Heat-resistant buffer sheet and heat-pressing treatment method

By designing a heat-resistant buffer sheet with strong shape holding force in the thickness direction at high temperature, the problem of difficult deformation of the heat-resistant buffer sheet at high temperature in the prior art is solved, and effectively preventing the object and the hot pressurized surface at high temperature is achieved. The effect of contact.

CN114829469BActive Publication Date: 2024-11-22NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080088195.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-11-02
Publication Date
2024-11-22
Estimated Expiration
2040-11-02

AI Technical Summary

Technical Problem

Existing heat-resistant buffer sheets, such as PTFE sheets, are difficult to effectively prevent direct contact between the object and the hot pressurized surface at the expected higher temperatures and pressures.

Method used

A heat-resistant buffer sheet was designed, with a compression strain change of ΔS250 at 25°C and 250°C of more than -5%, and a strong shape retention force in the thickness direction at high temperatures. It was evaluated by thermomechanical analysis (TMA). The thickness changes and the sheet is arranged in a heat pressurized process to prevent direct contact.

Benefits of technology

The heat-resistant buffer sheet can better cope with the rise of temperature and pressure at high temperatures, maintain the shape stability in the thickness direction, prevent direct contact between the object and the hot pressing surface, and improve the safety and efficiency of the hot pressing treatment. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114829469B_ABST
    Figure CN114829469B_ABST
Patent Text Reader

Abstract

The heat-resistant buffer sheet provided is arranged between the heat-pressing surface of the heat-pressing device and the object during the heat-pressing treatment of the object, thereby preventing the object from directly contacting the heat-pressing surface. The compressive strain S at 25°C is 25 and the compressive strain S at 250℃ 250 Difference S 250 ‑S 25 That is, the change in compressive strain ΔS 250 More than 5%. Among them, S 25 and S 250 The compressive strain S of the heat-resistant buffer sheet at evaluation temperatures of 25°C and 250°C evaluated by thermomechanical analysis (TMA) are respectively T . Compression strain S T The thickness of the heat-resistant buffer sheet at 25°C is defined as t0, the thickness of the sheet at the evaluation temperature T (°C) when a compressive force is applied in the thickness direction of the heat-resistant buffer sheet by TMA is defined as t1, and the thickness of the sheet is defined as t2. T =(t1-t0) / t0×100(%). The heat-resistant buffer sheet can more reliably cope with the expected further increase in the processing temperature and pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a heat-resistant buffer sheet and a heat-pressing treatment method using the same. Background Art

[0002] Fluororesins are known as heat-resistant resins. Patent Document 1 discloses a cutting sheet of polytetrafluoroethylene (hereinafter referred to as "PTFE"), which is a type of fluororesin. The PTFE sheet as a heat-resistant resin sheet is assumed to be used at high temperatures.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-341138 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] Sometimes, a heat pressurizing device is used to perform heat pressurizing treatment on an object. In this case, it is considered to arrange a heat-resistant buffer sheet between the heat pressurizing surface of the heat pressurizing device and the object (processing object) to prevent the object from directly contacting the heat pressurizing surface, and to use a heat-resistant resin sheet, such as the PTFE sheet of Patent Document 1, as the heat-resistant buffer sheet. However, according to the research of the present inventors, the PTFE sheet of Patent Document 1 may not be able to fully cope with the further increase in processing temperature and pressure that can be expected in the future.

[0008] The object of the present invention is to provide a sheet which is a heat-resistant buffer sheet which is arranged between the heat pressing surface of a heat pressing device and the object during heat pressing treatment of the object to prevent direct contact between the object and the heat pressing surface, and which can more reliably cope with further increases in the expected processing temperature and pressure.

[0009] Solutions for solving problems

[0010] The present invention provides a heat-resistant buffer sheet which is arranged between a heat-pressing surface of a heat-pressing device and the object during heat-pressing treatment of the object, thereby preventing the object from directly contacting the heat-pressing surface.

[0011] The compressive strain S of the heat-resistant buffer sheet at 25°C 25 and the compressive strain S at 250℃ 250 Difference S 250 -S 25 That is, the change in compressive strain ΔS 250 It is above -5%.

[0012] Among them, S 25 and S 250The compressive strain S of the heat-resistant buffer sheet at evaluation temperatures of 25° C. and 250° C. evaluated by thermomechanical analysis (TMA) are respectively T . Compression strain S T The thickness of the heat-resistant buffer sheet at 25°C is defined as t0, the thickness of the sheet at the evaluation temperature T (°C) when a compressive force is applied in the thickness direction of the heat-resistant buffer sheet by TMA is defined as t1, and the thickness of the sheet is defined as t1 by the formula: T =(t1-t0) / t0×100(%) to determine.

[0013] According to another aspect, the present invention provides a heat-resistant buffer sheet which is arranged between a heat-pressing surface of a heat-pressing device and the object during heat-pressing treatment of the object, thereby preventing the object from directly contacting the heat-pressing surface.

[0014] The thickness of the heat-resistant buffer sheet at 25°C after hot pressing at 250°C, 20 MPa and 3 minutes is greater than the thickness of the sheet at 25°C before hot pressing.

[0015] According to another aspect, the present invention provides a method for heat and pressure treatment of an object using a heat and pressure device, wherein:

[0016] A heat-resistant buffer sheet is arranged between the object and the heat-pressing surface of the device, and the heat-pressing treatment is performed in a state where the sheet prevents the object from directly contacting the heat-pressing surface.

[0017] The heat-resistant buffer sheet is the heat-resistant buffer sheet of the present invention.

[0018] Effects of the Invention

[0019] In the heat-resistant buffer sheet of the present invention, the compressive strain S at 25°C evaluated by TMA is 25 and the compressive strain S at 250℃ 250 Difference S 250 -S 25 That is, the change in compressive strain ΔS 250 This means that the easier it is to deform the sheet against the compressive force in the thickness direction (the easier it is to deform, the higher the compressive strain S T In the negative direction, the value of the heat-resistant buffer sheet of the present invention is larger (in the negative direction), but it does not increase significantly at 250°C compared to 25°C, which means that the compression resistance in the thickness direction at high temperature (shape retention in the thickness direction under compression) is high. Therefore, the heat-resistant buffer sheet of the present invention can more reliably cope with the expected further increase in the processing temperature and pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a cross-sectional view schematically showing an example of the heat-resistant buffer sheet of the present invention.

[0021] Figure 2 This is used to explain the change in compressive strain ΔS for evaluating the heat-resistant buffer sheet. 250 Schematic diagram of the method.

[0022] Figure 3 This is a schematic diagram for explaining an example of a method of hot pressing a heat-resistant buffer sheet.

[0023] Figure 4 This is a schematic diagram for explaining an example of heat-pressing treatment using the heat-resistant buffer sheet of the present invention.

[0024] Figure 5 This is a diagram showing the appearance of a heat-resistant buffer sheet after the heat-pressing test A performed in the examples.

[0025] Figure 6 This is a diagram showing the appearance of a heat-resistant buffer sheet after the heat-compression test B performed in the examples. DETAILED DESCRIPTION

[0026] Hereinafter, the embodiments of the present invention will be described with reference to the attached drawings. Figure 1 While explaining.

[0027] [Heat-resistant buffer sheet]

[0028] Figure 1 An example of the heat-resistant buffer sheet of the present invention is shown. Figure 1 The heat-resistant buffer sheet 1 shown is composed of a PTFE sheet 2 . Figure 1 The heat-resistant buffer sheet 1 has a single-layer structure of a PTFE sheet 2. The heat-resistant buffer sheet 1 has high heat resistance and softness derived from the PTFE contained in the sheet 2. In addition to preventing the object (processing object) from directly contacting the heat-pressing surface, the heat-resistant buffer sheet 1 may also have the function of making the heat and / or pressure applied from the heat-pressing surface to the object uniform and adjusting the speed of applying heat and / or pressure, depending on its specific method, the type of heat-pressing treatment, the structure of the heat-pressing device, etc.

[0029] Compression strain S of heat-resistant buffer sheet 1 at 25°C 25 and the compressive strain S at 250℃ 250 Difference S 250 -S 25 That is, the change in compressive strain ΔS 250 "-5% or more" means a value that is -5% or greater than -5% in the positive direction. 25 and S 250The compressive strain S of the heat-resistant buffer sheet 1 at evaluation temperatures of 25°C and 250°C evaluated by TMA are respectively T . Compression strain S T The thickness of the heat-resistant buffer sheet 1 at 25°C is defined as t0, the thickness of the sheet at the evaluation temperature T (°C) when a compressive force is applied in the thickness direction of the heat-resistant buffer sheet 1 by TMA is defined as t1, and the thickness of the sheet is defined as t1 by the formula: T =(t1-t0) / t0×100(%). Figure 2 While explaining.

[0030] The heat-resistant buffer sheet 1 was cut out to prepare a test piece 12, and its thickness t0 ( Figure 2 (a)). The shape of the test piece 12 is, for example, a square or rectangle with a side of 5 to 10 mm. Next, the test piece 12 is placed on the stage 11 of the TMA apparatus maintained at 25°C and the compression probe 13 is lowered ( Figure 2 (b)). The shape and front end diameter of the compression probe 13 are set to be cylindrical and Next, the temperature was kept at 25°C, and a pressure (5 MPa) was applied to the test piece 12 in the thickness direction by a compression probe 13, and the thickness t1 of the test piece 12 at 25°C was measured to obtain the compressive strain S 25 ( Figure 2 (c)). Then, the applied pressure is maintained at 5 MPa, and the temperature is raised at a rate of 5°C / min. The thickness t1 of the test piece 12 when the temperature reaches 250°C is measured to determine the compressive strain S. 250 ( Figure 2 (d)). The obtained compressive strain S 250 With S 25 The compressive strain change ΔS is calculated as the difference between 250 The thickness t1 can be obtained as the distance between the mounting surface of the stage 11 and the tip of the compression probe 13 using a TMA apparatus.

[0031] Compression strain change ΔS 250 It may be -3% or more, -1% or more, 0% or more, 2% or more, or 4% or more. 250 The upper limit is, for example, 20% or less.

[0032] Compression strain S of heat-resistant buffer sheet 1 at 25°C 25 and the compressive strain S at 300℃ 300 Difference S 300 -S 25 That is, the change in compressive strain ΔS 300For example, it is -15% or more. In this case, it is possible to more reliably cope with further increases in the processing temperature and pressure. 300 It may be -10% or more, -5% or more, -3% or more, -1% or more, 0% or more, 2% or more, 3% or more, 4% or more, or even 5% or more. 300 The upper limit of is, for example, 20% or less. 300 and the change in compression strain ΔS 250 The ratio can increase in the positive direction. 300 The evaluation temperature T can be set at 25°C and 300°C and compared with the compressive strain change ΔS 250 Calculate in the same way.

[0033] The heat-resistant buffer sheet 1 may be a sheet that has a greater thickness at 25°C after hot pressing at a temperature of 250°C, a pressure of 20 MPa, and a holding time of 3 minutes than the thickness of the sheet 1 at 25°C before hot pressing at a temperature of 250°C, a pressure of 20 MPa, and a holding time of 3 minutes. The heat-resistant buffer sheet 1 has a high shape retention force in the thickness direction under high-temperature compression. At this time, the compressive strain change ΔS of the heat-resistant buffer sheet 1 is 250 and / or ΔS 300 The heat-pressing of the heat-resistant buffer sheet 1 is performed by placing a simulated object 24 on a carrier 22 of a heat-pressing device 21 and placing the heat-resistant buffer sheet 1 on the simulated object 24, and heat-pressing the entire sheet 1 using a heat-pressing head 23 (see Figure 3 ). Among them, the heat-resistant buffer sheet 1 is configured in a manner covering the entire upper surface of the simulated object 24. In addition, hot pressing is performed after the temperature of the upper surface of the simulated object 24 reaches the set temperature of the carrier 22 (the temperature of the mounting surface). The surface of the simulated object 24 that is usually in contact with the carrier 22 and the surface that is in contact with the heat-resistant buffer sheet 1 are both metal plates that are smooth to the same extent as the mounting surface of the carrier 22 and the hot pressing surface of the hot pressing head 23. The shape of the simulated object 24 is typically a circular plate, a cube or a cuboid. In order to ensure the measurement accuracy, the area of ​​the surface of the simulated object 24 that is in contact with the heat-resistant buffer sheet 1 is preferably 15cm 2 The thickness of the simulated object 24 is preferably 2 to 4 mm. The thickness of the heat-resistant buffer sheet 1 is measured near the center of the pressurized region of the sheet 1 (for example, within a circle with a diameter of 10 mm).

[0034] The thickness of the heat-resistant buffer sheet 1 at 25°C before hot pressing is defined as T0, and the thickness at 25°C after hot pressing is defined as T1. T = (T1-T0) / T0×100(%)Thickness increase rate IR T(20 MPa) is, for example, 1% or more, and may be 2% or more, 4% or more, 5% or more, 7% or more, or 9% or more. T The upper limit of (20 MPa) is, for example, 30% or less.

[0035] The heat-resistant buffer sheet 1 may be a sheet that has a greater thickness at 25°C after hot pressing than the thickness of the sheet 1 at 25°C before hot pressing at a temperature of 250°C, a pressure of 30 MPa, and a holding time of 3 minutes. Hot pressing may be performed in the same manner as when a pressure of 20 MPa is applied. In this case, the thickness increase rate IR T (30 MPa) can be, for example, 1% or more, 2% or more, 3% or more, 4% or more, or 5% or more. T The upper limit of (30 MPa) is, for example, 20% or less.

[0036] Figure 1 The heat-resistant buffer sheet 1 is composed of a PTFE sheet 2. However, the resin contained in the heat-resistant buffer sheet 1 is not limited to PTFE. The resin can be a fluororesin, in other words, the heat-resistant buffer sheet 1 can contain a sheet of fluororesin. Examples of fluororesins are PTFE, modified PTFE, ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) and polyvinylidene fluoride (PVDF). From the aspect of particularly excellent heat resistance and softness, the fluororesin is preferably PTFE, modified PTFE, ETFE, and particularly preferably PTFE and modified PTFE.

[0037] Modified PTFE is a copolymer of TFE and a modified comonomer. In order to be classified as modified PTFE, the content of tetrafluoroethylene (TFE) units in the copolymer needs to be more than 99 mass %. Modified PTFE is, for example, a copolymer of TFE and at least one modified comonomer selected from ethylene, perfluoroalkyl vinyl ether and hexafluoropropylene.

[0038] The PTFE sheet 2 is preferably a sintered PTFE sheet containing sintered PTFE. In this specification, sintering PTFE means heating PTFE obtained by polymerization to a temperature higher than its melting point (327°C), for example, 340 to 380°C.

[0039] The thickness of the heat-resistant buffer sheet 1 is, for example, 10 μm or more, 50 μm or more, 100 μm or more, 250 μm or more, 300 μm or more, 400 μm or more, or 500 μm or more. The upper limit of the thickness is, for example, 2000 μm or less, 1500 μm or less, or 1000 μm or less.

[0040] The tensile strength of the heat-resistant buffer sheet 1 varies depending on the type of resin contained in the heat-resistant buffer sheet 1. For example, for MD (usually the length direction in a strip-shaped sheet), it is 30 MPa or more, and it can also be 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 90 MPa or more, and then 100 MPa or more. The tensile strength for TD (usually the width direction in a strip-shaped sheet) is 10 MPa or more, and it can also be 15 MPa or more, 20 MPa or more, 25 MPa or more, 30 MPa or more, 35 MPa or more, 40 MPa or more, and then 45 MPa or more. The upper limit of the tensile strength is, for example, 500 MPa or less. According to the heat-resistant buffer sheet 1 having the tensile strength in the above range, for example, it is possible to more reliably and stably implement the supply based on the transportation between the hot pressurization surface and the object.

[0041] The maximum tensile elongation of the heat-resistant buffer sheet 1 varies depending on the type of resin contained in the heat-resistant buffer sheet 1. For example, for MD, it is 300% or less, and it can also be 275% or less, 250% or less, 225% or less, 200% or less, 180% or less, 160% or less, 140% or less, 120% or less, 100% or less, 90% or less, and further 80% or less. For MD, the lower limit of the maximum tensile elongation is, for example, 5% or more. For TD, the maximum tensile elongation is, for example, 200% or more, and it can also be 400% or more, 410% or more, 420% or more, 425% or more, 430% or more, 435% or more, and further 440% or more. For TD, the upper limit of the maximum tensile elongation is, for example, 700% or less. According to the heat-resistant buffer sheet 1 having the maximum tensile elongation in the above range with respect to MD, in particular, the heat-resistant buffer sheet 1 having the maximum tensile elongation of 200% or less, when the heat-resistant buffer sheet 1 is supplied by conveyance between a hot press surface and an object, for example, even if a part of the heat-resistant buffer sheet 1 is bonded to the hot press surface and / or the object, the sheet 1 can be prevented from following these members by the elongation. In other words, the continuous supply property of the heat-resistant buffer sheet 1 to the hot press treatment can be further improved.

[0042] The tensile strength and maximum tensile elongation of the heat-resistant buffer sheet 1 can be obtained by a tensile test using a tensile testing machine. The shape of the test piece is, for example, a dumbbell No. 3 shape specified in Japanese Industrial Standard (JIS) K6251:1993. The measurement conditions when using the above test piece are, for example, a distance between markings of 20 mm, a distance between chucks of 35 mm, and a tensile speed of 200 mm / min. The maximum tensile elongation can be calculated based on the distance between markings before the test and the distance between markings at the time of fracture. The measurement temperature is, for example, 25±10°C.

[0043] The dimensional change rate of the heat-resistant buffer sheet 1 (the dimensional change rate when left to stand for 1 hour in an atmosphere of 270°C without applying pressure, the same below) is, for example, -5.0% or less in MD, and may be -7.5% or less, -10.0% or less, -12.5% ​​or less, -15.0% or less, and further -17.5% or less. For MD, the lower limit of the dimensional change rate is, for example, -30.0% or more. For TD, the dimensional change rate is, for example, 1.5% or less, and may be 1.3% or less, 1.0% or less, 0.7% or less, 0.5% or less, 0.3% or less, and further 0% or less. For TD, the lower limit of the dimensional change rate is, for example, -2.0% or more. The dimensional change rate in the thickness direction is, for example, 5.0% or more, and may be 7.5% or more, 10.0% or more, 12.5% ​​or more, 15.0% or more, 17.5% or more, and further 20.0% or more. The upper limit of the dimensional change rate in the thickness direction is, for example, 40.0% or less. The dimensional change rate is given by the formula: (X1-X0) / X0×100(%). X0 is the dimension before heating, and X1 is the dimension after heating.

[0044] The heat-resistant buffer sheet 1 may have other layers disposed on at least one main surface. However, when good thermal conductivity is required for the heat-resistant buffer sheet 1, it is preferred that no other layers be disposed on the main surface. In other words, the heat-resistant buffer sheet 1 may be a single layer.

[0045] The heat-resistant buffer sheet 1 is preferably a non-porous sheet. The heat-resistant buffer sheet 1 may be a non-porous sheet having no holes connecting the two main surfaces at least in the use area. The heat-resistant buffer sheet 1 may also be an impermeable sheet that does not allow fluids such as water to penetrate in the thickness direction based on the high liquid repellency (water repellency and oil repellency) of the material contained in the sheet 1, such as PTFE. In addition, the heat-resistant buffer sheet 1 may also be an insulating sheet (non-conductive sheet) based on the high insulation of the material contained in the sheet 1, such as PTFE. The insulation is measured by, for example, 1×10 14 The surface resistivity can be expressed as 1×10 15 Ω / □ or more, 1×10 16 Ω / □ or more, and further 1×10 17 Ω / □ or more. The heat-resistant buffer sheet 1 may contain a conductive material such as carbon black. In this case, the heat-resistant buffer sheet 1 may have a function based on the conductive material, such as an antistatic function. The surface resistivity of the heat-resistant buffer sheet 1 containing a conductive material is, for example, 1×10 12 Ω / □ or less, or 1×10 8 Ω / □ or less, 1×10 4 Ω / □ or less.

[0046] The shape of the heat-resistant buffer sheet 1 can be, for example, a polygon including a square and a rectangle, a circle, an ellipse, and a strip. The corners of the polygon can be rounded. However, the shape of the heat-resistant buffer sheet 1 is not limited to these examples. The polygonal, circular, and elliptical heat-resistant buffer sheets 1 can be circulated in the form of a single sheet, and the strip-shaped heat-resistant buffer sheet 1 can be circulated in the form of a winding body (roll) wound on a winding core. The width of the strip-shaped heat-resistant buffer sheet 1 and the width of the winding body formed by winding the strip-shaped heat-resistant buffer sheet 1 can be freely set.

[0047] [Method for producing heat-resistant buffer sheet]

[0048] Hereinafter, an example of a method for producing the heat-resistant buffer sheet 1 will be described by taking the heat-resistant buffer sheet 1 composed of the PTFE sheet 2 or the modified PTFE sheet as an example. However, the method for producing the heat-resistant buffer sheet 1 is not limited to the example described below.

[0049] First, PTFE powder (molding powder) is introduced into a mold, and a predetermined pressure is applied to the powder in the mold for a predetermined time to perform preforming. Preforming can be performed at room temperature. In order to enable cutting based on a cutting lathe described later, the shape of the internal space of the mold is preferably cylindrical. At this time, a cylindrical preform and a PTFE block are obtained. When the PTFE block is cylindrical, the cutting lathe can be used to rotate the block while continuously cutting the surface, so that a heat-resistant buffer sheet 1 can be efficiently formed. Then, the obtained preform is taken out of the mold, and sintered at a temperature above the melting point of PTFE (327°C) for a predetermined time to obtain a PTFE block. Then, the obtained PTFE block is cut into a predetermined thickness to obtain a PTFE sheet as a cutting sheet. Then, the obtained PTFE sheet is calendered to obtain a PTFE sheet 2 as a calendered sheet. The obtained PTFE sheet 2 can be used directly as a heat-resistant buffer sheet 1, or it can be used as a heat-resistant buffer sheet 1 after undergoing a predetermined treatment, lamination with other layers, etc. The calendering is typically uniaxial calendering of the MD. The calendering can be performed using a roller calendering device having a pair of metal rollers. The calendering ratio is, for example, 1.5 times or more based on the thickness, and can also be 1.8 times or more, 2.0 times or more, 2.3 times or more, 2.5 times or more, 2.8 times or more, and further 3.0 times or more. The upper limit of the calendering ratio is, for example, 10.0 times or less. The calendering temperature is, for example, 100 to 200°C, and can also be 200 to 300°C, and further 300°C or more. It should be noted that according to the above-mentioned method, the thickness of the heat-resistant buffer sheet 1 formed is relatively easy to control, and a strip-shaped heat-resistant buffer sheet 1 can also be formed. In addition, by using modified PTFE powder instead of PTFE powder, a modified PTFE sheet can be formed by the above-mentioned method.

[0050] [Use of heat-resistant buffer sheet]

[0051] like Figure 4 As shown, the heat-resistant buffer sheet 1 can be used as a heat-resistant buffer sheet arranged between the heat-pressing surface 34 of the heat-pressing device 31 and the object 35 to prevent the two from sticking to each other during the heat-pressing treatment of the object 35 by the heat-pressing device 31. The heat-resistant buffer sheet 1 has excellent buffering properties. Figure 4 The heat press device 31 includes a stage 32 and a heat press head 33 having a heat press surface 34. The heat-resistant buffer sheet 1 is disposed between the heat press head 33 and the object 35. The heat press treatment in this example is performed by bringing the heat press head 33 and the stage 32 close to each other while the object 35 is placed on the stage 32, typically by lowering the heat press head 33. The heat press treatment is, for example, heat compression bonding or heat pressing of the object 35.

[0052] The heat-resistant buffer sheet 1 can be supplied by conveyance and arranged between the heat-pressing surface 34 and the object 35. The heat-resistant buffer sheet 1 supplied by conveyance and arranged is, for example, in a belt shape.

[0053] The heating setting temperature of the heat press device 31 during the heat press treatment, in other words, the use temperature of the heat-resistant buffer sheet 1 is, for example, 200°C or more, and may be 225°C or more, 250°C or more, 275°C or more, and further 300°C or more. The upper limit of the use temperature is, for example, 330°C or less. The press setting pressure of the heat press device 31 during the heat press treatment, in other words, the use pressure of the heat-resistant buffer sheet 1 is, for example, 10MPa or more, and may be 15MPa or more, 20MPa or more, 25MPa or more, and further 30MPa or more. The upper limit of the use pressure is, for example, 50MPa or less. However, the use temperature and the use pressure of the heat-resistant buffer sheet 1 are not limited to these ranges. The heat-resistant buffer sheet 1 may also be used at a lower use temperature and / or use pressure than those exemplified above.

[0054] [Heat and pressure treatment method]

[0055] The heat-resistant buffer sheet 1 of the present invention can be used to perform a heat-pressing treatment on the object 35. The heat-pressing treatment method is a heat-pressing treatment method for the object 35 performed using a heat-pressing device, wherein the heat-resistant buffer sheet 1 is arranged between the object 35 and the heat-pressing surface 34, and the heat-pressing treatment is performed in a state where the heat-resistant buffer sheet 1 is prevented from directly contacting the object 35 with the heat-pressing surface 34. The heat-resistant buffer sheet 1 can be supplied and arranged between the object 35 and the heat-pressing surface 34 by conveyance, for example.

[0056] [Method for producing heat-pressed product]

[0057] The heat-resistant buffer sheet 1 of the present invention can be used to manufacture a heat-pressed product. The manufacturing method includes the following steps: placing the heat-resistant buffer sheet 1 between the object 35 and the heat-pressed surface 34, performing heat-pressed treatment in a state where the object 35 is prevented from directly contacting the heat-pressed surface 34 by the sheet 1, thereby obtaining a heat-pressed product of the object. The heat-pressed treatment is, for example, heat-compression bonding or heat-pressing of the object 35, and in this case, a heat-compressed product or a heat-pressed product is obtained.

[0058] Example

[0059] The present invention is described in more detail below by way of examples. The present invention is not limited to the following examples.

[0060] First, the evaluation method of the heat-resistant buffer sheet produced in this example is described.

[0061] [thickness]

[0062] The thickness was determined as the average value of the values ​​measured at 25° C. using a digital micrometer (minimum scale: 0.001 mm) at any three points.

[0063] [Compression strain]

[0064] The compression strain change ΔS is calculated by the above method. 250 and ΔS 300 The shape and size of the test piece used for TMA were set to a square of 5 mm×5 mm. The TMA apparatus used was TMA4000SA manufactured by BRUKER.

[0065] [Hot pressure test on simulated object]

[0066] <Test A>

[0067] A circular stainless steel plate A (see FIG. 1 ) with a diameter of 47 mm and a thickness of 3 mm was placed on the stage 22 of the hot pressing device 21 having the stage 22 and the hot pressing head 23 as a simulated hot pressing object (simulated object) 24. Figure 3 ). The set temperature of the carrier 22 is set to 250°C. After the temperature of the upper surface of the simulated object 24 reaches the set temperature of the carrier 22, the heat-resistant buffer sheet 1 of the evaluation object cut into a square of size 60mm×60mm is arranged on the simulated object 24, and the hot pressing head 23 is quickly lowered to implement a hot pressing test at a temperature of 250°C, an applied pressure of 20MPa or 30MPa, and a holding time of 3 minutes. The heat-resistant buffer sheet 1 is arranged in a manner covering the entire upper surface of the simulated object 24. After the test, after cooling to 25°C, the heat-resistant buffer sheet 1 is peeled off from the stainless steel plate A, and the thickness and appearance of the heat-resistant buffer sheet 1 at 25°C after the test are evaluated. The thickness is measured near the center of the heat-resistant buffer sheet 1 (within a circle with a diameter of 10mm). The appearance after the test is shown in Figure 5.

[0068] <Test B>

[0069] The hot pressing test was carried out in the same manner as in Test A, except that the simulated object 24 used a stainless steel plate B (a circular plate with a diameter of 47 mm and a thickness of 4 mm and a through hole with a diameter of 2 mm extending in the thickness direction at the center) instead of the stainless steel plate A. The applied pressure was set to 30 MPa. After the test, the heat-resistant buffer sheet 1 was peeled off from the stainless steel plate B after cooling to 25°C, and the penetration amount of the heat-resistant buffer sheet 1 into the through hole of the stainless steel plate B was evaluated. The penetration amount was measured using a vernier caliper. The appearance after the test is shown in Figure 6 It should be noted that in Comparative Example 1, since the penetrated PTFE diffused to the back side of the stainless steel plate B, the heat-resistant buffer sheet could not be peeled off from the stainless steel plate B (see Figure 6 . Figure 6 In the figure, only the back side of the stainless steel plate B is shown for Comparative Example 1).

[0070] [Tensile strength and maximum tensile elongation]

[0071] The tensile strength (tensile breaking strength) and the maximum tensile elongation are obtained by a tensile test using a tensile testing machine (manufactured by Shimadzu Corporation, AG-I). The evaluation is carried out separately in the length direction (MD) and the width direction (TD) of the heat-resistant buffer sheet. The shape of the test piece is set to the dumbbell No. 3 shape (the distance between the markings is 20 mm) specified in JIS K6251:1993. The measurement conditions are set to a measurement temperature of 25°C, a distance between the chucks of 35 mm, and a tensile speed of 200 mm / min. The maximum tensile elongation is calculated based on the distance between the markings before the test and the distance between the markings at the time of fracture.

[0072] [Dimensional change rate]

[0073] The dimensional change rate during heating is evaluated by placing the heat-resistant buffer sheet to be evaluated in a heating tank, leaving it at 270°C for 1 hour, cooling it to 25°C, and measuring the dimensions. The dimensions are measured using a vernier ruler. The evaluation is performed in the MD, TD, and thickness directions of the heat-resistant buffer sheet. It should be noted that the dimensional change rate is a value evaluated without applying pressure to the heat-resistant buffer sheet.

[0074] (Comparative Example 1)

[0075] PTFE powder (DAIKIN INDUSTRIES, LTD., Polyflon PTFE M-12) was introduced into a cylindrical mold and preformed under the conditions of temperature 23°C, pressure 8.5 MPa and pressure application time of 1 hour. Then, the preformed product was taken out from the mold and sintered at 370°C for 24 hours to obtain a cylindrical PTFE block with a height of 300 mm and an outer diameter of 470 mm. Then, the obtained PTFE block was cut using a cutting lathe to produce a PTFE cutting film (thickness 486 μm), which was used as the heat-resistant buffer sheet of Comparative Example 1.

[0076] (Example 1)

[0077] The PTFE block obtained in the same manner as in Comparative Example 1 was cut using a cutting lathe to obtain a PTFE cut film. Next, the cut film was rolled using a roll calendering device having a pair of metal rolls maintained at 175° C. to produce a PTFE rolled film (thickness 508 μm), which was used as the heat-resistant buffer sheet of Example 1. The rolling ratio was set to 2.0 times based on the thickness.

[0078] (Example 2)

[0079] A PTFE rolled film (thickness 497 μm) was prepared as a heat-resistant buffer sheet of Example 2 in the same manner as in Example 1 except that the rolling ratio was set to 2.5 times based on the thickness.

[0080] (Example 3)

[0081] A PTFE rolled film (thickness 500 μm) was prepared as a heat-resistant buffer sheet of Example 3 in the same manner as in Example 1 except that the rolling ratio was 3.0 times based on the thickness.

[0082] The evaluation results are summarized in Table 1 below.

[0083] [Table 1]

[0084]

[0085] As shown in Table 1, the compressive strain changes ΔS of Examples 1 to 3 are 250 and ΔS 300 , especially ΔS 300 , compared with Comparative Example 1, the values ​​are larger in the positive direction, that is, the heat-resistant buffer sheets of Examples 1 to 3 are excellent in the compression resistance in the thickness direction at high temperatures. In addition, in the actual hot press test, the thickness reduction of the heat-resistant buffer sheet (in some examples, the thickness even increased) was suppressed, and the deformation of the sheet including the penetration into the through hole was also suppressed (refer to Figure 5 ,6 ). Based on the results of the dimensional change rate, it is speculated that these characteristics are derived from the following phenomenon: the compressive stress in the thickness direction generated in the sheet due to rolling during production is released due to heat.

[0086] Industrial Applicability

[0087] The heat-resistant buffer sheet of the present invention can be placed between the heat-pressing surface of a heat-pressing device and the object during heat-pressing treatment of the object to prevent direct contact between the object and the heat-pressing surface. The heat-pressing treatment is, for example, thermocompression bonding or thermopressing.

Claims

1. A heat-resistant buffer sheet, which is arranged between a heat-pressing surface of a heat-pressing device and the object during heat-pressing treatment of the object, thereby preventing the object from directly contacting the heat-pressing surface. The compressive strain S of the heat-resistant buffer sheet at 25°C 25 and the compressive strain S at 250℃ 250 Difference S 250 -S 25 That is, the change in compressive strain ΔS 250 is -5% or more, in, S 25 and S 250 The compressive strain S of the heat-resistant buffer sheet at evaluation temperatures of 25° C. and 250° C. evaluated by thermomechanical analysis (TMA) are respectively T , compression strain S T The thickness of the heat-resistant buffer sheet at 25°C is defined as t0, the thickness of the sheet at the evaluation temperature T (°C) when a compressive force is applied in the thickness direction of the heat-resistant buffer sheet by TMA is defined as t1, and the thickness of the sheet is defined as t2 by the formula: T =(t1-t0) / t0×100(%) to determine.

2. A heat-resistant buffer sheet, which is arranged between a heat-pressing surface of a heat-pressing device and the object during heat-pressing treatment of the object, thereby preventing the object from directly contacting the heat-pressing surface. The thickness of the heat-resistant buffer sheet at 25°C after hot pressing at a temperature of 250°C, a pressure of 20 MPa and a holding time of 3 minutes is greater than the thickness of the sheet at 25°C before hot pressing.

3. The heat-resistant buffer sheet according to claim 1 or 2, wherein: The heat-resistant buffer sheet includes a fluororesin sheet.

4. The heat-resistant buffer sheet according to claim 3, wherein: The fluororesin is polytetrafluoroethylene (PTFE) or modified PTFE, The content of tetrafluoroethylene (TFE) units in the modified PTFE is 99% by mass or more.

5. A method for heat and pressure treatment of an object, which is a method for heat and pressure treatment of an object using a heat and pressure device, wherein: A heat-resistant buffer sheet is arranged between the object and the heat-pressing surface of the device, and the heat-pressing treatment is performed in a state where the sheet prevents the object from directly contacting the heat-pressing surface. The heat-resistant buffer sheet is the heat-resistant buffer sheet according to claim 1 or 2.