A method for predicting the UV aging life of polymer-based composite materials

Through the accelerated aging experiment and kinetic curve analysis of fluorescent ultraviolet lamps, the ultraviolet aging life prediction method for polymer-based composite materials was established, which solved the problem of performance deterioration of polymer-based fiber composites under ultraviolet light, and achieved its life and Effective assessment of reliability.

CN114813527BActive Publication Date: 2024-11-15NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210246074.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-14
Publication Date
2024-11-15
Estimated Expiration
2042-03-14

AI Technical Summary

Technical Problem

The performance of polymer-based fiber composites deteriorates under ultraviolet light, resulting in a reduction in adhesion in service environments, making it difficult to effectively predict their lifespan and reliability. The prior art lacks effective aging lifespan prediction methods.

Method used

Using fluorescent ultraviolet lamp artificial accelerated aging experiment, combined with mechanical performance test and kinetic curve empirical formula, life prediction equation is established through least squares method and the Arenius formula, the equivalent relationship between artificial accelerated aging and natural aging is established, and the ultraviolet is calculated. Photooxygen aging lifespan.

Benefits of technology

A method for predicting ultraviolet aging life of polymer-based composites is provided, which can accurately predict the strength retention rate and life under different aging conditions, providing a basis for the reliability evaluation of equipment in natural environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114813527B_ABST
    Figure CN114813527B_ABST
Patent Text Reader

Abstract

The present invention provides a method for predicting the ultraviolet aging life of polymer-based composite materials, comprising: step 1, performing an artificial accelerated aging experiment using a fluorescent ultraviolet lamp on a polymer-based fiber composite material; step 2, performing a mechanical property test on the polymer-based composite material before and after aging, and calculating the strength retention rate at different aging times; step 3, obtaining the reaction rate constant K at different experimental temperatures using the least squares method; step 4, extrapolating the reaction rate constant K at room temperature using the least squares method; step 5, establishing an equivalent relationship under different aging conditions through the ratio of the single-day cumulative radiation energy, and obtaining the ultraviolet aging life under natural conditions. The present invention provides technical support for the prediction of the ultraviolet aging life of polymer-based fiber composite materials, making it possible to predict the service life under any tensile / compressive strength retention rate and any temperature ultraviolet aging condition, and providing a basis for the service reliability evaluation of polymer-based composite materials under natural conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of dynamic risk assessment of mobile pressure-bearing equipment, and in particular relates to a method for predicting the ultraviolet aging life of a polymer-based composite material. Background Art

[0002] Polymer-based fiber composite materials are a series of high-performance composite materials made of advanced composite material molding and processing technology with fiber as reinforcement and resin and other polymers as matrix. They have high specific strength and specific stiffness, corrosion resistance, fatigue resistance and other characteristics. Due to the above characteristics, they are widely used in aerospace, rail transportation, pressure vessels and other fields. In recent years, as the country attaches great importance to the development of hydrogen energy, lightweight and high-strength carbon fiber composite materials have become the preferred material for the winding layer of hydrogen storage cylinders. The carbon fiber composite winding layer used in type III and IV gas cylinders can provide a higher load-bearing capacity and meet the unit mass hydrogen storage density requirements. Due to the unique structural characteristics of polymer-based composite materials, their load-bearing capacity is affected by the degree of bonding between the fiber and the polymer. In complex service environments, ultraviolet rays, humidity, heat, high temperature, etc. will make the bonding between the polymer and the fiber deteriorate.

[0003] Hydrogen storage cylinders are inevitably exposed to sunlight during transportation, and the ultraviolet rays in sunlight can deteriorate the performance of carbon fiber composites. Therefore, artificial indoor accelerated aging experiments were carried out to explore the attenuation law of mechanical properties of polymer-based fiber composites in the service environment. A life prediction method for polymer-based fiber composites under ultraviolet aging conditions was established, which is of great significance for regular inspection of equipment service and reliability evaluation of service. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for predicting the life of polymer-based composite materials under ultraviolet aging, and to establish an equivalent relationship between artificial accelerated aging and natural aging, so as to provide a basis for evaluating the service reliability of polymer-based composite materials under natural environment. The specific steps are as follows:

[0005] Step 1, performing an artificial accelerated aging experiment using a fluorescent ultraviolet lamp on the polymer-based composite material;

[0006] Step 2: Test the mechanical properties of the polymer-based composite material before and after aging. In this example, the tensile and compressive mechanical properties of the unidirectional ply of the carbon fiber / epoxy resin composite laminate are selected as the test objects, and the strength retention rate under different aging times is calculated;

[0007] Step 3, based on the empirical formula of the kinetic curve, the reaction rate constant K at different experimental temperatures is obtained using the least squares method;

[0008] Step 4: Based on the Arrhenius formula, the reaction rate constant K is combined with the empirical formula of the kinetic curve to obtain the life prediction equation at any temperature;

[0009] Step 5: Due to the dose difference between artificial accelerated aging and natural atmospheric aging, the equivalent relationship under different aging conditions is established through the daily cumulative radiation energy ratio, and finally the ultraviolet oxygen aging life under natural conditions is obtained.

[0010] Step 1 includes:

[0011] Step 1.1, design the size of the polymer-based composite material specimen. The tensile specimen size refers to ASTM D3039 and cuts the tensile specimen into 250×15×1mm. In order to avoid the specimen slipping during the 0° tensile process, glass fiber reinforcement sheets are attached to both ends of the specimen, and the specimen is bonded with Kafuter K-801 modified acrylic ester AB adhesive. After bonding, it is dried in an oven at 70℃ for 16 hours. Referring to ASTM D6641, the compression specimen is cut into 140×12×2mm, and glass fiber reinforcement sheets are also used to avoid slipping;

[0012] Step 1.2, set the UV aging experiment parameters: UV intensity 1W / (m2·nm), UV irradiation temperature (50℃, 60℃, 70℃), UV irradiation cycle 24h, sampling cycle number (10, 20, 30, 40, 60);

[0013] Step 2 includes:

[0014] Step 2.1, perform a tensile compression test, with a tensile rate of 2 mm / min and a compression rate of 1 mm / min, using a displacement-controlled loading mode, testing X1 (generally 5) specimens in each group, and taking the average value of the test results as the tensile and compressive strengths under different aging cycles;

[0015] Step 2.2, calculate the tensile and compressive strength retention rate f(p) at different aging times:

[0016] f(p)=p / p0, (1)

[0017] p is the intensity value after aging, and p0 is the intensity value before aging.

[0018] Step 3 includes:

[0019] Step 3.1: According to the first-order kinetic behavior between the UV aging strength retention rate of polymer-based composite materials and the aging time, the residual mechanical properties at different aging times are characterized according to the empirical formula of the kinetic curve, as shown in the following formula:

[0020] f(p)=Aexp(-Kt) (2)

[0021] Where A is the unknown parameter, t is the aging time, and K represents the reaction rate constant at room temperature extrapolated from the Arrhenius formula. Taking the logarithm of the above formula, formula (2) is transformed into the following formula:

[0022] ln(f(p))=lnA-Kt, (3)

[0023] Let the intermediate parameter x = t, the intermediate parameter y = ln(f(p)), the coefficient a1 = lnA, the coefficient b1 = K, and transform formula (3) into a linear form:

[0024] y=a1+b1x; (4)

[0025] Step 3.2: Use the least squares method to calculate the coefficients a1 and b1 as shown below:

[0026]

[0027]

[0028] n is the number of experimental test groups.

[0029] Step 4 includes:

[0030] Step 4.1, according to the Arrhenius formula, the temperature and reaction rate constant K are fitted by least squares to obtain the Arrhenius model coefficient. Similarly, the reaction rate constant K at multiple aging temperatures is obtained. Then, the reaction rate constant K at room temperature is extrapolated according to the Arrhenius formula. K and T obey the Arrhenius equation, as shown in the following formula:

[0031]

[0032] Where T is absolute temperature, Kelvin (K). Z is the Arrhenius constant, E is the activation energy, and R is the molar gas constant, which is 8.31344 J / (mol·K). Taking the logarithm of formula (7), we get:

[0033]

[0034] Let coefficient a2 = lnZ, coefficient b2 = -E / R, intermediate parameter X = 1 / T, intermediate parameter Y = ln(K), formula (8) becomes the following linear form:

[0035] Y=a2+b2X; (9)

[0036] Step 4.2: Calculate coefficients a2 and b2 using the least squares method:

[0037]

[0038]

[0039] Step 5 includes:

[0040] Step 5.1: There are differences in radiation doses under artificial accelerated aging and atmospheric natural aging conditions. The equivalent relationship under different aging conditions can be established through the daily cumulative radiation energy ratio β, as shown in the following formula:

[0041] H=3.6It,

[0042] Q = HSN,

[0043]

[0044] In the formula, Q represents the cumulative radiation energy of ultraviolet aging, in kJ; Q0 represents the radiation energy of natural light, in kJ; H represents the radiation energy, in kJ / m 2 ; I represents the irradiance, the unit is W / m 2 ; t represents the aging time; S represents the sample area; N represents the number of lamp tubes, and β represents the daily irradiation energy ratio.

[0045] Step 5.2: According to step 3, the life prediction equation at any temperature is as follows:

[0046]

[0047] in is the mean value of the parameter a1 of the kinetic curve formula at different aging temperatures.

[0048] Finally, the life span t0 of UV oxygen aging under natural conditions is obtained:

[0049] t0=βt.

[0050] Beneficial effects: The present invention establishes a method for predicting the life of polymer-based fiber composite materials under ultraviolet aging. The method is based on the kinetic curve straight line method and provides an equivalent relationship between artificial accelerated aging and natural aging. This method enables the prediction of the service life under any tensile / compressive strength retention rate and any temperature ultraviolet aging, providing a basis for the service reliability evaluation of polymer-based composite materials under natural environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0052] Figure 1a It is a schematic diagram of the fitting curve of the kinetic empirical formula at different aging temperatures of the present invention.

[0053] Figure 1b It is a schematic diagram of the fitting curve of the kinetic empirical formula at different aging temperatures of the present invention.

[0054] Figure 2 It is the lnK bar graph of the present invention at different temperatures. DETAILED DESCRIPTION

[0055] The present invention provides a method for predicting the ultraviolet aging life of a polymer-based composite material, comprising:

[0056] Step 1, performing an artificial accelerated aging experiment using a fluorescent ultraviolet lamp on the polymer-based composite material;

[0057] Step 2: Test the mechanical properties of the polymer-based composite material before and after aging. In this example, the tensile and compressive mechanical properties of the unidirectional ply of the carbon fiber / epoxy resin composite laminate are selected as the test objects, and the strength retention rate under different aging times is calculated;

[0058] Step 3, based on the empirical formula of the kinetic curve, the reaction rate constant K at different experimental temperatures is obtained using the least squares method;

[0059] Step 4: Based on the Arrhenius formula, the reaction rate constant K is combined with the empirical formula of the kinetic curve to obtain the life prediction equation at any temperature;

[0060] Step 5: Due to the dose difference between artificial accelerated aging and natural atmospheric aging, the equivalent relationship under different aging conditions is established through the daily cumulative radiation energy ratio, and finally the ultraviolet oxygen aging life under natural conditions is obtained.

[0061] Step 1 includes:

[0062] Step 1.1, design the size of the polymer-based composite material specimen. The tensile specimen size refers to ASTM D3039 and cuts the tensile specimen into 250×15×1mm. In order to avoid the specimen slipping during the 0° tensile process, glass fiber reinforcement sheets are attached to both ends of the specimen, and the specimen is bonded with Kafuter K-801 modified acrylic ester AB adhesive. After bonding, it is dried in an oven at 70℃ for 16 hours. Referring to ASTM D6641, the compression specimen is cut into 140×12×2mm, and glass fiber reinforcement sheets are also used to avoid slipping;

[0063] Step 1.2, set the UV aging experiment parameters: UV intensity 1W / (m2·nm), UV irradiation temperature (50℃, 60℃, 70℃), UV irradiation cycle 24h, sampling cycle number (10, 20, 30, 40, 60);

[0064] Step 2 includes:

[0065] Step 2.1, perform a tensile compression test, with a tensile rate of 2 mm / min and a compression rate of 1 mm / min, using a displacement-controlled loading mode, testing X1 (generally 5) specimens in each group, and taking the average value of the test results as the tensile and compressive strengths under different aging cycles;

[0066] Step 2.2, calculate the tensile and compressive strength retention rate f(p) at different aging times:

[0067] f(p)=p / p0, (1)

[0068] p is the intensity value after aging, and p0 is the intensity value before aging.

[0069] Step 3 includes:

[0070] Step 3.1: According to the first-order kinetic behavior between the UV aging strength retention rate of polymer-based composite materials and the aging time, the residual mechanical properties at different aging times are characterized according to the empirical formula of the kinetic curve, as shown in the following formula:

[0071] f(p)=Aexp(-Kt) (2)

[0072] Where A is the unknown parameter, t is the aging time, and K represents the reaction rate constant of the Arrhenius formula at room temperature. Taking the logarithm of the above formula, formula (2) is transformed into the following formula:

[0073] ln(f(p))=lnA-Kt, (3)

[0074] Let the intermediate parameter x = t, the intermediate parameter y = ln(f(p)), the coefficient a1 = lnA, the coefficient b1 = K, and transform formula (3) into a linear form:

[0075] y=a1+b1x; (4)

[0076] Step 3.2: Use the least squares method to calculate the coefficients a1 and b1 as shown below:

[0077]

[0078]

[0079] n is the number of experimental test groups.

[0080] Step 4 includes:

[0081] Step 4.1, according to the Arrhenius formula, the temperature and reaction rate constant K are fitted by least squares to obtain the Arrhenius model coefficient. Similarly, the reaction rate constant K at multiple aging temperatures is obtained. Then, the reaction rate constant K at room temperature is extrapolated according to the Arrhenius formula. K and T obey the Arrhenius equation, as shown in the following formula:

[0082]

[0083] Where T is absolute temperature, Kelvin (K). Z is the Arrhenius constant, E is the activation energy, and R is the molar gas constant, which is 8.31344 J / (mol·K). Taking the logarithm of formula (7), we get:

[0084]

[0085] Let coefficient a2 = lnZ, coefficient b2 = -E / R, intermediate parameter X = 1 / T, intermediate parameter Y = ln(K), formula (8) becomes the following linear form:

[0086] Y=a2+b2X; (9)

[0087] Step 4.2: Calculate coefficients a2 and b2 using the least squares method:

[0088]

[0089]

[0090] Step 5 includes:

[0091] Step 5.1: There are differences in radiation doses under artificial accelerated aging and atmospheric natural aging conditions. The equivalent relationship under different aging conditions can be established through the daily cumulative radiation energy ratio β, as shown in the following formula:

[0092] H=3.6It,

[0093] Q = HSN,

[0094]

[0095] In the formula, Q represents the cumulative radiation energy of ultraviolet aging, in kJ; Q0 represents the radiation energy of natural light, in kJ; H represents the radiation energy, in kJ / m 2 ; I represents the irradiance, the unit is W / m 2 ; t represents the aging time; S represents the sample area; N represents the number of lamp tubes, and β represents the daily irradiation energy ratio.

[0096] Step 5.2: According to step 3, the life prediction equation at any temperature is as follows:

[0097]

[0098] in is the mean value of the parameter a1 of the kinetic curve formula at different aging temperatures.

[0099] Finally, the life span t0 of UV oxygen aging under natural conditions is obtained:

[0100] t0=βt.

[0101] Example 1

[0102] The present invention provides a method for predicting the ultraviolet aging life of a polymer-based composite material, comprising:

[0103] Step 1, performing an artificial accelerated aging experiment using a fluorescent ultraviolet lamp on the polymer-based composite material;

[0104] Step 2: Test the mechanical properties of the polymer-based composite material before and after aging. In this example, the uniaxial tensile and compressive mechanical properties of the carbon fiber / epoxy composite material are selected as the characterization quantities, and the tensile / compressive strength retention rate f(p) at different aging times is calculated as shown in Tables 1 and 2:

[0105] Table 1

[0106]

[0107]

[0108] Table 2

[0109]

[0110] Step 3: Based on the empirical formula of the kinetic curve, the reaction rate constant K at different experimental temperatures was obtained using the least squares method. First, lnf(p) was calculated, and lnf(p) and the aging time t were fitted by the least squares method. It was found that the two had a good linear relationship, such as Figure 1a , Figure 1b As shown, according to the fitting results, the slope b1, intercept a1 and correlation coefficient R are obtained. 2 , and further obtained the reaction rate constant K and the unknown parameter A. The fitting parameters are shown in Table 3:

[0111] Table 3

[0112]

[0113] Step 4 Figure 2The relationship curve between lnK and 1 / T under tension / compression conditions is shown in Table 4. Based on the Arrhenius formula, lnK and 1 / T are fitted by least squares to obtain the fitting parameters of the Arrhenius formula. In this way, the reaction rate constant K at room temperature 20°C can be calculated. The calculation results are shown in Table 4:

[0114] Table 4

[0115]

[0116] Step 5: The amount of ultraviolet radiation used in the laboratory is much greater than the sunlight in the natural environment. The TN-340 ultraviolet radiation monitor continuously monitors the ultraviolet radiation intensity of natural light for ten months, and the cumulative radiation energy for 10 months is 405.1 kJ / m 2 The average daily radiation exposure is 1.35 kJ / m 2 The UV accelerated aging test box in this paper has four UVA-340 fluorescent UV lamps built into one side, with an irradiation intensity of 1W / (m2·nm), and the daily irradiation is 18.8Kj / m 2 , the cumulative radiation energy ratio β is calculated to be 13.93.

[0117] Example 2

[0118] This example is a prediction of the ultraviolet aging life of carbon fiber / epoxy resin composite materials, selecting room temperature 20°C as the prediction temperature, and strength retention rates of 70%, 60%, and 50%. According to the correlation coefficient obtained by the life prediction model obtained above, the aging life under different strength retention rates is calculated as shown in Table 5:

[0119] Table 5

[0120]

[0121] As shown in Table 5, at a strength retention rate of 70%, the life prediction based on tension is 9.06 years and the life prediction based on compression is 4.92 years. The tensile bearing capacity of carbon fiber / epoxy resin-based composites is stronger under UV aging.

[0122] The present invention provides a method for predicting the life of polymer-based composite materials by ultraviolet aging. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A method for predicting the ultraviolet aging life of a polymer-based composite material, characterized in that: The following steps are included Step 1, performing an artificial accelerated aging experiment using a fluorescent ultraviolet lamp on the polymer-based composite material; Step 2, testing the mechanical properties of the polymer-based composite material before and after aging, and calculating the strength retention rate at different aging times; Step 3, based on the empirical formula of the kinetic curve, the reaction rate constant K at different experimental temperatures is obtained using the least squares method; Step 4: Based on the Arrhenius formula, the reaction rate constant K is combined with the empirical formula of the kinetic curve to obtain the life prediction equation at any temperature; Step 5, establish the equivalent relationship under different aging conditions through the daily cumulative radiation energy ratio, and finally obtain the ultraviolet oxygen aging life under natural conditions; Step 2 includes: Step 2.1, conduct tension and compression tests, test X1 specimens in each group, and take the average value of the test results as the static strength under different aging cycles; Step 2.2, calculate the tensile and compressive strength retention rate f(p) at different aging times: f(p)=p / p0, (1) p is the strength value after aging, and p0 is the strength value before aging; Step 3 includes: Step 3.1: Characterize the performance residual at different aging times according to the empirical formula of the kinetic curve, as shown in the following formula: f(p)=A exp(-Kt) (2) Where A is the unknown parameter, t is the aging time, and K represents the reaction rate constant of the Arrhenius formula at room temperature. Taking the logarithm of the above formula, formula (2) is transformed into the following formula: ln(f(p))=ln A-Kt, (3) Let the intermediate parameter x = t, the intermediate parameter y = ln(f(p)), the coefficient a1 = lnA, the coefficient b1 = K, and transform formula (3) into a linear form: y=a1+b1x; (4) Step 3.2, use the least squares method to calculate coefficients a1, b1: n is the number of experimental test groups; Step 4 includes: Step 4.1, K and T obey the Arrhenius equation, as shown below: Where T is the absolute temperature, Z is the Arrhenius constant, E is the activation energy, and R is the molar gas constant. Taking the logarithm of formula (7), we get: Let coefficient a2 = lnZ, coefficient b2 = -E / R, intermediate parameter X = 1 / T, intermediate parameter Y = ln(K), formula (8) becomes the following linear form: Y=a2+b2X; (9) Step 4.2: Calculate coefficients a2 and b2 using the least squares method: n is the number of experimental test groups.

2. The method according to claim 1, characterized in that Step 1 includes: Step 1.1, design the size of the polymer matrix composite material sample; Step 1.2: Set the UV aging experiment parameters and set multi-cycle and multi-temperature UV aging conditions.

3. The method according to claim 1, characterized in that Step 5 includes: Step 5.1: Establish the equivalent relationship between laboratory accelerated aging and natural aging conditions through the daily cumulative radiation energy ratio β, as shown in the following formula: H=3.6It, Q = HSN, In the formula, Q represents the cumulative radiation energy of ultraviolet aging; Q0 represents the radiation energy of natural light; H represents the radiation energy; I represents the radiation intensity; S represents the sample area; N represents the number of lamps, and β represents the radiation energy ratio of a single day; Step 5.2: The life prediction equation at any temperature is as follows: in is the mean value of the parameter a1 of the kinetic curve formula at different aging temperatures; Finally, the life span t0 of UV-oxidation aging under natural conditions is obtained: t0=βt.