoted as V, and the thickness of the phase difference adjustment layer is denoted as T. A When , the following formula (1) is satisfied: 6.0≤V×T A ≤30.0…(1), Wherein, V is expressed in mass%, T A The unit is mm.
5. The liquid crystal display protection plate according to claim 1 or 2, characterized in that: Furthermore, the resin plate has a cured film on at least one surface thereof.
6. The liquid crystal display protection plate according to claim 1 or 2, characterized in that: The resin plate is an extrusion-molded plate.