A method for reducing high-valent metal ions
By adding organic matter to the acid leaching solution and controlling the pH value, the electrolysis reaction is used to reduce high-valence metal ions to low-valence states, which solves the problems of impurity introduction and high power consumption in the reduction process of high-valence metal ions in the existing technology, and achieves Low energy consumption and efficient reduction effect, and use organic products as by-products.
Patent Information
- Application Number
- CN202210472620.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-04-29
AI Technical Summary
In the reduction process of high-priced metal ions, the existing technology easily introduces non-volatile impurities or uses a large amount of metal elements, resulting in high production costs and low electrolysis efficiency. In particular, a large amount of electricity is wasted on oxygen evolution side reactions during the electrolysis process.
By adding organic matter to the acid leaching solution and energizing the anode and cathode for reaction, the pH value is controlled between -1 and 5, and the oxidation of organic matter is used to reduce the valence of metal ions, thereby reducing power consumption during the electrolysis process and avoiding oxygen evolution at the anode.
It achieves the reduction of high-valence metal ions to low-valence states with low energy consumption without introducing non-volatile impurities and without using a large amount of metal elements, reducing the energy consumption of the electrolysis process and using organic products as by-products, which has industrial Practical value.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and in particular relates to a method for reducing high-valent metal ions. Background Art
[0002] In the process of preparing metal salts, high-valent metal ions need to be reduced. The "Method for Reducing Trivalent Iron Ions" invented by Liu Qiang et al. reported a method for reducing trivalent iron ions by adding hydrothermal biochar powder to a trivalent iron solution. There are also literature reports that the purpose of reducing high-valent metal ions is achieved by adding metal elements to react with high-valent metal ions.
[0003] During the reduction process of high-valent metal ions, substances different from the reduced metal ions are often introduced, which introduces non-volatile impurities into the reaction system, or the same metal element as the reduced metal ions is used, which increases production costs and brings difficulties to subsequent processing steps.
[0004] The method of reducing high-valent metal ions by electrolysis does not introduce non-volatile impurities or use a large amount of metal elements. However, in the electrolysis of high-valent metal ions, mass transfer factors often have a greater impact on the electrolysis efficiency, that is, a large amount of electrolysis energy consumption will be wasted on the oxygen evolution side reaction, which is intuitively manifested as low electrolysis efficiency. Summary of the invention
[0005] The purpose of the present invention is to provide a method for reducing high-valent metal ions. Without introducing non-volatile impurities and using a large amount of metal elements, the reaction energy barrier is reduced by adding organic matter, thereby achieving the purpose of reducing liquid phase high-valent metal ions to low-valent metal ions or metals without releasing a large amount of oxygen and with low energy consumption.
[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0007] A method for reducing high-valent metal ions comprises the following steps:
[0008] (1) adding organic matter to an acid leaching solution containing high-valent metal ions to obtain a mixed solution;
[0009] (2) Inserting a cathode and an anode into the obtained mixed solution and connecting an external power source to react, and controlling the pH value to -1 to 5, the high-valent metal ions therein can be reduced to low-valent metal ions or metals.
[0010] According to the above scheme, the high-valent metal ions include any one of positive trivalent iron ions, positive divalent copper ions, positive trivalent cobalt ions, and positive trivalent nickel ions, or a mixture thereof.
[0011] According to the above scheme, the acid leaching solution containing high-valent metal ions is any one of the acid leaching solution of lithium iron phosphate recycled material lithium slag, the acid leaching solution of azurite, the acid leaching solution of copper oxide ore, the acid leaching solution of limonite, the acid leaching solution of iron oxide, the acid leaching solution of ternary recycled material of lithium battery, copper sulfate electrolyte, and circuit board etching solution.
[0012] According to the above scheme, the organic matter is one or any combination of alcohols, aldehydes, phenols, esters, dimethyl ether, and formic acid; the alcohol is any one of methanol, ethanol, propanol, and butanol; the aldehyde is any one of formaldehyde, acetaldehyde, and benzaldehyde; the phenol is any one of phenol and cresol; the ester is any one of ethyl formate, methyl formate, and monomethyl sulfate.
[0013] According to the above scheme, the concentration of high-valent metal ions in the acid leaching solution containing high-valent metal ions is 0.1 to 5 mol per liter; the molar ratio of the organic matter to the high-valent metal ions is (0.1 to 5):1.
[0014] According to the above scheme, the cathode is any one of an iron electrode, a stainless steel electrode, a titanium electrode, a copper electrode, a nickel-plated iron electrode, and a graphite electrode.
[0015] According to the above scheme, the anode is any one of a platinum electrode, a silver electrode, a gold electrode, a ruthenium electrode, a tantalum electrode, and an iridium electrode, or an electrode electroplated or doped with platinum, silver, gold, ruthenium, tantalum, or iridium.
[0016] According to the above scheme, the voltage of the external power supply is 0.1V~5V.
[0017] According to the above scheme, the temperature of the power-on reaction is 0°C≤T1≤110°C; the optimized temperature is 50°C~80°C.
[0018] According to the above scheme, it also includes adding acid-soluble high-valent metal ion raw materials and stirring during the electrical reaction process.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention adopts a method of adding organic matter to electrolyze to reduce the valence of high-valent metal ions in the acid leaching solution to achieve the purpose of reducing the high-valent metal ions. Through the oxidation of the organic matter, oxygen evolution at the anode during the electrolytic reduction process is avoided to a large extent. At the same time, during the reduction of the high-valent metal ions, part of the electrons are provided by the organic matter through chemical reactions, which greatly reduces the power consumption during the electrolytic process.
[0021] The present invention realizes the electrolytic reduction of high-valent metal ions by adding organic matter without introducing non-volatile impurities and using a large amount of metal elements, and the oxidized organic products in the production process can also be sold as by-products, which has high industrial practical value. DETAILED DESCRIPTION
[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] A method for reducing high-valent metal ions is provided in a specific embodiment:
[0024] (1) adding organic matter to an acid leaching solution containing high-valent metal ions to obtain a mixed solution;
[0025] (2) Inserting a cathode and an anode into the obtained mixed solution and connecting an external power source to react, and controlling the pH value to -1 to 5, the high-valent metal ions therein can be reduced to low-valent metal ions or metals.
[0026] The high-valent metal ions include any one of trivalent iron ions, divalent copper ions, trivalent cobalt ions, and trivalent nickel ions, or a mixture thereof.
[0027] Further preferably, the acid leaching solution containing high-valent metal ions is any one of the acid leaching solution of lithium iron phosphate recycled material lithium slag, the acid leaching solution of azurite, the acid leaching solution of copper oxide ore, the acid leaching solution of limonite, the acid leaching solution of iron oxide, the acid leaching solution of ternary recycled material of lithium battery, copper sulfate electrolyte, and circuit board etching solution.
[0028] The organic matter is one or any combination of alcohols, aldehydes, phenols, esters, dimethyl ether, and formic acid; the alcohol is any one of methanol, ethanol, propanol, and butanol; the aldehyde is any one of formaldehyde, acetaldehyde, and benzaldehyde; the phenol is any one of phenol and cresol; the ester is any one of ethyl formate, methyl formate, and monomethyl sulfate.
[0029] The concentration of high-valent metal ions in the acid leaching solution containing high-valent metal ions is 0.1 to 5 mol per liter; the molar ratio of the organic matter to the high-valent metal ions is (0.1 to 5):1.
[0030] The cathode is any one of an iron electrode, a stainless steel electrode, a titanium electrode, a copper electrode, a nickel-plated iron electrode and a graphite electrode.
[0031] The anode is any one of a platinum electrode, a silver electrode, a gold electrode, a ruthenium electrode, a tantalum electrode, and an iridium electrode, or an electrode electroplated or doped with platinum, silver, gold, ruthenium, tantalum, or iridium.
[0032] The voltage of the external power supply is 0.1V-5V.
[0033] The temperature of the power-on reaction is 0°C≤T1≤110°C; the optimized temperature is 50°C~80°C.
[0034] The method also includes adding a raw material capable of dissolving high-valent metal ions in an acid and stirring the raw material during the electrical reaction.
[0035] Example 1
[0036] The lithium slag after lithium extraction from a certain lithium iron phosphate positive electrode material is treated with nitric acid leaching to obtain an acid leaching solution containing trivalent iron.
[0037] (1) Adding a mixture of methanol, formaldehyde and formic acid in any ratio to the nitric acid leaching solution of lithium slag to obtain a mixed solution, wherein the molar ratio of organic matter to trivalent iron in the leaching solution is 1:1, and Fe 3+ The concentration is 3 mol per liter;
[0038] (2) Insert an iron electrode cathode and a ruthenium-iridium anode into the obtained mixed solution, and connect an external 2V power supply, raise the temperature to 50°C, add lithium extraction slag, mix and stir, and continue to power on until the pH value of the solution is 4. The reaction time is 3 hours.
[0039] In this embodiment, when the pH value of the acid leaching solution is 4, the Fe 2+ / Fe 3+ The molar ratio is equal to 100, there is no oxygen evolution at the anode, and formic acid by-product can be obtained after distillation of the acid leaching solution.
[0040] Example 2
[0041] Azurite, a raw material whose main component is basic copper carbonate, is leached with sulfuric acid to obtain an acid leaching solution containing divalent copper ions.
[0042] (1) Adding a mixture of acetaldehyde and ethanol in any ratio to the acid leaching solution of azurite to obtain a mixed solution, wherein the molar ratio of organic matter to divalent copper in the acid leaching solution is 1.5:1, and the Cu in the acid leaching solution is 2+ The concentration is 2 mol per liter;
[0043] (2) inserting a nickel-plated iron electrode cathode and a tantalum electrode anode into the obtained mixed solution, and connecting an external 2.3V power supply, heating to 40°C, and stopping the power supply when the pH value of the acid immersion solution reaches 0.
[0044] In this embodiment, the divalent copper ions are reduced to copper element at the cathode, no oxygen is evolved at the anode, and acetic acid byproduct can be obtained after distillation of the acid leaching solution.
[0045] Example 3
[0046] A certain limonite ore was leached with sulfuric acid to obtain an acid leaching solution containing trivalent iron.
[0047] (1) Add a mixture of formaldehyde and acetaldehyde in any ratio to the acid leaching solution of limonite to obtain a mixed solution in which the organic matter and Fe in the acid leaching solution are 3+ The molar ratio of Fe in the acid leaching solution is 5:1. 3+ The concentration is 5 mol per liter;
[0048] (2) inserting a graphite cathode and a titanium-based platinum-plated anode into the obtained mixed solution, and connecting an external 1V power supply, heating to 60°C, and stopping the power supply when the pH value of the acid immersion solution is 3.
[0049] The Fe content of the acid leaching solution after treatment in this embodiment 2+ / Fe 3+ The molar ratio is equal to 20, there is no oxygen evolution at the anode, the amount of elemental iron used in subsequent treatment is greatly reduced, and the treated acid leaching solution can be evaporated and crystallized to obtain ferrous sulfate.
[0050] Example 4
[0051] The ternary recycled material of lithium battery is mainly composed of lithium nickel cobalt manganese oxide. After acid leaching with a mixed acid of hydrochloric acid, sulfuric acid and nitric acid in any ratio, an acid leaching solution containing trivalent cobalt ions, trivalent nickel ions and monovalent lithium ions is obtained.
[0052] (1) Adding a mixture of benzaldehyde, phenol and cresol in any ratio to the acid leaching solution of the ternary recycled material to obtain a mixed solution, wherein the molar ratio of the organic matter to the trivalent cobalt ions and trivalent nickel ions in the acid leaching solution is 2:1, and the Co in the acid leaching solution is 1:1. 3+ with Ni 3+ The sum of the concentrations is 1 mol per liter;
[0053] (2) Insert a copper electrode cathode and a gold electrode anode into the obtained mixed solution, and connect an external 5V power supply, raise the temperature to 45°C, add the ternary recycled material, mix and stir, and stop powering when the pH value of the acid leaching solution reaches 5.
[0054] In this embodiment, the trivalent cobalt ions and trivalent nickel ions in the acid leaching solution of the lithium battery ternary recycled material are reduced to divalent cobalt ions and metallic nickel at the cathode. Under the action of the electrode, the organic matter reacts with the nickel and cobalt ions, and the organic product is separated from the acid leaching solution after reduced pressure distillation. While achieving the reduction of nickel and cobalt high-valent ions, no non-volatile impurities are introduced into the acid leaching solution.
[0055] Example 5
[0056] Copper sulfate electrolyte, the main components are sulfuric acid and copper sulfate solution.
[0057] (1) adding a mixture of ethanol, propanol, formic acid, and butanol in any ratio to a copper sulfate electrolyte to obtain a mixed solution, wherein the molar ratio of the organic matter to the divalent copper ions in the electrolyte is 0.5:1, and the concentration of the copper ions is 0.1 mol / L;
[0058] (2) inserting a titanium electrode cathode and a silver electrode anode into the obtained mixed solution, and connecting an external 0.5V power supply, heating to 110°C, and stopping the power supply when the pH value of the copper sulfate electrolyte reaches -1.
[0059] In this embodiment, the divalent copper ions are reduced to single copper at the cathode. When the copper ion concentration in the electrolyte is reduced to 1 gram per liter, the reaction time is 60 minutes. Under the action of the electrode, the organic matter and the copper ions directly react chemically, and the power consumption is greatly reduced.
[0060] Example 6
[0061] Circuit board etching solution, the main components are cupric chloride and hydrochloric acid.
[0062] (1) adding a mixture of ethyl formate, ethanol, methyl formate, monomethyl sulfate, and dimethyl ether in any ratio to a circuit board etching solution to obtain a mixed solution, wherein the molar ratio of the organic matter to the divalent copper ions in the electrolyte is 0.2:1, and the concentration of the copper ions is 1 mol / L;
[0063] (2) inserting a stainless steel electrode cathode and a titanium-based tantalum-iridium-plated anode into the obtained mixed solution, and connecting an external 2.4V power supply, heating the solution to 100°C, and stopping the power supply when the pH value of the copper sulfate electrolyte reaches 0.
[0064] In this embodiment, the divalent copper ions are reduced to copper at the cathode. When the copper ion concentration in the electrolyte is reduced to 1 gram per liter, the reaction time is 40 minutes. Under the action of the electrode, the organic matter and the copper ions directly react chemically, and the power consumption is greatly reduced.
Claims
1. A method for reducing high-valent metal ions, characterized in that The steps include: (1) Adding organic matter to an acid leaching solution containing high-valent metal ions to obtain a mixed solution; the acid leaching solution containing high-valent metal ions is any one of an acid leaching solution of lithium iron phosphate recovery material lithium slag, an acid leaching solution of azurite, an acid leaching solution of limonite, and an acid leaching solution of ternary recovery material of lithium battery; the concentration of high-valent metal ions in the acid leaching solution containing high-valent metal ions is 0.1 to 5 mol / L; the molar ratio of the organic matter to the high-valent metal ions is (0.1 to 5):1; the organic matter is a combination of any two or more of alcohols, aldehydes, and phenols; the alcohol is any one of methanol, ethanol, propanol, and butanol; the aldehyde is any one of formaldehyde, acetaldehyde, and benzaldehyde; the phenol is any one of phenol and cresol; (2) Inserting a cathode and an anode into the obtained mixed solution and connecting an external power source to react, while controlling the pH value between -1 and 5, the high-valent metal ions therein can be reduced to low-valent metal ions or metals.
2. The method for reducing high-valent metal ions according to claim 1, characterized in that The high-valent metal ions include any one of positive trivalent iron ions, positive divalent copper ions, positive trivalent cobalt ions, and positive trivalent nickel ions, or a mixture thereof.
3. The method for reducing high-valent metal ions as claimed in claim 1, characterized in that The cathode is any one of an iron electrode, a stainless steel electrode, a titanium electrode, a copper electrode, a nickel-plated iron electrode and a graphite electrode.
4. The method for reducing high-valent metal ions according to claim 1, characterized in that The anode is any one of a platinum electrode, a silver electrode, a gold electrode, a ruthenium electrode, a tantalum electrode, and an iridium electrode, or an electrode doped with platinum, silver, gold, ruthenium, tantalum, or iridium.
5. The method for reducing high-valent metal ions as claimed in claim 1, characterized in that The voltage of the external power supply is 0.1V-5V.
6. The method for reducing high-valent metal ions according to claim 1, characterized in that The temperature of the power-on reaction is 0℃≤T1≤110℃.
7. The method for reducing high-valent metal ions according to claim 1, characterized in that The method also includes adding a raw material capable of dissolving high-valent metal ions in an acid and stirring the raw material during the electrical reaction.
Citation Information
Patent Citations
Use of alcohol for increasing the current efficiency of chromium plating
CA1225357A
Method for electrolyzing high-quality nickel from electroless nickel plating wastewater
CN107083559A
Citric acid-tartrate pre-plated copper plating solution and application method thereof
CN108034970A
Oxidation of organic compounds
EP0244812A1
Method of oxidizing organic compound at cathode and anode simultaneously to product specialty chemical
TW226415B