Optical laminate and image display device
By using a combination of polarizer, light selection absorbent adhesive layer and intermediate layer in the polarizer plate, the problem of decolorization of polarizer at high temperature and high humidity is solved, and durability improvement and bonding in high temperature and high humidity environments are achieved. Avoid shrinkage of the agent layer.
Patent Information
- Application Number
- CN202080089259.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-13
- Filing Date
- 2020-11-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-11-30
AI Technical Summary
The conventional polarizing plate is prone to decolorization in a high temperature and high humidity environment, especially in the structure of a laminated protective film on one side of the polarizing plate, and the boron content is increased to suppress decolorization and may easily lead to the problem of shrinkage of the adhesive layer.
An optical laminate is adopted, which includes a polarizer, a light-selective absorbent adhesive layer and an intermediate layer. The polarizer absorbs iodine and the boron content is less than 5.0 mass %, and the light-selective absorbent adhesive layer contains a specific light-selective absorbent The absorbance at a wavelength of 410 nm is 0.1 or more and 2.3 or less, and an intermediate layer is provided between the polarizer and the adhesive layer to prevent decolorization.
It effectively suppresses the decolorization of the polarizer in high temperature and high humidity environment, improves the durability of the polarizer, and avoids the problem of shrinkage of the adhesive layer.
Smart Images

Figure CN114846377B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate and an image display device. Background Art
[0002] A polarizing plate formed by laminating and bonding a protective film on one or both sides of a polarizer is widely used as an optical member for image display devices such as liquid crystal display devices and organic electroluminescence (organic EL) display devices typified by mobile devices and televisions, especially various mobile devices such as mobile phones, smartphones, and tablet terminals in recent years.
[0003] The polarizing plate is often used by being bonded to an image display element (such as a liquid crystal cell or an organic EL display element) via an adhesive layer (for example, Japanese Patent Application Laid-Open No. 2010-229321 (Patent Document 1)). Therefore, the polarizing plate sometimes circulates in the market in the form of a polarizing plate with an adhesive layer having an adhesive layer provided on one of its sides in advance.
[0004] In addition, mobile devices are often used in severe environments of high temperature and high humidity, and high durability is required for polarizers. Japanese Patent Application Laid-Open No. 2013-105036 (Patent Document 2) describes that by increasing the boric acid content in the polarizer, boric acid crosslinking occurs more frequently, and thus, the I3 complex exists with high orientation and high stability, whereby the occurrence of blue leakage is suppressed, and a polarizer excellent in low-temperature and high-humidity durability can be obtained.
[0005] Prior Art Documents
[0006] Patent Documents
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2010-229321
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 2013-105036 Summary of the Invention
[0009] Problems to be Solved by the Invention
[0010] In a polarizing plate, there is a problem that discoloration (in Japanese: 色抜け) easily occurs at the end portion of the polarizer in an environment of high temperature and high humidity. This problem is significant in a configuration in which a protective film is laminated and bonded only on one side of the polarizer. Although there is a method of suppressing the discoloration of the polarizer by increasing the boron content in the polarizer, according to this method, there is a problem that it is likely to shrink due to heating.
[0011] An object of the present invention is to provide a novel optical laminate in which discoloration at the end portion of the polarizer is suppressed under high temperature and high humidity.
[0012] Means for Solving the Problems
[0013] The present invention provides the optical layered bodies exemplified below and image display devices using the optical layered bodies.
[0014] [1] An optical laminate comprising: a polarizing plate, a light selectively absorbing adhesive layer, and an intermediate layer laminated between the polarizing plate and the light selectively absorbing adhesive layer so as to be in contact with the polarizing plate and the light selectively absorbing adhesive layer;
[0015] The intermediate layer has only one or more layers selected from a liquid crystal solidification layer, an orientation layer, and a lamination layer.
[0016] The polarizer absorbs iodine and orients the iodine, and the boron content is 5.0 mass % or less.
[0017] The light selectively absorbing adhesive layer contains a light selective absorber and has an absorbance of 0.1 to 2.3 at a wavelength of 410 nm.
[0018] [2] The optical layered body according to [1], further comprising a protective film laminated on the side of the polarizer opposite to the intermediate layer side.
[0019] [3] The optical layered body according to [1] or [2], wherein
[0020] In the light selectively absorbing adhesive layer, the content of the light selective absorber per unit area is 0.01 g / m 2 Above and 5g / m 2 the following.
[0021] [4] The optical layered body according to any one of [1] to [3], wherein
[0022] The light selectively absorbing adhesive layer contains 0.1 parts by mass or more and 10 parts by mass or less of the light selective absorber with respect to 100 parts by mass of all resin components contained in the light selectively absorbing adhesive layer.
[0023] [5] The optical layered body according to any one of [1] to [4], wherein
[0024] The light selectively absorbing adhesive layer has a thickness of 0.1 μm or more and 150 μm or less.
[0025] [6] The optical layered body according to any one of [1] to [5], wherein
[0026] The light selective absorber is an organic light selective absorber having a molecular weight of 100 to 3000.
[0027] [7] The optical layered body according to any one of [1] to [6], wherein
[0028] The intermediate layer has a λ / 4 phase difference layer as the liquid crystal solidified layer.
[0029] [8] The optical layered body according to any one of [1] to [7], which is an antireflection polarizing plate.
[0030] [9] An image display device comprising: an image display panel; and the optical layered body according to [8] disposed on a front surface of the image display panel.
[0031]
[10] The image display device according to [9], wherein:
[0032] The image display panel is an organic EL display panel.
[0033] Effects of the Invention
[0034] According to the present invention, it is possible to provide an optical layered body in which discoloration at the edge of a polarizing plate is suppressed under a high-temperature and high-humidity environment, and an image display device including the optical layered body. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic cross-sectional view showing an example of the optical layered body of the present invention.
[0036] Figure 2 This is a schematic cross-sectional view showing an example of the optical layered body of the present invention.
[0037] Figure 3 This is a schematic cross-sectional view showing an example of the optical layered body of the present invention.
[0038] Figure 4 This is a diagram showing an example of an image observed using an optical microscope.
[0039] Figure 5 This is a diagram showing an example of converting an observed image into black and white 256-level data. DETAILED DESCRIPTION
[0040] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, in order to make each component easy to understand, the scale is appropriately adjusted and shown, and the scale of each component shown in the drawings is not necessarily consistent with the scale of the actual component.
[0041] <Optical laminate>
[0042] The optical laminate of the present invention comprises a polarizing plate, a light selectively absorbing adhesive layer, and an intermediate layer laminated between the polarizing plate and the light selectively absorbing adhesive layer so as to be in contact with the polarizing plate and the light selectively absorbing adhesive layer. An example of the layer structure of the optical laminate of the present invention is shown in Figure 1 , Figure 2 , Figure 3 .
[0043] Figure 1 This is a schematic cross-sectional view of an example of the optical layered body of the present invention. Figure 1 The optical laminate 100 shown in this example includes a protective film 11, a polarizing plate 10, an intermediate layer 300, and a light selectively absorbing adhesive layer (hereinafter also referred to as a "first adhesive layer") 20. The intermediate layer 300 includes only one or more layers selected from a liquid crystal solidification layer, an alignment layer, and a laminating layer.
[0044] Figure 2 This is a schematic cross-sectional view of an example of the optical layered body of the present invention. Figure 2 The optical laminate 101 shown has a protective film 11, a polarizing plate 10, an intermediate layer 300, and a light selectively absorbing adhesive layer 20 in this order. The intermediate layer 300 has a second adhesive layer 32, a first liquid crystal solidified layer 30, an adhesive layer 33, and a second liquid crystal solidified layer 31 in this order from the polarizing plate 10 side.
[0045] Figure 3 This is a schematic cross-sectional view of an example of the optical layered body of the present invention. Figure 3 The optical laminate 102 shown includes a protective film 11, a polarizing plate 10, an intermediate layer 300, and a light selectively absorbing adhesive layer 20 in this order. The intermediate layer 300 is formed of a second adhesive layer 32.
[0046] The thickness of the optical layered bodies 100 , 101 , 102 varies depending on the functions required of the optical layered bodies and the uses of the optical layered bodies, and is not particularly limited, and may be, for example, 5 μm to 200 μm, 10 μm to 150 μm, or 120 μm or less.
[0047] The light selectively absorbing adhesive layer contains a light selective absorber. The optical laminate of the present invention has light selective absorbing performance by at least making the light selectively absorbing adhesive layer have light selective absorbing performance, so that the optical laminate as a whole also has light selective absorbing performance. Therefore, when the optical laminate of the present invention is used on an image display element, it has the function of protecting the image display element from the influence of ultraviolet rays.
[0048] The optical laminate of the present invention may be a structure that includes a layer having light selective absorption performance in addition to the light selective absorption adhesive layer. Examples of other layers include a protective film 11 and an intermediate layer 300. In the present invention, since the light selective absorption adhesive layer has light selective absorption performance and contributes to the embodiment of the light selective absorption performance of the entire optical laminate, the degree of freedom in designing the light selective absorption performance in other layers can be increased. For example, for the protective film 11, it is sometimes necessary to increase its thickness in order to improve the light selective absorption performance, but since the degree of freedom in designing the light selective absorption performance is high, it is easy to make the protective film 11 thinner. For example, from the viewpoint of suppressing discoloration of the end of the polarizer under high temperature and high humidity, the intermediate layer 300 is preferably a structure that does not substantially contain a light selective absorber. In the case of containing a light selective absorber, its content is also preferably 0.5 g / m 2 When the intermediate layer 300 has a second adhesive layer, the second adhesive layer is also preferably configured to substantially not contain a light selective absorber. When a light selective absorber is contained, the content thereof is preferably 0.5 g / m 2 the following.
[0049] The present inventors have obtained the knowledge that there is a correlation between the content of the light selective absorber contained in the adhesive layer and the degree of discoloration of the end of the polarizer under high temperature and high humidity. Based on this knowledge, it can be considered that: under high temperature and high humidity, the light selective absorber in the light selective absorber adhesive layer is easy to move to the polarizer side, and this movement is one of the main reasons for the discoloration. The present inventors have further repeatedly conducted in-depth research and found that even if the light selective absorber adhesive layer contains a light selective absorber, by adjusting the lamination position and absorbance of the light selective absorber adhesive layer, the discoloration of the end of the polarizer under high temperature and high humidity can be suppressed, thereby completing the present invention.
[0050] [Polarizing plate]
[0051] The polarizer has the following properties: absorbs linear polarized light having a vibration plane parallel to its absorption axis and transmits linear polarized light having a vibration plane orthogonal to the absorption axis (parallel to the transmission axis). The polarizer 10 in the optical laminate of the present invention adsorbs iodine and aligns the iodine, and the boron content is 5.0 mass % or less.
[0052] By having a boron content of 5.0% by mass or less, preferably 4.5% by mass or less, shrinkage due to heating can be suppressed. The boron content is preferably 0.5% by mass or more, more preferably 1% by mass or more. In the polarizer 10, the less the boron content, the easier it is for the end of the polarizer to discolor under high temperature and high humidity to occur. The boron in the polarizer 10 increases the crosslinking degree of the polarizer 10, which helps to stably maintain iodine in the polarizer 10. Therefore, it is believed that if the boron content decreases, it will become impossible to stably maintain iodine and discoloration will occur. In the present invention, with respect to the polarizer 10, even if the boron content is 5.0% by mass or less, discoloration under high temperature and high humidity can be suppressed.
[0053] The polarizing plate 10 may include a stretched film or stretched layer adsorbed with a dichroic dye having absorption anisotropy, a cured product containing a polymerizable liquid crystal compound and a liquid crystal cured layer containing a dichroic dye, etc. A dichroic dye is a dye having a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction, and iodine is preferably used as the dye.
[0054] (1) A polarizing plate having a stretched film or stretched layer adsorbed with a dye having absorption anisotropy
[0055] A polarizing plate that is a stretched film adsorbed with a dye having absorption anisotropy can generally be manufactured through the following steps: a step of uniaxially stretching a polyvinyl alcohol resin film; a step of dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine to adsorb the dichroic dye; a step of treating the polyvinyl alcohol resin film adsorbed with the dichroic dye with an aqueous boric acid solution; and a step of washing with water after the treatment with the aqueous boric acid solution.
[0056] The thickness of the polarizer is usually 30 μm or less, preferably 15 μm or less, more preferably 13 μm or less, further preferably 10 μm or less, particularly preferably 8 μm or less. The thickness of the polarizer is usually 2 μm or more, preferably 3 μm or more, for example 5 μm or more.
[0057] The polyvinyl alcohol resin is obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, a copolymer of vinyl acetate and other monomers copolymerizable with vinyl acetate can be used. As other monomers copolymerizable with vinyl acetate, for example, unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group can be cited.
[0058] The saponification degree of the polyvinyl alcohol resin is usually 85 mol% or more and 100 mol% or less, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal, polyvinyl acetal, etc. modified by aldehydes may also be used. The degree of polymerization of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less.
[0059] As for the polarizer as a stretched layer adsorbed with a pigment having absorption anisotropy, it can usually be manufactured through the following steps: a step of applying a coating liquid containing the above-mentioned polyvinyl alcohol resin on a substrate film; a step of uniaxially stretching the obtained laminated film; a step of dyeing the polyvinyl alcohol resin layer of the uniaxially stretched laminated film with a dichroic pigment such as iodine so that it adsorbs the dichroic pigment to make a polarizer; a step of treating the film adsorbed with the dichroic pigment with an aqueous boric acid solution; and a step of washing with water after the treatment with an aqueous boric acid solution. The substrate film used to form the polarizer can also be used as a protective film 11. The substrate film can be peeled off from the polarizer as needed. The material and thickness of the substrate film can be the same as the material and thickness of the protective film 11 described later.
[0060] [Protective film]
[0061] The protective film 11 can be formed into a coating or film by the following components: optically transparent thermoplastic resins, such as cyclic polyolefin resins; cellulose acetate resins including resins such as cellulose triacetate and cellulose diacetate; polyester resins including resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resins; (meth) acrylic resins; polypropylene resins, or a mixture of one or more of these resins. The protective film 11 may contain a light selective absorber described later. It should be noted that the light selective absorber contained in the protective film 11 is retained in the protective film 11, so it is not easy to move to the polarizer.
[0062] A hard coating layer can be formed on the protective film 11. The hard coating layer can be formed on one side of the protective film 11 or on both sides. By providing a hard coating layer, a protective film 11 with improved hardness and scratch resistance can be made. The hard coating layer can be, for example, a cured layer of an acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, an amide resin, an epoxy resin, etc. In order to increase the strength, the hard coating layer can contain additives. The additives are not limited, and inorganic particles, organic particles, or mixtures thereof can be cited. The hard coating layer is, for example, a cured layer of an ultraviolet curable resin. As ultraviolet curable resins, for example, acrylic resins, silicone resins, polyester resins, polyurethane resins, amide resins, epoxy resins, etc. can be cited.
[0063] The thickness of the protective film is usually 1 to 100 μm, and is preferably 5 to 80 μm, more preferably 8 to 60 μm, and even more preferably 12 to 45 μm from the viewpoint of strength, handling properties, and the like.
[0064] The resin film as the protective film 11 is bonded to the polarizer 10 via, for example, an adhesive layer. As the adhesive forming the adhesive layer, water-based adhesives, active energy ray-curable adhesives, or thermosetting adhesives can be cited, preferably water-based adhesives and active energy ray-curable adhesives. The two opposing surfaces bonded via the adhesive layer may be subjected to corona treatment, plasma treatment, flame treatment, etc. in advance, and may have a primer layer, etc.
[0065] [Light selectively absorbing adhesive layer]
[0066] The light selectively absorbing adhesive layer 20 can be formed by dissolving or dispersing the adhesive composition in an organic solvent, applying the obtained diluted solution on a substrate and drying. As the substrate, a plastic film is preferred, and specifically, a release film subjected to a release treatment can be cited. As the release film, a release film obtained by subjecting one side of a film formed of a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, or polyarylate to a release treatment such as silicone treatment can be cited.
[0067] The thickness of the light selectively absorbing adhesive layer is, for example, 0.1 μm or more and 150 μm or less. When stacked with an image display panel, it is usually 8 μm or more and 60 μm or less. From the perspective of thinning, it is preferably 30 μm or less, more preferably 25 μm or less, and particularly preferably 20 μm or less. When stacked with other optical films, such as a λ / 4 phase difference layer, it is usually 2 μm or more and 30 μm or less, preferably 25 μm or less, more preferably 20 μm or less, and particularly preferably 18 μm or less. It is preferably 3 μm or more, and can be, for example, 10 μm or more. From the perspective of further thinning, it is preferably 10 μm or less, and particularly preferably 7 μm or less.
[0068] The absorbance of the light selectively absorbing adhesive layer at a wavelength of 410 nm is preferably 0.1 or more and 2.3 or less, and more preferably 0.2 or more and 2.0 or less. This is because by making the light selectively absorbing adhesive layer 20 have such an absorbance, the optical laminate as a whole can embody the desired light selective absorption performance, and the optical laminate as a whole can be easily constructed to be thin.
[0069] For the light selectively absorbing adhesive layer,
[0070] The absorbance at a wavelength of 390 nm is usually 5.0 or less, and may be 4.5 or less. The absorbance at a wavelength of 400 nm is usually 5.0 or less, and may be 4.5 or less. The absorbance at a wavelength of 420 nm is usually 1.00 or less, preferably 0.60 or less, more preferably 0.40 or less, and is 0.00 or more.
[0071] The absorbance at a wavelength of 430 nm is usually less than 0.20, preferably 0.18 or less, more preferably 0.10 or less, particularly preferably 0.05 or less, and is 0.00 or more.
[0072] The absorbance at a wavelength of 440 nm is usually less than 0.10, preferably 0.05 or less, and 0.00 or more.
[0073] By setting the absorbance at each wavelength to be within the above range, light in the ultraviolet region can be sufficiently absorbed and light in the visible light region can be directly transmitted.
[0074] The content of the light selective absorber per unit area of the light selectively absorbing adhesive layer is preferably 0.01 g / m 2 Above and 5g / m 2 By setting it as this range, the discoloration of the polarizing plate which occurs under high temperature and high humidity can be suppressed.
[0075] The optical layered body may be configured such that the light selectively absorbing pressure-sensitive adhesive layer 20 is provided on the outermost surface and the optical layered body is bonded to an adherend via the light selectively absorbing pressure-sensitive adhesive layer 20 .
[0076] [Adhesive composition]
[0077] The adhesive composition comprises a resin and a light selective absorber, and preferably further comprises a crosslinking agent.
[0078] The resin includes, for example, a (meth)acrylic, rubber, urethane, ester, silicone, or polyvinyl ether resin as a main component. Among them, a (meth)acrylic resin (A) as a main component is preferred.
[0079] (Light Selective Absorber)
[0080] The light selective absorber selectively absorbs light of a specific wavelength, and preferably contains a compound having at least one absorption maximum at a wavelength of 360 nm to 420 nm, and more preferably contains a compound having an absorption maximum at a wavelength of 380 nm to 410 nm.
[0081] As a light selective absorber (hereinafter sometimes referred to as light selective absorber (A)) containing a compound having an absorption maximum near a wavelength of 350 nm, for example, organic light selective absorbers such as oxybenzophenone-based light selective absorbers, benzotriazole-based light selective absorbers, salicylate-based light selective absorbers, benzophenone-based light selective absorbers, cyanoacrylate-based light selective absorbers, and triazine-based light selective absorbers can be cited. More specifically, for example, 5-chloro-2-(3,5-di-sec-butyl-2-hydroxyphenyl)-2H-benzotriazole, (2-2H-benzotriazole-2-yl)-6-(straight chain and side chain dodecyl)-4-methylphenol, 2-hydroxy-4-benzyloxybenzophenone, and 2,4-benzyloxybenzophenone can be cited. These organic light selective absorbers can be used alone or in combination of two or more. The molecular weight of the organic light selective absorber is preferably greater than 100 and less than 3000.
[0082] As the light selective absorber (A), commercially available products can be used. For example, as the triazine-based light selective absorber, there can be mentioned "Kemisorb 102" manufactured by Chemipro Kasei Co., Ltd., "Adecastab LA46" and "Adecastab LAF70" manufactured by ADEKA Co., Ltd., and "Tinuvin 109", "Tinuvin 171", "Tinuvin 234", "Tinuvin 326", "Tinuvin 327", "Tinuvin 328", "Tinuvin 928", "Tinuvin 400", "Tinuvin 460", "Tinuvin 405", and "Tinuvin 477" manufactured by BASF Japan. Examples of the benzotriazole-based light selective absorber include "Adecastab LA31" and "Adecastab LA36" manufactured by ADEKA Co., Ltd., "Sumisorb 200", "Sumisorb 250", "Sumisorb 300", "Sumisorb 340", and "Sumisorb 350" manufactured by SumikaChemtex Co., Ltd., "Kemisorb 74", "Kemisorb 79", and "Kemisorb 279" manufactured by Chemipro Kasei Co., Ltd., and "TINUVIN 99-2", "TINUVIN 900", and "TINUVIN 928" manufactured by BASF.
[0083] In addition, the light selective absorber (A) may be an inorganic light selective absorber. Examples of the inorganic light selective absorber include titanium oxide, zinc oxide, indium oxide, tin oxide, talc, kaolin, calcium carbonate, titanium oxide composite oxides, zinc oxide composite oxides, ITO (tin-doped indium oxide), ATO (antimony-doped tin oxide), etc. Examples of titanium oxide composite oxides include zinc oxide doped with silicon dioxide or aluminum oxide. These inorganic light selective absorbers may be used alone or in combination of two or more. In addition, an organic light selective absorber and an inorganic light selective absorber may be used in combination.
[0084] The light selective absorber (hereinafter sometimes referred to as light selective absorber (B)) containing a compound having an absorption maximum near a wavelength of 405 nm is preferably a compound satisfying the following formula (5), and more preferably a compound further satisfying the following formula (6).
[0085] ε(405)≥20(5)
[0086] [In formula (5), ε(405) represents the molar absorption coefficient of the compound at a wavelength of 405 nm.
[0087] The unit of gram molecular absorption coefficient is L / (g·cm).]
[0088] ε(405) / ε(440)≥20(6)
[0089] [In formula (6), ε(405) represents the molar absorption coefficient of the compound at a wavelength of 405 nm, and ε(440) represents the molar absorption coefficient at a wavelength of 440 nm.]
[0090] It should be noted that the molar absorbance coefficient was measured by the method described in the Examples.
[0091] The larger the value of ε(405), the easier it is for the compound to absorb light of 405 nm wavelength, and the more it suppresses the degradation of the optical laminate and image display device under ultraviolet light or short-wavelength visible light. When the value of ε(405) is less than 20L / (g·cm), if the content of the light selective absorber (B) in the adhesive composition is not increased, there is a tendency that it is difficult to reflect the inhibitory function of the degradation of the phase difference film and the organic EL light-emitting element caused by ultraviolet light and short-wavelength visible light. The value of ε(405) is preferably 20L / (g·cm) or more, more preferably 30L / (g·cm) or more, and further preferably 40L / (g·cm) or more, and usually 500L / (g·cm) or less.
[0092] The larger the value of ε(405) / ε(440), the less likely the compound is to hinder the color display of the image display device, and it can absorb light near 405 nm, thereby suppressing the light degradation of display devices such as retardation films and organic EL elements. The value of ε(405) / ε(440) is preferably 20 or more, more preferably 40 or more, further preferably 70 or more, and particularly preferably 80 or more.
[0093] The compound that selectively absorbs light of wavelength 405 nm is preferably a compound containing a merocyanine structure in the molecule. The molecular weight of the compound containing a merocyanine structure in the molecule is preferably 100 or more and 3000 or less. As the compound containing a merocyanine structure in the molecule, there can be mentioned: a compound containing a partial structure represented by -(NC=CC=C)- in the molecule, for example, a merocyanine compound, a cyanine compound, an indole compound, a benzotriazole compound, etc. Preferred are merocyanine compounds, phthalocyanine compounds and benzotriazole compounds, and more preferably are compounds represented by formula (I).
[0094] [Chemical formula 1]
[0095]
[0096] [Where R 1 and R 5 Each independently represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, an aralkyl group having 7 to 15 carbon atoms which may have a substituent, an aryl group having 6 to 15 carbon atoms, or a heterocyclic group, and the -CH2- contained in the alkyl group or the aralkyl group may be replaced by -NR1A-, -CO-, -SO2-, -O- or -S-.
[0097] R 1A It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0098] R 2 , R 3 and R 4 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms which may have a substituent, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent, and the -CH2- contained in the alkyl group may be replaced by -NR 1 B-, -CO-, -SO2-, -O- or -S- replacement.
[0099] R 1B It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0100] R 6 and R 7 Each independently represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms, or an electron withdrawing group, or R 6and R 7 Optionally, they are linked to each other to form a ring structure.
[0101] R 1 and R 2 Optionally linked to each other to form a ring structure, R 2 and R 3 Optionally linked to each other to form a ring structure, R 2 and R 4 Optionally linked to each other to form a ring structure, R 3 and R 6 They are optionally linked to each other to form a ring structure.]
[0102] As R 1 and R 5 Examples of the alkyl group having 1 to 25 carbon atoms include methyl, ethyl, n-propyl, isopropyl, 2-cyanopropyl, n-butyl, tert-butyl, sec-butyl, n-pentyl, n-hexyl, 1-methylbutyl, 3-methylbutyl, n-octyl, n-decyl, and 2-hexyl-octyl.
[0103] As R 1 and R 5 The substituent which the alkyl group having 1 to 25 carbon atoms represented by may have includes the groups described in the following Group A.
[0104] Group A includes: nitro, hydroxyl, carboxyl, sulfo, cyano, amino, halogen, alkoxyl having 1 to 6 carbon atoms, alkylsilyl having 1 to 12 carbon atoms, alkylcarbonyl having 2 to 8 carbon atoms, *-R a1 -(OR a2 ) t1 -R a3 (R a1 and R a2 Each independently represents a chain alkanediyl group having 1 to 6 carbon atoms, R a3 represents an alkyl group having 1 to 6 carbon atoms, and t1 represents an integer of 1 to 3. ) and the like.
[0105] Examples of the alkylsilyl group having 1 to 12 carbon atoms include monoalkylsilyl groups such as methylsilyl, ethylsilyl and propylsilyl; dialkylsilyl groups such as dimethylsilyl, diethylsilyl and methylethylsilyl; and trialkylsilyl groups such as trimethylsilyl, triethylsilyl and tripropylsilyl.
[0106] Examples of the alkylcarbonyl group having 2 to 8 carbon atoms include a methylcarbonyl group and an ethylcarbonyl group.
[0107] Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom.
[0108] As R1 and R 5 Examples of the aralkyl group having 7 to 15 carbon atoms include benzyl and phenethyl. Examples of the group in which -CH2- contained in the aralkyl group is replaced by -SO2- or -COO- include ethyl 2-phenylacetate.
[0109] As R 1 and R 5 The substituent which the aralkyl group having 7 to 15 carbon atoms represented by α-C 7 may have includes the groups described in the above group A.
[0110] As R 1 and R 5 Examples of the aryl group having 6 to 15 carbon atoms represented by include phenyl, naphthyl, anthracenyl and the like.
[0111] As R 1 and R 5 The substituent which the aryl group having 6 to 15 carbon atoms represented by may have includes the groups described in the above group A.
[0112] As R 1 and R 5 Examples of the heterocyclic group having 6 to 15 carbon atoms represented by : include aromatic heterocyclic groups having 3 to 9 carbon atoms such as pyridyl, pyrrolidinyl, quinolyl, thienyl, imidazolyl, oxazolyl, pyrrolyl, thiazolyl and furyl.
[0113] As R 1A and R 1B Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, sec-butyl, n-pentyl and n-hexyl.
[0114] As R 2 , R 3 and R 4 The alkyl group having 1 to 6 carbon atoms represented by R 1B The alkyl groups represented by these are the same as those having 1 to 6 carbon atoms.
[0115] As R 2 , R 3 and R 4 The substituent which the alkyl group having 1 to 6 carbon atoms represented by ' may have includes the groups described in the above group A.
[0116] As R 2 , R 3 and R 4 Examples of the aromatic hydrocarbon group represented by include aryl groups having 6 to 15 carbon atoms, such as phenyl, naphthyl, and anthracenyl; and aralkyl groups having 7 to 15 carbon atoms, such as benzyl and phenethyl.
[0117] As R2 , R 3 and R 4 As the substituent which the aromatic hydrocarbon group represented by may have, the groups described in the above-mentioned Group A can be mentioned.
[0118] As R 2 , R 3 and R 4 Examples of the aromatic heterocyclic ring represented by include aromatic heterocyclic groups having 3 to 9 carbon atoms such as pyridyl, pyrrolidinyl, quinolyl, thienyl, imidazolyl, oxazolyl, pyrrolyl, thiazolyl and furyl.
[0119] As R 2 , R 3 and R 4 As the substituent which the aromatic heterocyclic ring represented by is optionally embodied, the groups described in the above-mentioned Group A can be mentioned.
[0120] As R 6 and R 7 The alkyl group having 1 to 25 carbon atoms represented by R 1 and R 5 The alkyl groups represented by these are the same as those having 1 to 25 carbon atoms.
[0121] As R 6 and R 7 The substituent which the alkyl group having 1 to 25 carbon atoms represented by hereinafter may have includes the groups described in the above group A.
[0122] As R 6 and R 7 The alkyl group having 1 to 25 carbon atoms represented by R 1 and R 5 The alkyl groups represented by these are the same as those having 1 to 25 carbon atoms.
[0123] As R 6 and R 7 Examples of the electron withdrawing group represented by include a cyano group, a nitro group, a halogen atom, an alkyl group substituted with a halogen atom, and a group represented by the formula (I-1).
[0124] [Chemical formula 2]
[0125] * -X 1 -R 11 (l-1)
[0126] [Where R 11 It represents a hydrogen atom or an alkyl group having 1 to 25 carbon atoms, and at least one of the methylene groups contained in the alkyl group may be substituted with an oxygen atom.
[0127] X 1Indicates -CO-, -COO-, -OCO-, -CS-, -CSO-, -CSS-, -NR 12 CO-or-CONR 13 -.
[0128] R 12 and R 13 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group.]
[0129] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0130] Examples of the alkyl group substituted with a halogen atom include perfluoroalkyl groups such as trifluoromethyl, perfluoroethyl, perfluoropropyl, perfluoroisopropyl, perfluorobutyl, perfluorosec-butyl, perfluorotert-butyl, perfluoropentyl, and perfluorohexyl. The alkyl group substituted with a halogen atom usually has 1 to 25 carbon atoms.
[0131] R 6 and R 7 Optionally linked to each other to form a ring structure, as R 6 and R 7 Examples of the ring structure to be formed include a Michaelis acid structure, a barbituric acid structure, and a dimedone structure.
[0132] As R 11 The alkyl group having 1 to 25 carbon atoms represented by R 1 and R 5 represents the same group as the alkyl group.
[0133] As R 2 The ring structure formed by bonding R and R3 to each other includes: 2 The nitrogen-containing ring structure of the bonded nitrogen atom, for example, a 4- to 14-membered nitrogen-containing heterocyclic ring. 2 and R 3 The ring structure formed by connecting to each other may be a monocyclic ring or a polycyclic ring, and specifically, pyrrolidine ring, pyrroline ring, imidazolidine ring, imidazolidine ring, oxazoline ring, thiazoline ring, piperidine ring, morpholine ring, piperazine ring, indole ring, isoindole ring, etc. may be mentioned.
[0134] As R 1 and R 2 The ring structure formed by bonding to each other includes: 1 and R 2 The nitrogen-containing ring structure of the nitrogen atom to which it is bonded is, for example, a 4- to 14-membered (preferably 4- to 8-membered) nitrogen-containing heterocyclic ring. 1 and R 2 The ring structure formed by connecting with each other may be a single ring or a polycyclic ring. 2and R 3 The ring structures formed by connecting to each other are the same ring structures.
[0135] As R 2 and R 4 The ring structure formed by mutually bonding includes a 4- to 14-membered nitrogen-containing ring structure, and preferably a 5- to 9-membered nitrogen-containing ring structure. 2 and R 4 The ring structure formed by the mutual bonding may be a monocyclic ring or a polycyclic ring. These rings may optionally have a substituent, and examples of such a ring structure include the following: 2 and R 3 The ring structure formed is the same ring structure as the ring structure exemplified.
[0136] As R 3 and R 6 The ring structure formed by connecting to each other includes R 3 -C=CC=CR 6 The ring structure forming the skeleton of the ring includes, for example, phenyl and the like.
[0137] As R 2 With R 3 The compound represented by formula (I) which is linked to each other to form a ring structure includes a compound represented by formula (IA), as R 2 and R 4 Examples of the compound represented by the formula (I) that are linked to each other to form a ring structure include the compound represented by the formula (IB).
[0138] [Chemical formula 3]
[0139]
[0140] [In formula (IA) and formula (IB), R 1 , R 3 , R 4 , R 5 , R 6 and R 7 Each has the same meaning as above.
[0141] Ring W 1 And Ring W 2 Each independently represents a nitrogen-containing ring.]
[0142] Ring W 1 And Ring W 2 represents a nitrogen-containing ring containing a nitrogen atom as a ring constituent unit. 1 And Ring W 2 Each ring may be independently a monocyclic ring or a polycyclic ring, and may contain a heteroatom other than nitrogen as a ring constituent unit.1 And Ring W 2 Each independently is preferably a 5- to 9-membered ring.
[0143] The compound represented by formula (IA) is preferably a compound represented by formula (IA-1).
[0144] [Chemical formula 4]
[0145]
[0146] [In formula (IA-1), R 1 , R 4 , R 5 , R 6 and R 7 Each has the same meaning as above.
[0147] A 1 Represents -CH2-, -O-, -S- or -NR 1 D-.
[0148] R 14 and R 15 Each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.
[0149] R 1D represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.]
[0150] The compound represented by formula (IB) is preferably a compound represented by formula (IB-1) or a compound represented by formula (IB-2).
[0151] [Chemical formula 5]
[0152]
[0153] [In formula (IB-1), R 1 , R 6 and R 7 Each has the same meaning as above.
[0154] R 16 Each independently represents a hydrogen atom, an alkyl group or an aryl group having 1 to 12 carbon atoms.]
[0155] [Chemical formula 6]
[0156]
[0157] [In formula (IB-2), R 3 , R 5 , R 6 and R 7 Each has the same meaning as above.
[0158] R 30 It represents a hydrogen atom, a cyano group, a nitro group, a halogen atom, a mercapto group, an amino group, an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aromatic hydrocarbon group having 6 to 18 carbon atoms, an acyl group having 2 to 13 carbon atoms, an acyloxy group having 2 to 13 carbon atoms, or an alkoxycarbonyl group having 2 to 13 carbon atoms.
[0159] R 31 represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a mercapto group, an alkylthio group having 1 to 12 carbon atoms, an amino group or a heterocyclic group which may have a substituent.]
[0160] As R 30 Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0161] As R 30 R 30 Examples of the acyl group having 2 to 13 carbon atoms represented by include acetyl, propionyl and butyryl.
[0162] As R 30 Examples of the acyloxy group having 2 to 13 carbon atoms include methylcarbonyloxy, ethylcarbonyloxy, propylcarbonyloxy, and butylcarbonyloxy.
[0163] As R 30 Examples of the alkoxycarbonyl group having 2 to 13 carbon atoms include methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl and butoxycarbonyl.
[0164] As R 30 The aromatic hydrocarbon group having 6 to 18 carbon atoms represented by ' includes aryl groups having 6 to 18 carbon atoms such as phenyl, naphthyl and biphenyl; and aralkyl groups having 7 to 18 carbon atoms such as benzyl and phenethyl.
[0165] As R 30 The alkyl group having 1 to 12 carbon atoms represented by 14 The alkyl groups represented by these are the same as those of the alkyl groups having 1 to 12 carbon atoms.
[0166] As R 30 Examples of the alkyl group having 1 to 12 carbon atoms include methoxy, ethoxy, propoxy, butoxy, and pentyloxy.
[0167] R 30 Preferred is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an amino group, or a mercapto group.
[0168] As R 31 The alkyl group having 1 to 12 carbon atoms represented by 14The alkyl groups represented by these are the same as those of the alkyl groups having 1 to 12 carbon atoms.
[0169] As R 31 The alkoxy group having 1 to 12 carbon atoms represented by 30 The alkoxy groups having 1 to 12 carbon atoms are the same as those represented by the above.
[0170] As R 31 Examples of the alkylthio group having 1 to 12 carbon atoms include methylthio, ethylthio, propylthio, butylthio, pentylthio and hexylthio.
[0171] As R 31 The amino group which may be substituted includes amino group; amino group substituted with one alkyl group having 1 to 8 carbon atoms such as N-methylamino and N-ethylamino; amino group substituted with two alkyl groups having 1 to 8 carbon atoms such as N,N-dimethylamino, N,N-diethylamino and N,N-methylethylamino; etc.
[0172] As R 31 Examples of the heterocyclic ring represented by include nitrogen-containing heterocyclic groups having 4 to 9 carbon atoms, such as pyrrolidinyl, piperidinyl and morpholinyl.
[0173] As R 3 and R 6 are linked to each other to form a ring structure, and R 2 and R 4 Examples of the compound represented by formula (I) that are mutually bonded to form a ring structure include a compound represented by formula (IC).
[0174] [Chemical formula 7]
[0175]
[0176] [In formula (IC), R 1 , R 6 and R 7 Means the same as above.
[0177] R 21 , R 22 Each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a hydroxyl group.
[0178] X 2 and X 3 Each independently represents -CH2- or -N(R 25 )=.
[0179] R 25 represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms, or an aromatic hydrocarbon group which may have a substituent.]
[0180] As R25 The alkyl group having 1 to 25 carbon atoms represented by R 1 The alkyl groups represented by these are the same as those having 1 to 25 carbon atoms.
[0181] As R 25 The aromatic hydrocarbon group represented by may be aryl groups such as phenyl and naphthyl; aralkyl groups such as benzyl and phenethyl; biphenyl groups, etc., and preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms. 25 Examples of the substituent that the aromatic hydrocarbon group represented by may have include a hydroxyl group and the like.
[0182] R 3 and R 6 Each is independently preferably an electron withdrawing group.
[0183] As R 1 and R 2 are linked to each other to form a ring structure, and R 3 and R 6 Examples of the compound represented by formula (I) that are mutually bonded to form a ring structure include compounds represented by formula (ID).
[0184] [Chemical formula 8]
[0185]
[0186] [In formula (ID), R 4 , R 5 , R 7 Means the same as above.
[0187] R 25 , R 26 , R 27 and R 28 Each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, a hydroxyl group, or an aralkyl group.]
[0188] As R 25 , R 26 , R 27 and R 28 The alkyl group having 1 to 12 carbon atoms represented by 1A and R 1B The same group as the alkyl group having 1 to 12 carbon atoms represented by R 25 , R 26 , R 27 and R 28 The substituent which the alkyl group having 1 to 12 carbon atoms represented by hereinafter may have is exemplified by a hydroxyl group.
[0189] As R 25 , R 26 , R27 and R 28 The aralkyl group represented by includes aralkyl groups having 7 to 15 carbon atoms such as benzyl and phenethyl.
[0190] As R 6 and R 7 Examples of the compound (I) that is linked to each other to form a ring structure include compounds represented by formula (IE).
[0191] [Chemical formula 9]
[0192]
[0193] [In formula (IE), R 1 , R 2 , R 3 , R 4 , R 5 Each has the same meaning as above.
[0194] Ring W 3 represents a cyclic compound]
[0195] Ring W 3 The ring is a 5- to 9-membered ring, and may contain a hetero atom such as a nitrogen atom, an oxygen atom, or a sulfur atom as a ring constituent unit.
[0196] The compound represented by formula (IE) is preferably a compound represented by formula (IE-1).
[0197] [Chemical formula 10]
[0198]
[0199] [In formula (IE-1), R 1 , R 2 , R 3 and R 5 Each has the same meaning as above.
[0200] R 17 , R 18 , R 19 , R q Each independently represents a hydrogen atom or an alkyl group, aralkyl group or aryl group having 1 to 12 carbon atoms which may have a substituent, wherein the -CH2- group contained in the alkyl group or aralkyl group may be replaced by -NR 1D -, -C(=O)-, -C(=S)-, -O-, -S-, R 17 and R 18 Optionally linked to each other to form a ring structure, R 18 and R 19 Optionally linked to each other to form a ring structure, R 19 and Rq They are optionally linked to each other to form a ring structure. m, p, and q each independently represent an integer of 0 to 3.]
[0201] Examples of the compound represented by formula (I) include the following compounds.
[0202] [Chemical formula 11]
[0203]
[0204] [Chemical formula 12]
[0205]
[0206]
[0207] [Chemical formula 13]
[0208]
[0209] [Chemical formula 14]
[0210]
[0211] [Chemical formula 15]
[0212]
[0213] [Chemical formula 16]
[0214]
[0215] [Chemical formula 17]
[0216]
[0217] [Chemical formula 18]
[0218]
[0219] [Chemical formula 19]
[0220]
[0221] [Chemical formula 20]
[0222]
[0223] The total content of the light selective absorber is not limited as long as it is selected so that the absorbance of the adhesive layer at a wavelength of 410 nm is greater than 0.1 and less than 2.3. In the adhesive composition, for example, it is 0.01 to 20 parts by mass, preferably 0.05 to 15 parts by mass, and more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the total resin components.
[0224] The mass ratio of the light selective absorber (A) to the light selective absorber (B) (light selective absorber (A) / light selective absorber (B)) is usually 0.05-20, preferably 0.1-10.
[0225] ((Meth)acrylic resin (A))
[0226] The (meth)acrylic resin (A) is preferably a polymer having a structural unit derived from (meth)acrylate as a main component (preferably containing 50% by mass or more). The structural unit derived from (meth)acrylate may include one or more structural units derived from monomers other than (meth)acrylate (for example, structural units derived from monomers having polar functional groups). It should be noted that in this specification, (meth)acrylic acid refers to any substance of acrylic acid or methacrylic acid, and "(meth)" when referred to as (meth)acrylate, etc., also has the same purpose.
[0227] As the (meth)acrylate, there can be mentioned (meth)acrylates represented by the following formula (X).
[0228] [Chemical formula 21]
[0229]
[0230] [In formula (X), R 101 represents a hydrogen atom or a methyl group, R 102 represents an alkyl group having 1 to 14 carbon atoms or an aralkyl group having 7 to 20 carbon atoms, wherein the hydrogen atoms of the alkyl group or the aralkyl group may be substituted with an alkoxy group having 1 to 10 carbon atoms.]
[0231] In formula (X), R 102 An alkyl group having 1 to 14 carbon atoms is preferred, and an alkyl group having 1 to 8 carbon atoms is more preferred.
[0232] Examples of the (meth)acrylate represented by formula (X) include:
[0233] Straight-chain alkyl esters of (meth)acrylic acid such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, etc.;
[0234] Branched-chain alkyl (meth)acrylates such as isopropyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isopentyl (meth)acrylate, isohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isostearyl (meth)acrylate, and isopentyl (meth)acrylate;
[0235] Alkyl esters of (meth)acrylic acid containing an alicyclic skeleton, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentyl (meth)acrylate, cyclododecyl (meth)acrylate, methylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, and α-ethoxycyclohexyl acrylate;
[0236] (Meth)acrylic acid esters containing an aromatic ring skeleton, such as phenyl (meth)acrylate;
[0237] etc.
[0238] In addition, substituted alkyl (meth)acrylates in which a substituent is introduced into the alkyl group in the alkyl (meth)acrylate can also be mentioned. The substituent of the substituted alkyl (meth)acrylate is a group that replaces the hydrogen atom of the alkyl group, and specific examples thereof include phenyl, alkoxy, and phenoxy. As substituted alkyl (meth)acrylates, specifically, 2-methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-(2-phenoxyethoxy)ethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypoly (ethylene glycol) (meth)acrylate, etc. can be mentioned.
[0239] These (meth)acrylates may be used alone or in combination of two or more.
[0240] The (meth)acrylic resin (A) preferably contains a structural unit derived from an alkyl acrylate (a1) having a homopolymer glass transition temperature Tg of less than 0°C, and a structural unit derived from an alkyl acrylate (a2) having a homopolymer Tg of 0°C or more. The structural unit derived from the alkyl acrylate (a1) and the structural unit derived from the alkyl acrylate (a2) are advantageous in improving the high temperature durability of the adhesive layer. The Tg of the homopolymer of the alkyl (meth)acrylate can be, for example, a value in literature such as POLYMER HANDBOOK (Wiley-Interscience).
[0241] Specific examples of the alkyl acrylate (a1) include alkyl acrylates having an alkyl group with about 2 to 12 carbon atoms, such as ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, n-hexyl acrylate, isohexyl acrylate, n-heptyl acrylate, n-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, n-nonyl acrylate, isononyl acrylate, n-decyl acrylate, isodecyl acrylate and n-dodecyl acrylate.
[0242] The alkyl acrylate (a1) may be used alone or in combination of two or more. Among them, n-butyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, etc. are preferred from the viewpoint of followability and reworkability when the adhesive layer of the present invention is laminated to an optical laminate.
[0243] The alkyl acrylate (a2) is an alkyl acrylate other than the alkyl acrylate (a1). Specific examples of the alkyl acrylate (a2) include methyl acrylate, cyclohexyl acrylate, isobornyl acrylate, stearyl acrylate, t-butyl acrylate, and the like.
[0244] The alkyl acrylate (a2) may be used alone or in combination of two or more. From the viewpoint of high temperature durability, the alkyl acrylate (a2) preferably includes methyl acrylate, cyclohexyl acrylate, isobornyl acrylate, etc., and more preferably includes methyl acrylate.
[0245] Of all the structural units contained in the (meth)acrylic resin, the structural unit derived from the (meth)acrylate represented by formula (I) preferably accounts for 50% by mass or more, preferably 60 to 95% by mass, and more preferably 65 to 95% by mass or more.
[0246] As the structural unit derived from the monomer other than (meth)acrylate, the structural unit derived from the monomer having a polar functional group is preferred, and the structural unit derived from the (meth)acrylate having a polar functional group is more preferred. Examples of the polar functional group include hydroxyl, carboxyl, substituted or unsubstituted amino, heterocyclic groups such as epoxy, and the like.
[0247] Examples of the monomer having a polar functional group include:
[0248] 1-Hydroxymethyl (meth)acrylate, 1-hydroxyethyl (meth)acrylate, 1-hydroxyheptyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 1-hydroxypentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxypentyl (meth)acrylate, 2-hydroxyhexyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 3-hydroxypentyl (meth)acrylate, 3-hydroxyhexyl (meth)acrylate, 3-hydroxyheptyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxypentyl (meth)acrylate, 4 4-Hydroxyhexyl (meth)acrylate, 4-hydroxyheptyl (meth)acrylate, 4-hydroxyoctyl (meth)acrylate, 2-chloro-2-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 5-hydroxyhexyl (meth)acrylate, 5-hydroxyheptyl (meth)acrylate, 5-hydroxyoctyl (meth)acrylate, 5-hydroxynonyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 6-hydroxyheptyl (meth)acrylate, 6-hydroxyoctyl (meth)acrylate, 6-hydroxynonyl (meth)acrylate, 6-hydroxydecyl (meth)acrylate, 7-hydroxyheptyl (meth)acrylate, 7-hydroxyoctyl (meth)acrylate, 7-hydroxynonyl (meth)acrylate, 7-hydroxydecyl (meth)acrylate, 7-hydroxyundecyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 8-hydroxynonyl (meth)acrylate, 8-hydroxydecyl (meth)acrylate, 8-hydroxyundecyl (meth)acrylate, 8-hydroxydodecyl (meth)acrylate, 9-hydroxynonyl (meth)acrylate, 9-hydroxydecyl (meth)acrylate, 9-hydroxyundecyl (meth)acrylate, 9-hydroxydodecyl (meth)acrylate, 9-hydroxytridecyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 10-hydroxyundecyl (meth)acrylate, 10-hydroxydodecyl (meth)acrylate, 10-hydroxytridecyl (meth)acrylate, 10-hydroxytetradecyl (meth)acrylate, 11-hydroxyundecyl (meth)acrylate, 11-hydroxydodecyl (meth)acrylate, 11-hydroxytridecyl (meth)acrylate, 11-hydroxytetradecyl (meth)acrylate, 11-hydroxypentadecyl (meth)acrylate, 12-hydroxydodecyl (meth)acrylate, 12-hydroxytridecyl (meth)acrylate, 12-hydroxytetradecyl (meth)acrylate, 13-hydroxypentadecyl (meth)acrylate, 13-hydroxytetradecyl (meth)acrylate, 13-hydroxypentadecyl (meth)acrylate,A monomer having a hydroxyl group, such as 14-hydroxytetradecyl (meth)acrylate, 14-hydroxypentadecyl (meth)acrylate, 15-hydroxypentadecyl (meth)acrylate, or 15-hydroxyheptadecyl (meth)acrylate;
[0249] Monomers having a carboxyl group, such as (meth)acrylic acid, carboxyalkyl (meth)acrylate (e.g., carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate), maleic acid, maleic anhydride, fumaric acid, and crotonic acid;
[0250] Monomers having a heterocyclic group such as acryloylmorpholine, vinylcaprolactam, N-vinyl-2-pyrrolidone, vinylpyridine, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, glycidyl (meth)acrylate, and 2,5-dihydrofuran;
[0251] A monomer having a substituted or unsubstituted amino group, such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylate.
[0252] Among them, from the viewpoint of the reactivity between the (meth)acrylate polymer and the crosslinking agent, a monomer having a hydroxyl group and / or a monomer having a carboxyl group is preferred, and a monomer containing both a monomer having a hydroxyl group and a monomer having a carboxyl group is more preferred.
[0253] As the monomer having a hydroxyl group, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 5-hydroxypentyl acrylate, and 6-hydroxyhexyl acrylate are preferred. In particular, good durability can be obtained by using 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, and 5-hydroxypentyl acrylate.
[0254] As the monomer having a carboxyl group, acrylic acid is preferably used.
[0255] From the viewpoint of preventing excessive peeling force of a separator film (Japanese: セパレートフィルム) that can be laminated on the outer surface of the adhesive layer, the (meth) acrylic resin (A) preferably does not substantially contain a structural unit derived from a monomer having an amino group. Here, substantially not containing means that the amount is 0.1 parts by mass or less in 100 parts by mass of all the structural units constituting the (meth) acrylic resin (a).
[0256] The content of the structural unit derived from the monomer having a polar functional group is preferably 20 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, further preferably 0.5 parts by mass or more and 10 parts by mass or less, particularly preferably 1 part by mass or more and 7 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic resin (A).
[0257] The content of the structural unit derived from the monomer having an aromatic group is preferably 20 parts by mass or less, more preferably 4 parts by mass or more and 20 parts by mass or less, and further preferably 4 parts by mass or more and 16 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic resin (A).
[0258] Examples of the structural unit derived from a monomer other than a (meth)acrylate include a structural unit derived from a styrene-based monomer, a structural unit derived from a vinyl-based monomer, a structural unit derived from a monomer having a plurality of (meth)acryloyl groups in the molecule, and a structural unit derived from a (meth)acrylamide-based monomer.
[0259] Examples of the styrene monomer include styrene; alkyl styrenes such as methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, diethylstyrene, triethylstyrene, propylstyrene, butylstyrene, hexylstyrene, heptylstyrene, and octylstyrene; halogenated styrenes such as fluorostyrene, chlorostyrene, bromostyrene, dibromostyrene, and iodostyrene; nitrostyrene; acetylstyrene; methoxystyrene; and divinylbenzene.
[0260] Examples of the vinyl monomers include: fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, and vinyl laurate; halogenated vinyl compounds such as vinyl chloride and vinyl bromide; vinylidene halides such as vinylidene chloride; nitrogen-containing heterocyclic aromatic vinyl compounds such as vinyl pyridine, vinyl pyrrolidone, and vinyl carbazole; conjugated dienes such as butadiene, isoprene, and chloroprene; and unsaturated nitriles such as acrylonitrile and methacrylonitrile.
[0261] Examples of monomers having multiple (meth)acryloyl groups in the molecule include: monomers having two (meth)acryloyl groups in the molecule, such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; and monomers having three (meth)acryloyl groups in the molecule, such as trimethylolpropane tri(meth)acrylate.
[0262] Examples of the (meth)acrylamide monomer include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, N-(5-hydroxypentyl) (meth)acrylamide, N-(6-hydroxyhexyl) (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-(3-dimethylaminopropyl) (meth)acrylamide, N-(1,1-dimethyl-3-oxobutyl) (meth)acrylamide, N-[2-(2-oxo-1-imidazolidinyl)ethyl] (meth)acrylamide, 2-acrylamido-2-methyl-1-propanesulfonic acid, N-(methoxymethyl)acrylamide, N-(ethoxymethyl) (meth)acrylamide, N-(propoxy (methyl) (meth) acrylamide, N-(1-methylethoxymethyl) (meth) acrylamide, N-(1-methylpropoxymethyl) (meth) acrylamide, N-(2-methylpropoxymethyl) (meth) acrylamide, N-(butoxymethyl) (meth) acrylamide, N-(1,1-dimethylethoxymethyl) (meth) acrylamide, N-(2-methoxyethyl) (meth) acrylamide, N-(2-ethoxyethyl) (meth) acrylamide, N-(2-propoxyethyl) (meth) acrylamide, N-[2-(1-methylethoxy)ethyl] (meth) acrylamide, N-[2-(1-methylpropoxy)ethyl] (meth) acrylamide, N-[2-(2-methylpropoxy)ethyl] (meth) acrylamide, N-(2-butoxyethyl) (meth) acrylamide, N-[2-(1,1-dimethylethoxy)ethyl] (meth) acrylamide, and the like. Among them, N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propoxymethyl)acrylamide, N-(butoxymethyl)acrylamide, and N-(2-methylpropoxymethyl)acrylamide are preferred.
[0263] The weight average molecular weight (Mw) of (meth) acrylic resin (A) is preferably 500,000 to 2.5 million. If the weight average molecular weight is 500,000 or more, the durability of the adhesive layer in a high temperature environment is improved, and it is easy to suppress the undesirable conditions such as floating peeling between the adherend and the adhesive layer and the cohesive failure of the adhesive layer. If the weight average molecular weight is 2.5 million or less, it is advantageous from the viewpoint of coating. From the viewpoint of taking into account the durability of the adhesive layer and the coating of the adhesive composition, the weight average molecular weight is preferably 600,000 to 1.8 million, more preferably 700,000 to 1.7 million, and particularly preferably 1 million to 1.6 million. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is generally 2 to 10, preferably 3 to 8, and more preferably 3 to 6. The weight average molecular weight can be analyzed by gel permeation chromatography and is a value converted to standard polystyrene.
[0264] When the (meth)acrylic resin (A) is dissolved in ethyl acetate to prepare a solution having a concentration of 20% by mass, the viscosity at 25° C. is preferably 20 Pa·s or less, more preferably 0.1 to 15 Pa·s. If the viscosity is within this range, it is advantageous from the perspective of coating properties when the adhesive composition is applied to a substrate. It should be noted that the viscosity can be measured by a Brookfield viscometer.
[0265] The glass transition temperature (Tg) of the (meth)acrylic resin (A) is, for example, -60 to 20°C, preferably -50 to 15°C, more preferably -45 to 10°C, and particularly -40 to 0°C. If Tg is below the upper limit, it is beneficial to improve the wettability of the adhesive layer to the adherend substrate, and if it is above the lower limit, it is beneficial to improve the durability of the adhesive layer. It should be noted that the glass transition temperature can be measured by a differential scanning calorimeter (DSC).
[0266] The (meth)acrylic resin (A) can be produced by known methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization, and solution polymerization is particularly preferred. As a solution polymerization method, for example, a method of mixing a monomer and an organic solvent, adding a thermal polymerization initiator under a nitrogen atmosphere, and stirring for about 3 to 15 hours at a temperature of 40 to 90° C., preferably about 50 to 80° C. can be mentioned. In order to control the reaction, the monomer and the thermal polymerization initiator can be added continuously or intermittently during the polymerization. The monomer and the thermal initiator can be added in an organic solvent.
[0267] As the polymerization initiator, a thermal polymerization initiator, a photopolymerization initiator, etc. can be used. As the photopolymerization initiator, 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, etc. can be mentioned. Examples of the thermal polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), 2,2'-azobis(2-methylpropionic acid)dimethyl ester, and 2,2'-azobis(2-hydroxymethylpropionitrile); organic peroxides such as lauryl peroxide, tert-butyl hydroperoxide, benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, dipropyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, and (3,5,5-trimethylhexanoyl) peroxide; and inorganic peroxides such as potassium persulfate, ammonium persulfate, and hydrogen peroxide. Furthermore, a redox initiator using a peroxide and a reducing agent in combination may be used.
[0268] The ratio of the polymerization initiator is about 0.001 to 5 parts by mass based on 100 parts by mass of the total amount of monomers constituting the (meth)acrylic resin (A). The (meth)acrylic resin can be polymerized by a polymerization method using active energy rays (eg, ultraviolet rays).
[0269] Examples of the organic solvent include aromatic hydrocarbons such as toluene and xylene; esters such as ethyl acetate and butyl acetate; aliphatic alcohols such as propanol and isopropanol; and ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone.
[0270] The content of the (meth)acrylic resin (A) in 100% by mass of the pressure-sensitive adhesive composition is usually 60% to 99.9% by mass, preferably 70% to 99.5% by mass, and more preferably 80% to 99% by mass.
[0271] The crosslinking agent (B) reacts with polar functional groups (e.g., hydroxyl, amino, carboxyl, heterocyclic, etc.) in the (meth)acrylic resin (A). The crosslinking agent (B) forms a crosslinked structure with the (meth)acrylic resin, etc., which is advantageous for durability and reprocessability.
[0272] Examples of the crosslinking agent (B) include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, metal chelate crosslinking agents, and the like. In particular, isocyanate crosslinking agents are preferred from the viewpoints of the pot life of the adhesive composition, the durability of the adhesive layer, the crosslinking rate, and the like.
[0273] The isocyanate compound is preferably a compound having at least two isocyanate groups (-NCO) in the molecule, and examples thereof include aliphatic isocyanate compounds (e.g., hexamethylene diisocyanate, etc.), alicyclic isocyanate compounds (e.g., isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate), aromatic isocyanate compounds (e.g., toluene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, etc.), and the like. In addition, the crosslinking agent (B) may be an adduct (adduct) of the above-mentioned isocyanate compound based on a polyol compound [e.g., an adduct obtained by using glycerol, trimethylolpropane, etc.], an isocyanurate, a biuret-type compound, and a derivative such as an isocyanate compound of a urethane prepolymer type obtained by addition reaction with polyether polyol, polyester polyol, acrylic polyol, polybutadiene polyol, polyisoprene polyol, etc. The crosslinking agent (B) may be used alone or in combination of two or more. Among these, representative examples include: aromatic isocyanate compounds (e.g., toluene diisocyanate, xylene diisocyanate), aliphatic isocyanate compounds (e.g., hexamethylene diisocyanate), or their adducts based on polyol compounds (e.g., glycerol, trimethylolpropane), or isocyanurates. This is probably because if the crosslinking agent (B) is an aromatic isocyanate compound and / or its adduct based on a polyol compound or isocyanurate, it is conducive to forming an optimal crosslinking density (or crosslinking structure), which can improve the durability of the adhesive layer. In particular, if it is a toluene diisocyanate compound and / or its adduct based on a polyol compound, the durability can be improved even when the adhesive layer is applied to a polarizing plate.
[0274] The content of the crosslinking agent (B) is usually 0.01 to 15 parts by mass, preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin (A).
[0275] The adhesive composition forming the light selectively absorbing adhesive layer of the present invention may further contain a silane compound (D).
[0276] Examples of the silane compound (D) include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxypropylethoxydimethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.
[0277] The silane compound (D) may be a silicone oligomer. Specific examples of the silicone oligomer are as follows, if shown as a combination of monomers.
[0278] 3-mercaptopropyltrimethoxysilane-tetramethoxysilane oligomer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane oligomer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane oligomer, 3-mercaptopropyltriethoxysilane-tetraethoxysilane oligomer and the like mercaptopropyl group-containing oligomers; mercaptomethyltrimethoxysilane-tetramethoxysilane oligomer, mercaptomethyltrimethoxysilane-tetraethoxysilane oligomer, mercaptomethyltriethoxysilane-tetramethoxysilane oligomer, mercaptomethyltriethoxysilane-tetraethoxysilane oligomer and the like mercaptomethyl group-containing oligomers; 3-glycidyloxypropyltrimethoxysilane-tetramethoxysilane copolymer, 3-glycidyloxypropyltrimethoxysilane-tetramethoxysilane copolymer Copolymers containing 3-glycidoxypropyl groups such as oxypropyltrimethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropyltriethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropyltriethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropylmethyldiethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropylmethyldiethoxysilane-tetraethoxysilane copolymer; 3-methacryloxypropyltrimethoxysilane Oligomers containing a methacryloxypropyl group, such as 3-methacryloxypropyl trimethoxysilane-tetraethoxysilane oligomer, 3-methacryloxypropyl triethoxysilane-tetramethoxysilane oligomer, 3-methacryloxypropyl triethoxysilane-tetraethoxysilane oligomer, 3-methacryloxypropyl methyldimethoxysilane-tetramethoxysilane oligomer, 3-methacryloxypropyl methyldimethoxysilane-tetraethoxysilane oligomer, 3-methacryloxypropyl methyldiethoxysilane-tetramethoxysilane oligomer, and 3-methacryloxypropyl methyldiethoxysilane-tetraethoxysilane oligomer ; 3-acryloxypropyl trimethoxysilane-tetramethoxysilane oligomer, 3-acryloxypropyl trimethoxysilane-tetraethoxysilane oligomer, 3-acryloxypropyl triethoxysilane-tetramethoxysilane oligomer, 3-acryloxypropyl triethoxysilane-tetraethoxysilane oligomer, 3-acryloxypropyl methyl dimethoxysilane-tetramethoxysilane oligomer, 3-acryloxypropyl methyl dimethoxysilane-tetraethoxysilane oligomer, 3-acryloxypropyl methyl diethoxysilane-tetramethoxysilane oligomer, 3-acryloxypropyl methyl diethoxysilane-tetraethoxysilane oligomer and other oligomers containing acryloxypropyl groups;Oligomers containing vinyl groups, such as vinyl trimethoxysilane-tetramethoxysilane oligomers, vinyl trimethoxysilane-tetraethoxysilane oligomers, vinyl triethoxysilane-tetramethoxysilane oligomers, vinyl triethoxysilane-tetraethoxysilane oligomers, vinyl methyl dimethoxysilane-tetramethoxysilane oligomers, vinyl methyl dimethoxysilane-tetraethoxysilane oligomers, vinyl methyl diethoxysilane-tetramethoxysilane oligomers, and vinyl methyl diethoxysilane-tetraethoxysilane oligomers; 3-aminopropyl trimethoxysilane - Copolymers containing amino groups such as tetramethoxysilane copolymers, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymers, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymers, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymers, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymers, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymers, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymers, and 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymers. ;
[0279] The silane compound (D) may be a silane compound represented by the following formula (d1). If the adhesive composition contains a silane compound represented by the following formula (d1), the adhesion to the substrate, glass, transparent electrode, etc. can be further improved, thereby forming a durable adhesive layer that is not prone to floating, peeling, foaming, etc. in a high temperature environment.
[0280] [Chemical formula 22]
[0281]
[0282] (wherein, B represents a chain alkane diyl group having 1 to 20 carbon atoms or a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, wherein -CH2- constituting the chain alkane diyl group and the alicyclic hydrocarbon group may be substituted with -O- or -CO-, and R d7 represents an alkyl group having 1 to 5 carbon atoms, R d8 , R d9 , R d10 , R d11 and R d12 Each independently represents an alkyl group having 1 to 5 carbon atoms or an alkoxy group having 1 to 5 carbon atoms)
[0283] In formula (d1), B represents a chain alkane diyl group having 1 to 20 carbon atoms, such as methylene, ethylene, trimethylene, tetramethylene, hexamethylene, heptamethylene, octamethylene, etc.; a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, such as cyclobutylene (e.g., 1,2-cyclobutylene), cyclopentylene (e.g., 1,2-cyclopentylene), cyclohexylene (e.g., 1,2-cyclohexylene), cyclooctylene (e.g., 1,2-cyclooctylene), or a group in which -CH2- constituting these chain alkane diyl groups and the above-mentioned alicyclic hydrocarbon groups is substituted with -O- or -CO-. Preferably, B is a chain alkane diyl group having 1 to 10 carbon atoms. Rd7 represents an alkyl group having 1 to 5 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl, etc., and R d8 , R d9 , R d10 , R d11 and R d12 Each independently represents the above R 21 The alkyl group having 1 to 5 carbon atoms as exemplified in the above, or an alkoxy group having 1 to 5 carbon atoms such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, sec-butoxy, tert-butoxy, etc. d8 , R d9 , R d10 , R d11 and R d12 Each independently represents an alkoxy group having 1 to 5 carbon atoms. These silane compounds (D) can be used alone or in combination of two or more.
[0284] Specific examples of the silane compound represented by the formula (d1) include (trimethoxysilyl)methane, 1,2-bis(trimethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,3-bis(trimethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,5-bis(triethoxysilyl)pentane, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,6-bis(tripropoxysilyl)hexane, 1,8-bis(trimethoxysilyl)octane, 1,8-bis(triethoxysilyl)octane, 1,8-bis(tripropoxysilyl)octane and other bis(triC1 -5 alkoxysilyl) C1-10 alkanes; bis(dimethoxymethylsilyl)methane, 1,2-bis(dimethoxymethylsilyl)ethane, 1,2-bis(dimethoxyethylsilyl)ethane, 1,4-bis(dimethoxymethylsilyl)butane, 1,4-bis(dimethoxyethylsilyl)butane, 1,6-bis(dimethoxymethylsilyl)hexane, 1,6-bis(dimethoxyethylsilyl) C1-10 alkanes such as bis(di-C1-5 alkoxy-di-C1-5 alkylsilyl)C1-10 alkanes such as 1,6-bis(methoxydimethylsilyl)hexane and 1,8-bis(methoxydimethylsilyl)octane; and the like. Among these, preferred are bis(triC1-3 alkoxysilyl)C1-10 alkanes such as 1,2-bis(trimethoxysilyl)ethane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,6-bis(trimethoxysilyl)hexane, and 1,8-bis(trimethoxysilyl)octane, and particularly preferred are 1,6-bis(trimethoxysilyl)hexane and 1,8-bis(trimethoxysilyl)octane.
[0285] The content of the silane compound (D) is usually 0.01 to 10 parts by mass, preferably 0.03 to 5 parts by mass, more preferably 0.05 to 2 parts by mass, and further preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the (meth) acrylic resin (A). If it is below the above upper limit, it is beneficial to suppress the silane compound (A) from seeping out of the adhesive layer, and if it is above the above lower limit, it is easy to improve the adhesion (or adhesion) of the adhesive layer, the metal layer, the glass substrate, etc., which is beneficial to improve the peeling resistance, etc.
[0286] The adhesive composition may further contain an antistatic agent.
[0287] As antistatic agents, surfactants, silicone compounds, conductive polymers, ionic compounds, etc. can be cited, preferably ionic compounds. As ionic compounds, conventional compounds can be cited. As cationic components constituting ionic compounds, organic cations, inorganic cations, etc. can be cited. As organic cations, for example, pyridinium cations, pyrrolidinium cations, piperidinium cations, imidazolium cations, ammonium cations, sulfonium cations, phosphonium cations, etc. can be cited. As inorganic cations, for example, alkali metal cations such as lithium cations, potassium cations, sodium cations, cesium cations, magnesium cations, alkaline earth metal cations such as calcium cations, etc. can be cited. In particular, from the viewpoint of compatibility with (meth) acrylic resins, pyridinium cations, imidazolium cations, pyrrolidinium cations, lithium cations, potassium cations are preferred. As anionic components constituting ionic compounds, any type of inorganic anions and organic anions can be cited. From the perspective of antistatic performance, anionic components preferably containing fluorine atoms are preferred. Examples of the anion component containing a fluorine atom include hexafluorophosphate anion (PF6 - ), bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - ]、bis(fluorosulfonyl)imide anion [(FSO2)2N - ], tetrakis(pentafluorophenyl)borate anion [(C6F5)4B - ], etc. These ionic compounds can be used alone or in combination of two or more. The bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - ]、bis(fluorosulfonyl)imide anion [(FSO2)2N - ], tetrakis(pentafluorophenyl)borate anion [(C6F5)4B - ].
[0288] From the viewpoint of the temporal stability of the antistatic performance of the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition, an ionic compound that is solid at room temperature is preferred.
[0289] The content of the antistatic agent is, for example, 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 1 to 7 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin (A).
[0290] The adhesive composition may contain one or more additives such as a solvent, a crosslinking catalyst, a tackifier, a plasticizer, a softener, a pigment, a rust inhibitor, an inorganic filler, and light scattering fine particles.
[0291] [Middle layer]
[0292] The optical laminate of the present invention includes an intermediate layer 300. In the optical laminate of the present invention, the intermediate layer 300 sandwiched between the polarizer 10 and the light selectively absorbing adhesive layer 20 has the effect of inhibiting the light selective absorber contained in the light selectively absorbing adhesive layer 20 from moving to the polarizer 10. However, the intermediate layer 300 is a structure having only one or more layers selected from a liquid crystal solidification layer, an orientation layer, and a bonding layer, and is not a structure that completely blocks the transmission of the light selective absorber, so the inhibitory effect is insufficient. In the optical laminate of the present invention, by adjusting the absorbance of the light selectively absorbing adhesive layer, it is possible to inhibit the discoloration of the end of the polarizer under high temperature and high humidity.
[0293] The thickness of the intermediate layer 300 is not limited, but is, for example, 1 μm to 200 μm, and is preferably 5 μm to 200 μm from the viewpoint of suppressing the migration of the light selective absorber contained in the light selective absorbent adhesive layer.
[0294] From the viewpoint of suppressing discoloration in the polarizing plate 10, the intermediate layer 300 preferably does not contain a light selective absorber. If a light selective absorber is contained, the content of the light selective absorber per unit area is preferably 0.5 g / m 2 the following.
[0295] [Liquid crystal cured layer]
[0296] The optical laminate of the present invention may include a liquid crystal solidified layer as an intermediate layer. The liquid crystal solidified layer may be one layer or two or more layers. Figure 2 The optical stack 101 shown includes a first liquid crystal solidified layer 30 and a second liquid crystal solidified layer 31 .
[0297] The liquid crystal cured layer is a layer of a cured product of a polymerizable liquid crystal compound, and is, for example, a retardation layer.
[0298] As the retardation layer, there are first to fifth aspects, and the retardation layer is a cured product of a polymerizable liquid crystal compound.
[0299] First form: a phase difference layer in which the rod-like liquid crystal compound is aligned in a horizontal direction with respect to the supporting substrate
[0300] Second form: Retardation layer in which the rod-like liquid crystal compound is aligned in a vertical direction with respect to the supporting substrate
[0301] The third form: a phase difference layer in which the rod-like liquid crystal compound changes its orientation in a spiral shape within the plane
[0302] Fourth form: Phase difference layer with tilted orientation of discotic liquid crystal compounds
[0303] Fifth form: a biaxial phase difference layer in which a discotic liquid crystal compound is oriented perpendicularly to a supporting substrate
[0304] For example, as an optical laminate for an organic electroluminescent display, the first embodiment, the second embodiment, and the fifth embodiment are preferably used. Alternatively, retardation layers of these embodiments may be laminated and used.
[0305] The phase difference layer preferably has reverse wavelength dispersion. Reverse wavelength dispersion refers to an optical property in which the phase difference value in the liquid crystal orientation plane at a short wavelength is smaller than the phase difference value in the liquid crystal orientation plane at a long wavelength. The phase difference layer preferably satisfies the following formulas (7) and (8). It should be noted that Re(λ) represents the in-plane phase difference value relative to light of wavelength λnm.
[0306] Re(450) / Re(550)≤1 (7)
[0307] 1≤Re(630) / Re(550) (8)
[0308] In the optical laminate of the present invention, when the phase difference layer is in the first form and has reverse wavelength dispersion, since coloration during black display in a display device is reduced, it is preferred that in the above formula (7), 0.82≤Re(450) / Re(550)≤0.93 is more preferred. More preferably, 120≤Re(550)≤150 is further preferred.
[0309] Examples of polymerizable liquid crystal compounds for forming a phase difference layer include compounds having polymerizable groups among the compounds described in "3.8.6 Network (Completely Cross-linked Type)" and "6.5.1 Liquid Crystal Material b. Polymerizable Nematic Liquid Crystal Material" in the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2001), as well as polymerizable liquid crystal compounds described in Japanese Patent Publication No. 2010-31223, Japanese Patent Publication No. 2010-270108, Japanese Patent Publication No. 2011-6360, Japanese Patent Publication No. 2011-207765, Japanese Patent Publication No. 2011-162678, Japanese Patent Publication No. 2016-81035, International Publication No. 2017 / 043438 and Japanese Patent Table No. 2011-207765.
[0310] Examples of a method for producing a phase difference layer from a polymer in an aligned state of a polymerizable liquid crystal compound include a method described in Japanese Patent Application Laid-Open No. 2010-31223.
[0311] The thickness of the phase difference layer, which is a liquid crystal cured layer formed by curing the polymerizable liquid crystal compound, is, for example, 0.1 μm to 10 μm, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 6 μm.
[0312] The phase difference layer can be a λ / 4 phase difference layer that gives a phase difference of 1 / 4 wavelength to the transmitted light, a λ / 2 phase difference layer that gives a phase difference of 1 / 2 wavelength to the transmitted light, a positive type (Japanese: ポジティブ) A plate, and a positive type C plate. Figure 2 In the case where the optical laminate 101 shown includes a first liquid crystal solidification layer 30 and a second liquid crystal solidification layer 31, combinations of the first liquid crystal solidification layer 30 and the second liquid crystal solidification layer 31 include a combination of a λ / 2 phase difference layer and a λ / 4 phase difference layer, a combination of a λ / 4 phase difference layer and a positive C layer, and the like.
[0313] The optical layered body of the present invention may be constituted as a circularly polarizing plate having a λ / 4 phase difference layer. The circularly polarizing plate may be used as an antireflection polarizing plate.
[0314] [Orientation layer]
[0315] The alignment layer has an alignment restraining force that allows the liquid crystal compound contained in the liquid crystal curing layer formed on the alignment layer to be aligned in the desired direction. As the alignment layer, there can be cited: an alignment polymer layer formed by an alignment polymer, a photoalignment polymer layer formed by a photoalignment polymer, and a groove alignment layer having a concave-convex pattern and a plurality of grooves (grooves) on the surface of the layer. The thickness of the alignment layer is usually 0.01 to 10 μm, preferably 0.01 to 5 μm.
[0316] The oriented polymer layer can be formed by applying a composition obtained by dissolving the oriented polymer in a solvent on the substrate layer and removing the solvent, and then grinding as needed. In this case, in the oriented polymer layer formed by the oriented polymer, the orientation restriction force can be arbitrarily adjusted according to the surface state of the oriented polymer and the grinding conditions.
[0317] The photo-aligned polymer layer can be formed by applying a composition containing a polymer or monomer having a photoreactive group and a solvent to a substrate layer and irradiating the substrate with polarized light. In this case, the orientation restraining force in the photo-aligned polymer layer can be arbitrarily adjusted according to the polarized light irradiation conditions for the photo-aligned polymer.
[0318] The groove orientation layer can be formed, for example, by the following methods: a method of forming a concave-convex pattern by exposing and developing through an exposure mask having a slit in a pattern shape on the surface of a photosensitive polyimide film; a method of forming an uncured layer of an active energy ray-curable resin on a plate-shaped master disk having grooves on its surface, transferring the layer to a substrate layer and curing it; a method of forming an uncured layer of an active energy ray-curable resin on a substrate layer, pushing a rolled master disk having concave-convex on the layer, etc. to form concave-convex and concave and curing it, etc.
[0319] The substrate layer is preferably a film formed of a resin material. As the resin material, for example, a resin material having excellent transparency, mechanical strength, thermal stability, and stretchability can be used. Specifically, polyolefin resins such as polyethylene and polypropylene; cyclic polyolefin resins such as norbornene polymers; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; (meth) acrylic acid, poly(meth) methyl acrylate and other (meth) acrylic acid resins; cellulose ester resins such as cellulose triacetate, cellulose diacetate and cellulose acetate propionate; vinyl alcohol resins such as polyvinyl alcohol and polyvinyl acetate; polycarbonate resins; polystyrene resins; polyarylate resins; polysulfone resins; polyethersulfone resins; polyamide resins; polyimide resins; polyetherketone resins; polyphenylene sulfide resins; polyphenylene ether resins, and mixtures and copolymers thereof. Among these resins, it is preferred to use any resin or mixtures thereof among cyclic polyolefin resins, polyester resins, cellulose ester resins and (meth) acrylic resins. In addition, the above-mentioned "(meth)acrylic acid" means "at least one of acrylic acid and methacrylic acid".
[0320] The substrate layer may be a single layer of one of the above resins or a single layer of a mixture of two or more resins, or may have a multilayer structure of two or more layers. In the case of a multilayer structure, the resins forming each layer may be the same or different.
[0321] Any additives may be added to the resin material forming the resin film, and examples of the additives include light selective absorbers, antioxidants, lubricants, plasticizers, mold release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0322] The thickness of the substrate layer is not particularly limited, but is generally preferably 5 to 200 μm, more preferably 10 to 200 μm, and even more preferably 10 to 150 μm from the viewpoint of strength, handling properties, and the like.
[0323] In order to improve the adhesion between the substrate layer and the alignment layer, at least the surface of the substrate layer on the side where the alignment layer is to be formed may be subjected to corona treatment, plasma treatment, flame treatment, etc., or a primer layer may be formed. The substrate layer may be peeled off from the layer structure formed by the substrate layer / alignment layer / liquid crystal solidification layer, and the alignment layer / liquid crystal solidification layer may be used as a constituent element of the intermediate layer of the present invention, or the substrate layer / alignment layer may be peeled off and the liquid crystal solidification layer may be used as a constituent element of the intermediate layer of the present invention.
[0324] [Lamination layer]
[0325] The intermediate layer 300 may include a bonding layer for bonding two layers. Examples of the bonding layer include an adhesive layer, an adhesive layer (hereinafter also referred to as a "second adhesive layer"), and the like. Figure 2 The optical laminate 101 shown includes an adhesive layer 33 sandwiched between a first liquid crystal solidified layer 30 and a second liquid crystal solidified layer 31 to bond them together, and a second pressure-sensitive adhesive layer 32 laminated on the surface of the first liquid crystal solidified layer 30 opposite to the adhesive layer 33 .
[0326] The adhesive layer may be made of a water-based adhesive, an active energy ray-curable adhesive, or a thermosetting adhesive, etc. The thickness of the adhesive layer is, for example, 10 nm to 20 μm, preferably 100 nm to 10 μm, and more preferably 500 nm to 5 μm.
[0327] The second adhesive layer can be composed of the same adhesive composition as the adhesive composition forming the above-mentioned light selective absorption adhesive layer, or it can be composed of an adhesive composition (hereinafter also referred to as the "second adhesive composition") having a resin such as a (meth) acrylic acid series, a rubber series, a urethane series, an ester series, a silicone series, or a polyvinyl ether series as a main component. As the second adhesive composition, an adhesive composition using a (meth) acrylic acid resin having excellent transparency, weather resistance, heat resistance, etc. as a base polymer is preferred. The second adhesive composition can be an active energy ray-curable type or a thermosetting type. The thickness of the second adhesive layer is, for example, 0.1 to 150 μm, typically 8 to 60 μm, and is preferably less than 30 μm, and more preferably less than 20 μm, from the perspective of thinning.
[0328] From the viewpoint of suppressing discoloration in the polarizer 10 , the second pressure-sensitive adhesive layer preferably contains no light selective absorber. If a light selective absorber is contained, the amount of the light selective absorber is preferably 0.5 parts by mass or less based on 100 parts by mass of the total resin component per unit area.
[0329] <Method for producing optical layered body>
[0330] The optical laminate 100, 101, 102 can be manufactured by a method comprising a process of laminating the constituent layers to each other via a laminating layer. In addition, a process of peeling off a layer that is not a constituent layer may also be included. When laminating the layers to each other via a laminating layer, in order to improve adhesion, it is preferred that one or both sides of the laminating surface be subjected to a surface activation treatment such as a corona treatment.
[0331] <Optical laminate>
[0332] The optical laminate of the present invention is planar, and its area is, for example, 30 mm×30 mm to 180 mm×90 mm. The optical laminate of the present invention may be a rectangle such as a rectangle or a square, or may be a so-called irregular shape such as a shape in which a part of the side constituting the rectangle is cut off to have a cutout portion, a semicircular shape, or a shape having a through hole in the plane. In the case where the outer shape of the optical laminate has a straight side, the absorption axis of the polarizer constituting the optical laminate may be parallel to the side, or may be orthogonal, or may be inclined to cross at an angle of, for example, 45°. In the case where the optical laminate has a phase difference layer, and the phase difference layer has a slow axis in the plane, the slow axis and the absorption axis of the polarizer constituting the optical laminate may intersect at 45°, 15°, or 75°.
[0333] <Image display device>
[0334] The optical laminates 100, 101, and 102 are arranged on the front surface (visible side) of the image display panel and can be used as a component of the image display device. The optical laminate as a circular polarizing plate can also be used as an anti-reflection polarizing plate for imparting an anti-reflection function in the image display device. The image display device is not particularly limited, and examples thereof include organic electroluminescent (organic EL) display devices, inorganic electroluminescent (inorganic EL) display devices, liquid crystal display devices, and field-induced luminescent display devices.
[0335] Example
[0336] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples. Unless otherwise specified, "%" and "part" in Examples and Comparative Examples are "mass %" and "mass part".
[0337] [Production of single-sided protected polarizing plate]
[0338] (Production of polarizing film)
[0339] A polyvinyl alcohol film having a thickness of 20 μm, a degree of polymerization of 2400, and a saponification degree of more than 99% is uniaxially stretched on a hot roller to a stretching ratio of 4.1 times, and while maintaining the tension, is immersed in a dyeing bath containing 0.05 parts by weight of iodine and 5 parts by weight of potassium iodide per 100 parts by weight of water at 28° C. for 60 seconds.
[0340] Next, the film was immersed in a boric acid aqueous solution 1 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water at 64°C for 110 seconds. Next, the film was immersed in a boric acid aqueous solution 2 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water at 67°C for 30 seconds. Then, the film was washed with pure water at 10°C and dried to obtain a polarizer. The obtained polarizer had a thickness of 8 μm and a boron content of 4.3% by weight.
[0341] (Preparation of water-based adhesive)
[0342] 3 parts by weight of carboxyl-modified polyvinyl alcohol (Kuraray Co., Ltd., trade name "KL-318") was dissolved in 100 parts by weight of water, and 1.5 parts by weight of a polyamide epoxy additive (Taoka Chemical Industry Co., Ltd., trade name "Sumirez Resin (registered trademark) 650 (30), a 30% by weight aqueous solution of solid content concentration) as a water-soluble epoxy resin was added to the aqueous solution to prepare a water-based adhesive.
[0343] (Protective film A and release film B)
[0344] As the protective film A, a film having a thickness of 3 μm and a hard coat layer formed on a 25 μm-thick stretched film made of a norbornene-based resin (manufactured by Nippon Paper Industries, Ltd., trade name “COP25ST-HC”) was used.
[0345] A triacetylcellulose film (manufactured by Fujifilm Corporation, "TD80UL") was used as the release film B. The release film had a thickness of 80 μm and a water vapor permeability of 502 g / m 2 ·24 hr.
[0346] (Production of single-sided protective polarizing plate)
[0347] The produced polarizer is continuously conveyed, while the protective film A is continuously unwound from the roll of the protective film A, and the release film B is continuously unwound from the roll of the release film B. A water-based adhesive is injected between the polarizer and the corona-treated protective film A, and pure water is injected between the polarizer and the release film B, and the laminated film formed by the protective film A / water-based adhesive / polarizer / pure water / release film B is obtained by passing through a laminating roller. The laminated film is conveyed and subjected to a heat treatment at 80°C for 300 seconds in a drying oven, thereby drying the water-based adhesive and volatilizing and removing the pure water sandwiched between the polarizer and the release film B to obtain a single-sided protected polarizing plate with a release film. The release film B is peeled off from the single-sided protected polarizing plate with a release film to obtain a single-sided protected polarizing plate.
[0348] [Production of Phase Difference Laminated Body]
[0349] (Preparation of "Alignment Layer / First Liquid Crystal Solidification Layer")
[0350] An alignment layer formed on a substrate film and a λ / 4 phase difference layer (first liquid crystal solidified layer) which was a layer formed by solidifying a nematic liquid crystal compound were prepared. The total thickness of the alignment layer / first liquid crystal solidified layer was 2 μm.
[0351] (Production of “Alignment Layer / Second Liquid Crystal Solidification Layer”)
[0352] 10.0 parts by mass of polyethylene glycol di(meth)acrylate (A-600, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a composition for forming an alignment layer, 10.0 parts by mass of trimethylolpropane triacrylate (A-TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.), 10.0 parts by mass of 1,6-hexanediol di(meth)acrylate (A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), and 1.50 parts by mass of Irgacure 907 (Irg-907, manufactured by BASF) as a photopolymerization initiator were dissolved in 70.0 parts by mass of methyl ethyl ketone as a solvent to prepare a coating liquid for forming an alignment layer.
[0353] As a substrate film, a 20 μm thick long cyclic olefin resin (COP) film (manufactured by Japan Zeon Co., Ltd.) was prepared, and the coating liquid for forming an alignment layer was applied to one side of the substrate film using a wire bar coater.
[0354] The applied coating layer was heat treated at 80°C for 60 seconds and then at 220 mJ / cm 2 The composition for forming an alignment layer was polymerized and cured by irradiation with ultraviolet rays (UVB), thereby forming an alignment layer having a thickness of 2.3 μm on the base film.
[0355] 20.0 parts by mass of a photopolymerizable nematic liquid crystal compound (RMM28B manufactured by Merck) as a composition for forming a phase difference layer and 1.0 parts by mass of Irgacure 907 (Irg-907 manufactured by BASF) as a photopolymerization initiator were dissolved in 80.0 parts by mass of propylene glycol monomethyl ether acetate as a solvent to prepare a coating liquid for forming a phase difference layer.
[0356] The retardation layer-forming coating liquid was applied onto the alignment layer obtained above, and the coating layer was heat-treated at 80° C. for 60 seconds. 2 The composition for forming the phase difference layer was polymerized and cured by irradiation with ultraviolet light (UVB), and a phase difference layer (second liquid crystal cured layer) with a thickness of 0.7 μm was formed on the alignment layer. In this way, a "alignment layer / second liquid crystal cured layer" with a total thickness of 3 μm was obtained on the substrate film.
[0357] (Production of Phase Difference Laminated Body)
[0358] The "orientation layer / first liquid crystal curing layer" laminated on the substrate film and the "orientation layer / second liquid crystal curing layer" laminated on the substrate film were laminated by an ultraviolet curing adhesive (thickness 1 μm) in such a way that the respective liquid crystal curing layer surfaces (surfaces on the opposite side of the substrate film) became the laminating surfaces. Next, ultraviolet rays were irradiated to cure the ultraviolet curing adhesive, and a phase difference laminated body including two liquid crystal curing layers, the first liquid crystal curing layer and the second liquid crystal curing layer, was prepared.
[0359] [Preparation of Light-Selectively Absorbing Adhesive Layer]
[0360] (Preparation of acrylic resin (A-1))
[0361] A mixed solution of 86.4 parts of ethyl acetate, 61.9 parts of butyl acrylate and 1.9 parts of 2-hydroxyethyl acrylate as a solvent was placed in a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer and a stirrer, and the internal temperature was raised to 60°C while replacing the air in the device with nitrogen to make it oxygen-free. Then, the entire amount of a solution obtained by dissolving 0.4 parts of azobisisobutyronitrile (polymerization initiator) in 10 parts of ethyl acetate was added. The obtained mixture was kept at 60°C for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while the internal temperature was kept at 50-70°C. The addition of ethyl acetate was stopped at the moment when the concentration of the acrylic resin reached 35%, and the temperature was further maintained from the start of the addition of ethyl acetate until 12 hours had passed. Finally, ethyl acetate was added and adjusted to a concentration of 20% of the acrylic resin to prepare an ethyl acetate solution of the acrylic resin. The polystyrene-equivalent weight average molecular weight Mw of the obtained acrylic resin based on GPC was 600,000, and Mw / Mn was 7.0. It was referred to as acrylic resin (A-1). The glass transition temperature based on DSC was -52.9°C.
[0362] (Preparation of Adhesive Layer (1))
[0363] In an ethyl acetate solution of an acrylic resin (A-1) (resin concentration: 20%), 0.5 parts of a crosslinking agent (CORONATE L, solid content 75%: manufactured by Tosoh), 0.5 parts of a silane compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 2.5 parts of a compound represented by the following formula (aa2) described as a light selective absorption compound (2) in Synthesis Example 2 described in paragraph
[0142] of Japanese Patent Application Laid-Open No. 2019-007001 (light selective absorption agent) were mixed with respect to 100 parts of the solid content of the solution, and 2-butanone was further added in such a manner that the solid content concentration became 14%, thereby obtaining an adhesive composition (1). It should be noted that the amount of the crosslinking agent (CORONATE L) is the mass fraction based on the active ingredient.
[0364] [Chemical formula 23]
[0365]
[0366] The adhesive composition (1) prepared above was applied to the release-treated surface of a polyethylene terephthalate film (SP-PLR382050 manufactured by LINTEC, hereinafter referred to as "spacer") using an applicator so that the thickness of the adhesive layer after drying was 17 μm, and dried at 100° C. for 1 minute to prepare an adhesive layer. The obtained adhesive layer was referred to as an adhesive layer (1). Table 1 shows the content of the light selective absorber per unit area of the adhesive layer (1).
[0367] (Preparation of Adhesive Layer (2))
[0368] The adhesive layer (2) was prepared in the same manner as the adhesive layer (1) except that the amount of the light selective absorber was 3.7 parts. Table 1 shows the content of the light selective absorber per unit area of the adhesive layer (2).
[0369] (Preparation of Adhesive Layer (3))
[0370] The adhesive layer (3) was prepared in the same manner as the adhesive layer (1) except that the amount of the light selective absorber was 5.4 parts. Table 1 shows the content of the light selective absorber per unit area of the adhesive layer (3).
[0371] [Preparation of Second Adhesive Layer]
[0372] 0.5 parts of a crosslinking agent (CORONATE L, solid content 75%: manufactured by Tosoh) and 0.5 parts of a silane compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed with an ethyl acetate solution of the acrylic resin (A-1) (resin concentration: 20%), and 2-butanone was further added so that the solid content concentration became 14%, thereby obtaining an adhesive composition. It should be noted that the amount of the crosslinking agent (CORONATE L) is the mass fraction based on the active ingredient.
[0373] The adhesive composition was applied to the release-treated surface of the spacer for forming the light selective absorption adhesive layer using an applicator so that the thickness of the adhesive layer after drying would be 5 μm, and dried at 100° C. for 1 minute to form a second adhesive layer.
[0374] [Production of optical laminate]
[0375] (Examples 1 and 3)
[0376] The second adhesive layer is bonded to the polarizer side of the manufactured single-sided protective polarizing plate, and the spacer is peeled off. The surface of the second adhesive layer after the spacer is peeled off is bonded to the surface exposed by peeling off the substrate film on the first liquid crystal solidification layer side of the manufactured phase difference laminate. Then, the substrate film on the second liquid crystal solidification layer side is peeled off, and the adhesive layer described in Table 1 is bonded to the surface of the orientation layer on the second liquid crystal solidification layer side as a light selective absorption adhesive layer to obtain an optical laminate having a layer structure of "protective film A / water-based adhesive / polarizer / second adhesive layer / orientation layer / first liquid crystal solidification layer / second liquid crystal solidification layer / orientation layer / light selective absorption adhesive layer / spacer". In this optical laminate, the intermediate layer has a layer structure of "second adhesive layer / orientation layer / first liquid crystal solidification layer / second liquid crystal solidification layer / orientation layer", and the total thickness is 11μm.
[0377] In the above operation, the adhesive layer was applied using an applicator so that the thickness was 5 μm, and dried at 100° C. for 1 minute to prepare the second adhesive layer. The total thickness of the “alignment layer / first liquid crystal solidification layer” was 2 μm. The total thickness of the “alignment layer / second liquid crystal solidification layer” was 3 μm.
[0378] The thickness of the ultraviolet curing adhesive was 1 μm.
[0379] (Examples 2, 4, and Comparative Example 1)
[0380] The second adhesive layer was attached to the polarizer side of the produced single-sided protective polarizing plate, and the spacer was peeled off. The adhesive layer listed in Table 1 was attached to the surface of the second adhesive layer after the spacer was peeled off as a light selective absorption adhesive layer, to obtain an optical laminate having a layer structure of "protective film A / water-based adhesive / polarizer / second adhesive layer / light selective absorption adhesive layer / spacer". In this optical laminate, the intermediate layer was composed of the "second adhesive layer" and had a thickness of 5 μm.
[0381] In the above operation, the adhesive layer was applied using an applicator so as to have a thickness of 5 μm, and dried at 100° C. for 1 minute to prepare a second adhesive layer.
[0382] [Measurement of absorbance of adhesive layer]
[0383] Adhesive layers (1) to (3) were respectively bonded to glass, and after the spacer was peeled off, a cycloolefin polymer (COP) film (ZF-14 manufactured by Japan Zeon Co., Ltd.) was bonded to the adhesive layer to prepare a laminate for adhesive layer evaluation. The laminate for adhesive layer evaluation was placed in a spectrophotometer UV-2450 (manufactured by Shimadzu Corporation), and the absorbance was measured by a double beam method with a step size of 1 nm in a wavelength range of 300 to 800 nm. The absorbance of the prepared adhesive layer at a wavelength of 410 nm is shown in Table 1. It should be noted that the absorbance of the glass at a wavelength of 410 nm and the absorbance of the COP film are both 0.
[0384] [Measurement of weight average molecular weight (Mw)]
[0385] The weight average molecular weight (Mw) of the acrylic resin (A-1) was determined as the number average molecular weight (Mn) in terms of polystyrene by size exclusion chromatography (SEC) using tetrahydrofuran as the mobile phase. The (meth)acrylic polymer to be measured was dissolved in tetrahydrofuran at a concentration of about 0.05% by mass, and 10 μL was injected into SEC.
[0386] The mobile phase was allowed to flow at a flow rate of 1.0 mL / min. PLgel MIXED-B (manufactured by Polymer Laboratories) was used as a chromatographic column. A UV-VIS detector (trade name: Agilent GPC) was used as a detector.
[0387] [Determination of Boron Content]
[0388] 0.2 g of the polarizer was dissolved in 200 g of a 1.9 wt% mannitol aqueous solution, and the resulting aqueous solution was titrated with a 1 mol / L NaOH aqueous solution, and the boron content of the polarizer was calculated by comparing the amount of NaOH solution required for neutralization with the calibration curve.
[0389] [Wet and heat resistance test and observation of discoloration]
[0390] The separators of the optical layered bodies obtained in Examples 1 to 4 and Comparative Example 1 were peeled off, and the plates were bonded to a non-alkali glass plate, followed by leaving the plates to stand in an environment of a temperature of 65° C. and a humidity of 90% RH for 500 hours.
[0391] Then, a polarizing plate was bonded to the non-alkali glass surface opposite to the tested optical layered body so as to form a crossed Nicol relationship, and the image was observed with an optical microscope, and the observed image was saved. The optical microscope used was "VHX-500" manufactured by Keyence Corporation. Figure 4 An example of an image observed using an optical microscope is shown. Figure 4When observing from the end 50 of the optical laminate inwardly along the straight line indicated by the arrow (a straight line extending in the vertical direction from the end 50), it can be seen that there are a discolored area 51 and an area 52 where no discoloration occurs (non-discolored area).
[0392] [Measurement of the amount of decolorization by image processing]
[0393] The image observed by the microscope was converted into black and white 256 levels (0 to 255) using the image analysis software "ImageJ (free software)". The method of converting into black and white 256 levels (0 to 255) was a method of taking the average of RGB values. Figure 5 An example of the converted data is shown. Figure 4 The midpoint between the bleached area 51 and the non-bleached area 52 in the gradation curve (in the middle of the bleached depth) is taken as the bleached end portion ( Figure 5 ), and the distance (μm) from the end 50 of the optical layered body to the discolored end was measured as the discolored distance. The discolored distances of the optical layered body are shown in Table 1. The smaller the discolored distance, the narrower the discolored range, and the better the moist heat resistance.
[0394] [Table 1]
[0395]
[0396] Description of Reference Numerals
[0397] 10 polarizing plate, 11 protective film, 20 light selectively absorbing adhesive layer, 30 first liquid crystal solidification layer, 31 second liquid crystal solidification layer, 32 second adhesive layer, 33 adhesive layer, 50 end of optical laminate, 51 bleached area, 52 non-bleached area, 100, 101, 102 optical laminate, 300 intermediate layer.
Claims
1. An optical laminate comprising: a polarizing plate, a light selectively absorbing adhesive layer, and an intermediate layer laminated between the polarizing plate and the light selectively absorbing adhesive layer so as to be in contact with the polarizing plate and the light selectively absorbing adhesive layer. The intermediate layer has only one or more layers selected from a liquid crystal solidification layer, an alignment layer and a lamination layer, The polarizer absorbs iodine and orients the iodine, and the boron content is 5.0 mass % or less. The light selectively absorbing adhesive layer contains a light selective absorber and has an absorbance of 0.1 or more and 2.3 or less at a wavelength of 410 nm. In the light selectively absorbing adhesive layer, the content of the light selective absorber per unit area is 0.01 g / m 2 Above 0.47g / m 2 the following. 2 . The optical laminate according to claim 1 , further comprising a protective film laminated on the side of the polarizing plate opposite to the intermediate layer side.
3. The optical layered body according to claim 1 or 2, wherein: The light selectively absorbing adhesive layer contains 0.1 parts by mass or more and 10 parts by mass or less of the light selective absorber with respect to 100 parts by mass of all resin components contained in the light selectively absorbing adhesive layer.
4. The optical layered body according to claim 1 or 2, wherein: The light selectively absorbing adhesive layer has a thickness of 0.1 μm or more and 150 μm or less.
5. The optical layered body according to claim 1 or 2, wherein: The light selective absorber is an organic light selective absorber having a molecular weight of 100 to 3000.
6. The optical layered body according to claim 1 or 2, wherein: The intermediate layer has a λ / 4 phase difference layer as the liquid crystal solidified layer. The optical layered body according to claim 1 or 2, which is a polarizing plate for antireflection. 8 . An image display device comprising an image display panel and the optical laminate according to claim 7 disposed on a front surface of the image display panel.
9. The image display device according to claim 8, wherein: The image display panel is an organic EL display panel.