A method for improving the efficiency of heterojunction batteries
By treating the surface of amorphous silicon wafers with a planar ICP plasma source, the problems of pollution, oxidation and water vapor adsorption in heterojunction batteries are solved, the battery efficiency is improved, and water vapor desorption is achieved without affecting the production cycle, which is suitable for high output. Craftsmanship.
Patent Information
- Application Number
- CN202210466722.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-04-29
AI Technical Summary
In the existing heterojunction cell process, the pollution and oxidation of the amorphous silicon surface and the water vapor adsorption problem on the tray surface lead to efficiency losses, and there is a contradiction between increasing the water vapor desorption speed and the production cycle of the existing equipment, which cannot be fundamentally solved. these questions.
A planar ICP plasma source is used to set up a coil on the vacuum side, generate plasma through radio frequency magnetic flux, and perform surface treatment on the amorphous silicon wafer to remove contamination and oxidation layers, and perform surface treatment before TCO film preparation, combined with the TCO film deposition process , to achieve water vapor desorption and avoid increasing the number of machines and affecting the production rhythm.
It effectively removes pollutants and oxide layers on the surface of the amorphous silicon film layer, quickly desorbs water vapor on the surface of the tray, and improves battery efficiency. It is suitable for large-area processing and adapts to high output requirements. It has a simple structure, low maintenance costs, and does not affect the uptime of the equipment.
Smart Images

Figure CN114823990B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of heterojunction batteries, and in particular to a method for improving the efficiency of heterojunction batteries. Background Art
[0002] The existing process flow of heterojunction batteries is as follows: Figure 1 The main steps include texturing and cleaning, amorphous silicon deposition, TCO film preparation and gate line preparation.
[0003] The main problem with the existing heterojunction battery preparation process is that after the amorphous silicon is deposited and before the TCO film is deposited, although in order to protect the amorphous silicon surface from being affected, most manufacturers have placed the products (batteries after the amorphous silicon is deposited) in a nitrogen cabinet for storage, but there are still various situations such as transportation and staying in the atmospheric environment in the middle, and it is impossible to completely avoid the contamination and oxidation of the amorphous silicon surface, which ultimately affects the bulk performance of the amorphous silicon film layer and its contact performance with the TCO film, resulting in efficiency loss. The location where contamination and oxidation occur is as follows: Figure 2 shown.
[0004] In addition, after the ITO film is deposited on the tray used to transport silicon wafers in the TCO thin film deposition process, due to the characteristic of the ITO film that it easily absorbs water vapor, the surface of the tray will quickly physically absorb water vapor and reach saturation during the transmission and waiting process of the carrier in the atmosphere. After the tray is loaded with silicon wafers, it enters the vacuum chamber. Due to the change in the air pressure, the adsorption rate on the surface decreases, and the entire tray is reflected as water vapor desorption in the vacuum chamber. The desorption of water vapor on the tray directly affects the water vapor content of the entire film-forming atmosphere. In general, the TCO thin film deposition atmosphere has stricter requirements on water vapor. A higher water vapor content will affect the electrical and optical properties of the TCO film and ultimately affect the efficiency of the battery. The changing trend of battery efficiency under different water vapor contents on the production line is as follows. Figure 3 shown.
[0005] At present, equipment and battery manufacturers on the market still use nitrogen cabinets to reduce pollution. The water vapor on the surface of the tray is desorbed as quickly as possible by heating in the vacuum chamber. However, the heating time of the tray in the vacuum chamber is inconsistent with the production cycle required by the equipment (the high output of the equipment requires a short production cycle, and a longer heating time is beneficial to the rapid desorption of water vapor). This does not fundamentally solve the problem.
[0006] Therefore, it is necessary to study a new heterojunction battery efficiency improvement method to address the shortcomings of existing technologies in order to solve or alleviate one or more of the above problems. Summary of the invention
[0007] In view of this, the present invention provides a method for improving the efficiency of heterojunction batteries, which can simultaneously solve the problems of pollution, oxidation and water vapor adsorption on the surface of silicon wafers, thereby improving the battery conversion efficiency without affecting the working rhythm of PVD equipment.
[0008] The present invention provides a method for improving the efficiency of a heterojunction battery. The method comprises the steps of texturing and cleaning, amorphous silicon deposition, TCO film preparation and gate line preparation, and amorphous silicon surface treatment is added before the TCO film preparation step to improve the pollution and oxidation problems on the surface of amorphous silicon wafers during the preparation of heterojunction batteries and remove water vapor adsorbed on the surface of a tray.
[0009] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the amorphous silicon surface treatment is implemented by using a planar ICP plasma source;
[0010] Specifically, a plurality of coils are arranged at the top of the vacuum side; the coils are connected to an external RF matcher to generate a radio frequency magnetic flux, and the radio frequency electric field induced by the radio frequency magnetic flux along the axial direction accelerates the electrons therein, thereby generating plasma;
[0011] The amorphous silicon wafer to be surface treated is located below the coil and passes through the plasma region in sequence at a preset speed.
[0012] According to the aspects and any possible implementations described above, an implementation is further provided, wherein the width and length of the coil are set to match the amorphous silicon wafer to be processed, so that large-area amorphous silicon wafer surface processing can be achieved.
[0013] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the planar ICP plasma source is disposed at a reserved cathode position of a PVD device.
[0014] According to the above aspects and any possible implementation, an implementation is further provided, under the condition of a travel speed of 1 m / min, the parameters of the amorphous silicon surface treatment include: the number of coil turns is 1-2 turns, the RF power of the planar ICP plasma source is 400W-1000W, the distance between the coil and the amorphous silicon wafer to be processed is more than 100mm, and the vacuum degree is less than 0.8 Pa. The travel speed can be in the range of 1-4 m / min, and the other parameters corresponding to different travel speeds will have certain changes.
[0015] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the number of turns of the coil is 2.
[0016] According to the aspects and any possible implementations described above, an implementation is further provided in which the RF power is 500W.
[0017] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the distance between the coil and the amorphous silicon wafer to be processed is 100 mm-200 mm.
[0018] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the vacuum degree is 0.5 Pa-0.8 Pa. The above vacuum degree is the environmental pressure obtained after the ultimate vacuum is drawn and then the discharge atmosphere is distributed.
[0019] Compared with the prior art, the present invention has the following advantages or beneficial effects: the ICP plasma source of the present invention can generate high-density low-energy plasma, and has a wide range of working pressure, perfectly adapts to the heterojunction battery process, and removes pollutants and oxide layers on the surface of the amorphous silicon film layer without damaging the original amorphous silicon film layer;
[0020] Another technical solution in the above technical solution has the following advantages or beneficial effects: the present invention uses the characteristics of the ICP ion source with controllable energy and large process window to desorb the water vapor adsorbed by the carrier in the atmosphere, thereby achieving a stable process without losing the cycle time;
[0021] Another technical solution in the above technical solution has the following advantages or beneficial effects: the surface treatment is integrated with the TCO thin film deposition process, and the surface treatment can be completed without adding equipment and affecting the PVD equipment beat;
[0022] Another technical solution in the above technical solution has the following advantages or beneficial effects: the ICP plasma source generator of this structure can adjust the plasma coverage width and length according to the equipment requirements, so as to process large-area samples and is suitable for mass production introduction;
[0023] Another technical solution among the above technical solutions has the following advantages or beneficial effects: the ICP plasma source generator of the present invention has a simple structure and layout, low maintenance cost, and a long service life, and will not affect the uptime of the equipment (ie: equipment availability, equipment production time / total time*100%). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 It is a flow chart of the preparation of heterojunction batteries in the prior art;
[0026] Figure 2It is an indicator of the locations where existing heterojunction batteries are prone to contamination and oxidation;
[0027] Figure 3 This is the curve of the battery efficiency change under different water vapor contents in the existing heterojunction battery production line;
[0028] Figure 4 is a flow chart of the preparation of a heterojunction battery provided by one embodiment of the present invention;
[0029] Figure 5 It is a schematic diagram of the structure of a plasma source generator provided by one embodiment of the present invention;
[0030] Figure 6 is a layout diagram of a plasma source generator provided by one embodiment of the present invention;
[0031] Figure 7 is a curve diagram showing the relationship between the number of coil turns and the FF filling factor provided by one embodiment of the present invention;
[0032] Figure 8 is a curve diagram showing the relationship between FF fill factor and RF power provided by one embodiment of the present invention;
[0033] Fig. 9 is a curve diagram showing the relationship between the FF filling factor and the distance between the coil and the substrate provided by one embodiment of the present invention;
[0034] Fig.10 is a curve diagram showing the relationship between the FF filling factor and the film forming pressure provided by one embodiment of the present invention;
[0035] Fig.11 is a curve diagram showing the relationship between the water vapor partial pressure difference between the front and rear chambers and the number of coil turns provided by an embodiment of the present invention;
[0036] Fig.12 is a graph showing the relationship between the water vapor partial pressure difference between the front and rear chambers and the RF power provided by an embodiment of the present invention;
[0037] Fig.13 is a graph showing the relationship between the water vapor partial pressure difference between the front and rear chambers and the distance between the coil and the substrate provided by an embodiment of the present invention;
[0038] Fig.14 It is a curve diagram showing the relationship between the water vapor partial pressure difference between the front and rear chambers and the film forming pressure provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0040] It should be clear that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms of "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings. "First", "second" and "third" are only reference descriptions made to distinguish. It should also be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the objects associated before and after are in an "or" relationship.
[0042] In view of the shortcomings of the prior art, the present invention provides a method for improving the efficiency of a heterojunction battery. The preparation process of the heterojunction battery is as follows: Figure 4 As shown, based on the original processes of texturing and cleaning, amorphous silicon deposition, TCO film preparation and gate line preparation, an amorphous silicon surface treatment step is added before TCO film preparation to improve and avoid contamination and oxidation problems on the amorphous silicon surface in the prepared heterojunction battery, thereby ensuring the bulk performance of the amorphous silicon film layer and its contact effect with the TCO film, and improving battery efficiency.
[0043] The present invention uses a self-developed planar ICP (inductor coupling palsma) plasma source generator to treat the surface of amorphous silicon. The plasma source generator mainly includes a discharge chamber, a radio frequency antenna, a radio frequency power supply, and an air intake system. The length and width of the discharge chamber can be customized according to the actual cavity requirements; the radio frequency antenna and the discharge chamber are insulated; the air intake system can be multi-staged to ensure uniformity. Figure 5 This is a structural diagram of the ion source emitter, in which two sections of gas distribution are designed. Figure 5 The atmosphere side and the vacuum side are in an upper-lower relationship, with the plane where the cavity cover flange is located as the boundary, the lower side is the vacuum side, and the upper side is the atmosphere side.
[0044] According to a specific embodiment of the present invention, the above-mentioned ICP ion source is mainly composed of a gas feeding passage, an electrical feeding circuit, and a cooling water circuit, and all the components are placed on the vacuum chamber cover. Among them, the gas feeding passage: the inert gas is fed into the vacuum side through the air distribution holes divided into several sections after passing through the pipeline and MFC control; the MFC controller is arranged above the chamber cover, and is used to control the flow rate and / or quality of the feeding gas so that it can be fed in the amount required by the process; the air distribution holes are arranged below the chamber cover and in the upper inner part of the vacuum chamber, and when distributing the gas, the gas fed into the air distribution holes is evenly ejected downward, which can ensure that the gas pressure is evenly distributed everywhere in the chamber. The electrical feed is provided by an RF power supply (placed in an electrical cabinet, Figure 5 After the power is output to the RF matcher (not shown) (connected via a coaxial cable), it is matched to the plasma impedance by the matcher and then fed to the copper coil via a copper tape. The copper coil is fixedly arranged under the cavity cover and insulated from the entire cavity cover by an insulating pad. The cavity cover is at a grounding point, that is, the cavity cover is connected to the ground. The cooling water and the electrical feed circuit can be fed into a common copper water pipe, which is arranged at one end of the cavity cover, and the water supply pipeline and the electrical feed connection line extend into the vacuum chamber. The copper water pipe and the cavity cover and the inside of the copper water pipe are all sealed to ensure the vacuum state in the vacuum chamber. After the cooling water enters the internal circulation through the copper wire tube, it is discharged from the return water outlet next to the feed inlet, thereby cooling the copper coil.
[0045] In the above embodiments, the MFC controller may be an existing controller, which is not limited in the present invention; the RF power supply and RF matcher may be an existing power supply and matcher that meet the process parameter requirements, which is also not limited in the present invention.
[0046] The working principle of the ICP plasma source of the present invention is as follows: when radio frequency power is added to the coil through an RF matcher, radio frequency current flows through the coil, thereby generating radio frequency magnetic flux; the radio frequency magnetic flux induces a radio frequency electric field along the axial direction inside the discharge chamber; the electrons therein are accelerated by the electric field, thereby generating plasma, and the energy of the coil is coupled into the plasma. The copper coil is a rectangular coil or a circular coil, but the flatness of the rectangular coil in the horizontal direction and the straightness of the rectangular coil or the curvature of the circular coil must be ensured to ensure the planarity and uniformity of the ion source projected onto the surface of the amorphous silicon wafer.
[0047] ICP plasma source generator can generate high-density low-energy plasma with a wide range of working pressures, which is perfectly adapted to heterojunction battery technology. It can remove pollutants and oxide layers on the surface of amorphous silicon film without damaging the original amorphous silicon film. ICP plasma source generator can achieve large-area silicon wafer processing, adapt to the current trend of large-capacity heterojunction equipment, and is suitable for mass production.
[0048] In the above embodiment, the layout of the ICP plasma source generator is as follows: Figure 6As shown. The planar ICP plasma source structure can be completely set according to the size of the PVD equipment cavity opening and the effective width of the sample. The ion source is installed on the reserved cathode position of the PVD equipment. Such a layout will hardly generate additional modification costs and will not affect the production cycle and output of the equipment. The working process includes:
[0049] 1. After the amorphous silicon deposition is completed, the battery is transferred to the nitrogen cabinet or PVD automation;
[0050] 2. PVD automation loads the cells that have completed amorphous silicon deposition into the PVD tray;
[0051] 3. The pallet is transferred to C1, the gate valve between the automation and C1 is closed, and the air is pumped. After the air is pumped, the gate valve between C1 and C2 is opened. The pallet is transferred to C2, the gate valve between C1 and C2 is closed, and the gate valve between C2 and C3 is opened;
[0052] 4. The tray is transferred to C3 and then to C4 at the process speed. When the tray passes under the ICP ion source during the C4 transmission process, the ion source processes the surface of the silicon wafer. The process personnel adjust the RF power of the ion source according to the transmission speed to achieve rapid desorption of water vapor on the tray surface and treatment of surface contaminants and oxide layers of the silicon wafers loaded on the tray.
[0053] 5. Continue to move forward to complete the deposition of the TCO film, and then transfer out of the PVD equipment after the TCO deposition is completed.
[0054] The important work after adding the ion source in the present invention is to adjust the various parameters or settings of the ion source to achieve the best effect. The aspects that need to achieve the best effect include: 1. removing pollutants and oxide layers on the surface of the silicon wafer; 2. quickly desorbing water vapor adsorbed on the surface of the tray.
[0055] The following is the preferred configuration summarized based on the test data. The main relevant parameters are the number of coil turns, power supply power, distance between coil and substrate, anti-plate opening size, tray travel speed, gas flux (pressure / film forming pressure), etc. The results are oriented to the performance parameters of the battery and the peak water vapor partial pressure of the cavity after the tray enters the next cavity (tested using a residual gas analyzer).
[0056] 1. Remove silicon wafer contaminants and oxide layers (characterization parameters: cell conversion efficiency and fill factor):
[0057] The change of FF filling factor with the number of coil turns is as follows Figure 7 As shown. Figure 7It can be seen that when other variables remain unchanged, the number of coil turns between 1 and 2 turns will have a positive improvement in FF, and 2 turns is the optimal configuration. The table in the figure shows the setting values of other variables. When the values of other variables remain unchanged, the relationship between the number of coil turns and the FF filling factor is tested, the same below.
[0058] The change of FF fill factor with RF power is shown as follows Figure 8 As shown. Figure 8 It can be seen that when other variables remain unchanged, the FF fill factor remains basically unchanged when the RF power is between 100-300W, with no obvious effect. There is a significant FF improvement when the RF power is between 400-1000W, and 500W is the optimal configuration. When the RF power is 2000W, a significant FF decrease is seen. It is speculated that when the power is too high, the energy of the particles emitted by the ion source is too large, which may damage the amorphous silicon film layer.
[0059] The change of FF filling factor with the distance between coil and substrate is as follows: Fig. 9 As shown in the test results, when other variables remain unchanged, the distance between the coil and the substrate shows a loss of FF at 80 mm, starts to improve at 100 mm, and reaches the best at 200 mm. It can be seen that the distance between the coil and the substrate is preferably configured to be 200 mm or more.
[0060] The change of FF filling factor with film forming pressure is as follows Fig.10 As shown in the test results, when other variables remain unchanged, the film forming pressure shows a significant improvement below 0.5Pa, 0.5Pa is the optimal configuration, and it is basically the same as the benchmark at 0.8Pa, and the FF begins to decline at 1Pa.
[0061] In summary, the optimal configuration at a walking speed of 1 m / min is shown in Table 1.
[0062] Table 1
[0063]
[0064]
[0065] 2. Remove the water vapor adsorbed on the surface of the tray (characterization parameter: the difference between the water vapor partial pressure in the chamber before ion source treatment and the water vapor partial pressure in the chamber after treatment. In addition, the water vapor partial pressure before treatment is made uniform by controlling the variable)
[0066] The change of the water vapor partial pressure difference between the front and rear chambers with the number of coil turns is as follows: Fig.11As shown in the figure, the test results show that when other variables remain unchanged, the water vapor on the tray surface is significantly reduced after ICP treatment, but there is no obvious difference in the difference in water vapor partial pressure between the front and rear chambers with different coil turns, indicating that different coil turns have little effect on water vapor removal.
[0067] The change of the water vapor partial pressure difference between the front and rear chambers with RF power is shown in Fig.12 As shown in the test results, when other variables remain the same, the amount of water vapor removed from the tray surface is proportional to the RF power. The higher the RF power, the higher the removal rate of water vapor on the tray.
[0068] The difference in water vapor partial pressure between the front and rear chambers changes with the distance between the coil and the substrate as shown in the figure. Fig.13 As shown in the test results, when other variables remain the same, the amount of water vapor removed increases with the distance between the coil and the substrate, and remains basically unchanged after reaching 100mm, so the optimal distance between the substrate and the coil is ≥100mm.
[0069] The change of the water vapor partial pressure difference between the front and rear chambers with the film forming pressure is shown in Fig.14 As shown in the test results, when other variables remain the same, there will be a significant decrease in water vapor after ICP treatment, and the best water vapor removal effect is obtained at 0.5Pa-0.8Pa.
[0070] In summary, the optimal configuration for water vapor removal at 1 m / min is shown in Table 2.
[0071] Table 2
[0072]
[0073]
[0074] Based on the water vapor removal effect and the pollutant and oxide layer removal test results, the optimal process configuration at a travel speed of 1m / min is shown in Table 3.
[0075] Table 3
[0076] parameter Numeric unit Coil turns 2 lock up Distance between coil and substrate 200 mm RF Power 500 W Film forming pressure 0.5 Pa Pallet speed 1 m / min Anti-slip board opening size 150 mm
[0077] The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for a person skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for improving the efficiency of a heterojunction battery, the method comprising the steps of texturing and cleaning, amorphous silicon deposition, TCO film preparation and gate line preparation, characterized in that: Adding amorphous silicon surface treatment before the TCO film preparation step is used to improve the pollution and oxidation problems on the surface of the amorphous silicon wafer during the preparation of the heterojunction battery and remove the water vapor adsorbed on the surface of the tray; The amorphous silicon surface treatment is achieved by using a planar ICP plasma source generator; The planar ICP plasma source generator is set according to the cavity opening size of the PVD device and the effective width of the amorphous silicon wafer to be surface-treated, and the planar ICP plasma source generator is set at the reserved cathode position of the PVD device; When the amorphous silicon wafer to be surface treated is transferred to the bottom of the planar ICP plasma source generator in the PVD device, the planar ICP plasma source generator performs surface treatment on the amorphous silicon wafer to be surface treated; Among them, the planar ICP plasma source generator includes a chamber cover flange, a coil and an RF matcher. When the chamber cover flange is set at the reserved cathode position of the PVD equipment, a vacuum chamber is formed between the chamber cover flange and the PVD equipment; the coil is placed in the vacuum chamber and wound to form a rectangular or circular coil; the coil is connected to the RF matcher to form an RF magnetic flux when an RF current is fed in, and the RF magnetic flux induces an RF electric field, and the RF electric field accelerates the electrons therein to form plasma; cooling water flows inside the coil to cool the coil.
2. The method for improving heterojunction battery efficiency according to claim 1, characterized in that: The width and length of the coil are matched with the amorphous silicon wafer to be processed, so that large-area amorphous silicon wafer surface processing can be achieved.
3. The method for improving heterojunction battery efficiency according to claim 1, characterized in that: Under the condition of 1m / min travel speed, the parameters of amorphous silicon surface treatment include: the number of coil turns is 1-2 turns, the RF power of the planar ICP plasma source generator is 400W-1000W, the distance between the coil and the amorphous silicon wafer to be treated is more than 100mm, and the vacuum degree is less than 0.8pa.
4. The method for improving heterojunction battery efficiency according to claim 3, characterized in that: The number of turns of the coil is 2.
5. The method for improving heterojunction battery efficiency according to claim 3, characterized in that: The RF power is 500W.
6. The method for improving heterojunction battery efficiency according to claim 3, characterized in that: The distance between the coil and the amorphous silicon wafer to be processed is 100mm-200mm.
7. The method for improving heterojunction battery efficiency according to claim 3, characterized in that: The vacuum degree is 0.5pa-0.8pa.