Direct capture of carbon dioxide

By coating calcium adsorbent on the substrate for passive carbonation and regeneration, the problem of high cost and high energy consumption for carbon dioxide removal in the atmosphere in the prior art is solved, and a low-cost and high-efficiency carbon dioxide capture effect is achieved.

CN114901382BActive Publication Date: 2024-11-088 RIVERS CAPITAL LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080090580.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2020-12-03
Publication Date
2024-11-08
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

The prior art methods for efficiently removing carbon dioxide from the atmosphere have high cost and high energy consumption problems, and it is difficult to achieve cost-effectiveness on the industrial scale.

Method used

By adopting the passive carbonation process of calcium adsorbent, the carbon dioxide in ambient air is carbonated by coating a thin layer of calcium hydroxide or other calcium adsorbent on the substrate, and the adsorbent is regenerated through a calciner to reduce the cost. Chemicals and energy dependence.

Benefits of technology

It realizes low-cost and efficient removal of carbon dioxide from the atmosphere, reduces energy costs and equipment requirements, and is suitable for industrial-scale direct air capture systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114901382B_ABST
    Figure CN114901382B_ABST
Patent Text Reader

Abstract

The present disclosure provides systems and methods for direct air capture of carbon dioxide or other gases by calcium sorbents in a manner that allows large-scale, relatively low-cost implementation. In particular, the calcium sorbent can be provided as a substantially thin coating on one or more substrates and used for direct air capture of carbon dioxide by chemical adsorption. The carbonating sorbent can be processed for sequestration of carbon dioxide or regenerated by capturing carbon dioxide released from the carbonating sorbent during a regeneration process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to systems and methods for capturing carbon dioxide. More specifically, the systems and methods can capture carbon dioxide directly from air or other streams by using sorbents. Background Art

[0002] The world is working to address the increasing concentrations of greenhouse gases, particularly carbon dioxide (CO2), in the atmosphere. While much work has been done to reduce the amount of these gases released into the atmosphere each year, there is a growing recognition that reducing emissions alone may not be enough to address the problems associated with climate change. Therefore, research is currently underway into methods that can not only reduce greenhouse gas emissions, but also remove these gases that are already in the atmosphere.

[0003] Considering that global CO2 emissions are about 37 billion tons per year, the current large-scale deployment of CO2 capture from ambient air has not been successful, at least in part due to the high costs associated with known methods. For various reasons, current CO2 removal methods are burdened with high capital costs and high operating costs. For example, because the total CO2 concentration in ambient air is very dilute relative to the main components (such as nitrogen, oxygen and argon), the removal methods previously determined require high specificity and high efficiency to achieve cost-effectiveness. Although efficient removal methods have been determined in the past, such methods lack the ability to allow sufficient volume of ambient air to pass through the capture system to make the known methods simple enough and cost-effective enough for industrial-scale implementation. As a prerequisite for achieving high efficiency, the known removal methods require the use of renewable solvents and / or chemicals to offset the high cost of necessary materials. Therefore, these renewable solvents and / or chemicals used in known capture methods must be separated from the captured CO2 for regeneration, and this separation requirement also adds additional cost and energy to the process.

[0004] Despite a strong desire worldwide to implement CO2 removal technologies as a means of combating climate change, such implementation to date has been unreasonably costly. Without inexpensive technologies to remove existing CO2 from the atmosphere, the world will continue to struggle to reduce and reverse anthropogenic global warming. Therefore, there remains a need in the field for additional technologies that effectively remove greenhouse gases, including CO2, from ambient air. Summary of the invention

[0005] In one or more embodiments, the present disclosure can provide systems and methods suitable for or configured to capture carbon dioxide directly from ambient air. Beneficially, the systems and methods can maximize the available surface area of ​​the calcium adsorbent to increase the amount of carbon dioxide that can be removed from the ambient air. The present disclosure can also effectively minimize the costs associated with an integrated production and logistics system with a passive air capture process while reducing the accumulation of carbon dioxide in the atmosphere.

[0006] The presently disclosed systems and methods can efficiently and directly remove carbon dioxide from ambient air at a relatively low cost, particularly when compared to known carbon dioxide removal systems that require high cost chemicals that must be continuously regenerated. More specifically, the present systems and methods can be adapted or configured to accelerate the carbonation of a calcium sorbent in ambient air, and in some embodiments, this can be achieved by providing the sorbent on one or more substrates in a manner that maximizes the available sorbent surface area and utilizing a designed thickness, whereby the sorbent can be rapidly and thoroughly carbonated.

[0007] Calcium hydroxide has been previously proposed for chemically absorbing carbon dioxide from air (see, “Carbon Dioxide Extraction From Air: Is It An Option?” Lackner, 1999, and “Liquid-Like H2OAdsorption Layers to Catalyze the Ca(OH)2 / CO2 Solid-Gas Reaction and to Form a Non-Protective Solid Product Layer at 20°C” Beruto and Botter, 2000), but there are currently no known systems that effectively exploit these properties for viable direct air capture systems with passive carbonation. Instead, previous systems have relied on actively accelerating direct air capture through carbonators, air contactors, additional solvents, particle reactors, and additional heat and energy input. However, such active processes add significant costs and risks that the currently disclosed systems and methods beneficially avoid. Even known passive calcium direct air capture systems (see Erans et al., 2019) fail to provide a practical integrated system. For example, U.S. Pat. No. 10,570,018 discloses a passive calcium direct air capture system, but the system still fails to meet the necessary requirements for practical implementation (i.e., does not allow for accelerated carbonation at a sufficiently low cost). However, all of these failures can be overcome according to one or more embodiments of the presently disclosed systems and methods, which provide accelerated carbonation at a sufficiently low cost for practical implementation.

[0008] The currently disclosed systems and methods for direct air capture of at least carbon dioxide (i.e., other pollutants can be similarly removed from ambient air using the present disclosure) overcome several limitations in known methods for removing carbon dioxide from air. For example, known methods require efficient, high-speed adsorbents / chemicals to quickly remove carbon dioxide from ambient air. Due to excessive material costs, such processes require effective regeneration of the adsorbents / chemicals. Similarly, in order to achieve rapid turnover, such processes require active airflow (e.g., using a blower) to achieve rapid turnover. The currently disclosed systems and methods alleviate or completely overcome these limitations. As further described herein, the present systems and methods allow the use of low-cost adsorbents / chemicals that have been ignored by the prior art for viable air capture systems due to previously perceived efficiency limitations. Lower-cost adsorbents / chemicals also allow for integrated adsorbent production and capture processes. The present methods and systems can also be effectively performed without the need to fully regenerate the adsorbents / chemicals. In addition, the present methods and systems can be implemented in the apparent absence (if necessary) of any pressurized air components (e.g., blowers) because high efficiency can be achieved even when using slower reaction times. More specifically, the present systems and methods provide implementations for forming high surface area configurations that achieve high efficiency adsorption at low cost, even in the absence of partial or complete adsorbent / chemical regeneration, and even without the use of a pressurized air component.

[0009] In one or more embodiments, the present system and method may be used in conjunction with a passive calcium chemical adsorbent carbonation process. Exemplary embodiments may utilize one or more circulating and / or stationary suspended substrates that may be randomly distributed or specifically organized in a closed, semi-enclosed or covered structure. The circulating substrate may particularly utilize a vertical, horizontal and / or passive conveying system. The calcium adsorbent may be provided substantially in a process-ready state—that is, in a chemical state in which the calcium adsorbent is ready to undergo a spontaneous or catalytically driven process to absorb carbon dioxide. In some embodiments, a calcium adsorbent precursor may be treated to provide a process-ready material. For example, calcium carbonate (CaCO3) may be calcined and slaking to form a calcium hydroxide slurry or suspension. Preferably, this treatment is carried out with partial, substantially complete or substantially complete capture of any carbon dioxide driven by the calcium carbonate. Alternatively or additionally, calcium oxide and / or calcium hydroxide may be provided by further processing in which it is produced, preferably with capture of any produced carbon dioxide.

[0010] The substrate can be coated with a relatively thin layer of calcium hydroxide (or other calcium adsorbents), which can be in the form of a slurry or suspension in particular. This coating can be carried out in any suitable manner, but in particular can be carried out as further described herein. After coating, the coated substrate can be placed in the desired area of ​​the structure and remain substantially stationary. Alternatively, the coated substrate can be circulated in at least a portion of the structure. The coated substrate is contacted with ambient air for a sufficiently long time to evaporate (i.e., release H from calcium hydroxide O) and carbonate (i.e., absorb CO from air) to the desired amount. The carbonating coating that has absorbed a certain amount of carbon dioxide from the atmosphere can be removed from the substrate, and the substrate that has been substantially cleaned can be reused. The removed coating can be exported from the site for different processes, industrial uses, sales and / or sequestration. In some embodiments, the calcium adsorbent can be regenerated to be used again. For example, if desired, the carbonating material can be further carbonated before being treated by a calciner to drive off carbon dioxide, and the carbon dioxide can be captured for sequestration or for other purposes (e.g., enhancing oil recovery). This calcination can also generate calcium oxide. It can then be slaked to form calcium hydroxide for coating on substrates for further direct air capture of carbon dioxide.

[0011] Systems according to the present disclosure may include any combination of individual components and / or units for implementing process steps. For example, in some embodiments, a suitable system may include: a calciner, which is preferably suitable for or configured to capture at least a portion, substantially all, or all of the carbon dioxide released in the calciner. The system may also include a slaking device, a conveyor system (which may be suitable for or configured to operate with one or both of the vertical and horizontal parts), and one or more substrates that are suitable for or configured to be suspended at least partially above the ground level. The components of the system may exist in a single structure or in multiple structures.

[0012] The foregoing systems and methods, described in more detail below, provide distinct advantages over known calcium adsorbent applications for carbon dioxide capture. In particular, the present systems and methods provide for maximizing the surface area of ​​the calcium adsorbent, and therefore also maximizing the carbonation efficiency of the calcium adsorbent, while minimizing energy costs. In some embodiments, this can be achieved, in particular, by tailoring the coating thickness of the adsorbent on the substrate to obtain the most efficient rate of carbon dioxide transfer to the adsorbent. Thus, this particular design improves the performance of the direct air capture system and reduces costs.

[0013] The present disclosure provides further advantages over known carbon dioxide capture systems. For example, passive capture of carbon dioxide using high surface area adsorbents discussed herein can reduce, substantially eliminate, or completely eliminate the need for expensive equipment, such as air contactors, packed towers, fans, pumps and compressors, carbonators and / or particle reactors. In one or more embodiments, this advantageous high surface area arrangement can be achieved by using a relatively thin calcium adsorbent layer on one or more substrates used. Exemplary embodiments of suitable layer thicknesses can be within the range of about 1.5 kg or less of calcium adsorbent per square meter of exposed area of ​​the substrate. The thin layer can be arranged to have a relatively high vertical density, such as greater than five feet high, while maintaining the thinness of each individual calcium adsorbent layer. This combination of high surface area and low layer thickness can provide direct air capture of carbon dioxide within a reasonable length of time (e.g., a scale of several hours to several months, depending on the exact coating parameters and the desired processing output) without the need for excessive land cover. In addition, this substrate-based deposition method allows for thinner application of calcium adsorbents in practical and efficient arrangements, which at least solves some challenges and problems that were not solved by previous passive direct air capture systems. Thus, the present systems and methods can significantly outperform previously contemplated faster but more capital and energy intensive direct air capture systems, while also providing efficiencies previously unattainable in previous passive direct air capture systems.

[0014] In addition to the above, the reduction or elimination of any active air capture mechanisms can also reduce the associated equipment and the cost of generating the electricity and heat required to operate them. Thus, heating and operating the capture system produces less carbon dioxide, and the net carbon removal of the present system can significantly exceed that achievable with known systems and methods.

[0015] Spent calcium adsorbent (i.e., adsorbent that has been used for passive capture of carbon dioxide) can be calcined, thus separating the absorbed carbon dioxide for storage, thereby regenerating the calcium adsorbent for further air capture. This regeneration reduces the demand for limestone to produce the calcium adsorbent. Although calcination of calcium oxide (CaO) is a common process, it is combined with the passive high-density CaO carbonation process of the present application to effectively provide significant improvements in cost and energy use for the entire cycle of adsorbent use and regeneration compared to other direct air capture systems. Unlike previously described processes, the systems and methods of the present disclosure do not require additional chemicals or materials in the air capture stage that would complicate the calcination of the calcium adsorbent for use subsequent to carbon dioxide capture.

[0016] Previously disclosed methods for direct air capture using calcium oxide or calcium hydroxide do not manage the space and time required to scale up the methods to an industrial level, even when passive systems are proposed. Calcium adsorbents have been considered for direct air capture for approximately 20 years, but systems have never been developed to make passive capture of carbon dioxide by calcium feasible on a useful scale. The present disclosure addresses this challenge because of its full system design of high-density storage and logistics processes that apply a thin adsorbent layer to accelerate carbonation and minimize space and cost during carbonation, allowing passive direct air capture processes to operate effectively on an industrial scale.

[0017] In one or more embodiments, the present disclosure may provide, in particular, methods for direct air capture of carbon dioxide. In an exemplary embodiment, such methods may include: preparing a substantially continuous coating of a calcium adsorbent material having a density of less than 10 kg / m2 on one or more substrates; contacting one or more substrates having a substantially continuous coating of a calcium adsorbent material with air containing carbon dioxide for a sufficient period of time to allow the calcium adsorbent to react with the carbon dioxide, thereby capturing at least a portion of the carbon dioxide from the air and converting at least a portion of the calcium adsorbent to a carbonated form; removing at least a portion of the carbonated form of the calcium adsorbent from one or more substrates; and treating the carbonated form of the calcium adsorbent so that the carbon dioxide captured from the air is ready for storage or for other uses. In further embodiments, the method may be further limited to involving one or more of the following statements, which may be combined in any number and / or order.

[0018] The density of the substantially continuous coating of calcium adsorbent material is from about 0.1 ksm to about 5 ksm.

[0019] The substantially continuous coating of calcium sorbent material on the one or more substrates has an average thickness of less than 2.5 cm.

[0020] The substantially continuous coating of the calcium adsorbent material on the one or more substrates has an average thickness of about 0.01 mm to about 2 cm.

[0021] The one or more substrates are substantially configured as a sheet.

[0022] The substantially continuous coating of calcium adsorbent material is configured to exhibit a carbonation rate such that at least 25% by weight of the calcium adsorbent material is carbonated in 96 hours or less.

[0023] The substantially continuous coating of calcium adsorbent material is configured to exhibit a carbonation rate such that at least 50% by weight of the calcium adsorbent material is carbonated within a period of about 1 day to about 14 days.

[0024] Contacting the one or more substrates having the substantially continuous coating of calcium adsorbent material with air containing carbon dioxide includes suspending the one or more substrates having the substantially continuous coating of calcium adsorbent material at a location where the substantially continuous coating of calcium adsorbent material contacts the air.

[0025] Removing at least a portion of the carbonated form of the calcium sorbent from the one or more substrates includes subjecting the one or more substrates to a force sufficient to break and dissociate the substantially continuous coating of the calcium sorbent material from the one or more substrates.

[0026] Treating the carbonated form of the calcium sorbent may include granulating the carbonated form of the calcium sorbent to seal the carbonated form of the calcium sorbent.

[0027] Treating the carbonated form of the calcium sorbent may include further contacting the carbonated form of the calcium sorbent with ambient air for a time sufficient to increase the carbonation percentage.

[0028] Treating the carbonated form of the calcium sorbent may include: calcining the carbonated form of the calcium sorbent to release carbon dioxide therefrom and form calcium oxide; and capturing the carbon dioxide released from the calcium sorbent.

[0029] The method also includes slaking the calcium oxide to form a calcium sorbent material for preparing a substantially continuous coating.

[0030] The method also includes removing a portion of the carbonated form of the calcium sorbent prior to calcining and adding supplemental limestone during calcining.

[0031] The preparing a substantially continuous coating of calcium adsorbent material may include immersing one or more substrates in a reservoir of calcium adsorbent material.

[0032] Said preparing a substantially continuous coating of calcium adsorbent material may comprise dripping or spraying the calcium adsorbent material onto one or more substrates.

[0033] In one or more embodiments, the present invention further provides, inter alia, a system for direct air capture of carbon dioxide. In an exemplary embodiment, such a system may include: a coating system configured to apply a liquid calcium adsorbent material to one or more substrates to form a substantially continuous coating of the calcium adsorbent material on the one or more substrates; a storage unit configured to place the one or more substrates for a period of time, wherein the one or more substrates are in contact with air so that carbon dioxide in the air reacts with the calcium adsorbent material to form a calcium carbonate adsorbent material; and a collection unit configured to remove and collect the calcium carbonate adsorbent material from the one or more substrates. In further embodiments, the system may be further defined to involve one or more of the following statements, which may be combined in any number and / or order.

[0034] The coating system may include one or more reservoirs of liquid calcium sorbent material.

[0035] The coating system may further include a dipping unit configured to dip the one or more substrates into the one or more reservoirs of liquid calcium sorbent material.

[0036] The coating system may include a suspension unit configured to maintain one or more substrates in a substantially vertical position.

[0037] The coating system may further include one or more droppers configured to drop the calcium sorbent material onto the one or more substrates.

[0038] The system may also include a calciner configured to receive the calcium carbonate sorbent material and convert the calcium carbonate sorbent material into calcium oxide and carbon dioxide.

[0039] The system may also include a solids separator configured to separate the calcium oxide from the carbon dioxide.

[0040] The system may further include a lime slaking unit configured to receive calcium oxide and form calcium hydroxide for use as a calcium sorbent material.

[0041] By reading the following specific embodiments and the accompanying drawings briefly described below, these and other features, aspects and advantages of the present disclosure will be apparent. The present invention includes any combination of two, three, four or more of the above-mentioned embodiments and any combination of two, three, four or more features or elements set forth in the present disclosure, regardless of whether these features or elements are explicitly combined in the specific embodiment description herein. The present disclosure is intended to be interpreted as a whole, so that any separable features or elements of the disclosed invention in any of its various aspects and embodiments should be deemed to be intended to be combinable, unless the context clearly indicates otherwise. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1A is an illustration of a substrate coated with a substantially continuous layer of calcium adsorbent material according to an exemplary embodiment of the present disclosure.

[0043] Figure 1B is a partial cross-sectional view of a substrate coated with a substantially continuous layer of calcium adsorbent material according to an exemplary embodiment of the present disclosure.

[0044] Figure 2 is an illustration of a substrate being immersed in a reservoir containing a liquid calcium adsorbent material to form a substantially continuous layer of calcium adsorbent material on the substrate according to an exemplary embodiment of the present disclosure.

[0045] Figure 3is a flow chart showing a system and method for direct air capture of carbon dioxide according to an exemplary embodiment of the present disclosure.

[0046] Figure 4 is a flow chart showing example details of coating and removing sorbents in a system and method for direct air capture of carbon dioxide according to an exemplary embodiment of the present disclosure.

[0047] Figure 5 is a flow chart showing another example detail of coating and removing sorbent in a system and method for direct air capture of carbon dioxide according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION

[0048] Various aspects of the disclosure will now be described more fully below with reference to the accompanying drawings, in which some but not all embodiments of the disclosure are shown. In fact, various embodiments of the disclosure can be expressed in many different forms and should not be construed as limited to the embodiments set forth herein; on the contrary, these exemplary embodiments are provided to make the disclosure comprehensive and complete and will fully convey the scope of the disclosure to those skilled in the art. As used in the specification and the appended claims, the singular forms "a", "an", "the" include plural referents unless the context clearly indicates otherwise.

[0049] In one or more embodiments, the present disclosure provides systems and methods for directly capturing carbon dioxide from ambient air or atmospheric air. The systems and methods use a calcium adsorbent, which is preferably regenerable, but if necessary, it can be configured for non-regenerable applications. In some embodiments, the calcium adsorbent can be configured to cycle carbonation and calcination so that carbon dioxide can be removed from the atmosphere by absorption by the adsorbent and then captured during the regeneration of the adsorbent. For example, calcium oxide and / or calcium hydroxide can be used as the calcium adsorbent. Therefore, the calcium adsorbent can be adapted to or configured to spontaneously or catalytically absorb carbon dioxide from ambient air as needed. This absorption can effectively form the calcium adsorbent in a carbonated form, which can then be regenerated by calcination to discharge carbon dioxide, which can be captured during the calcination process.

[0050] In order to form the calcium adsorbent of initial calcium adsorbent and / or regenerated carbonated form, carbonate (e.g., calcium carbonate-CaCO ) can be injected into a calciner, which is preferably equipped with appropriate components to capture the carbon dioxide emitted during at least a portion of the calcination process. The limestone used to form the adsorbent can be provided in granular form to ensure that an entrained flow, rotary kiln or fluidized bed calciner can be used for CaO production. In some embodiments, the granular limestone / CaCO can have an average size of about 1 μm to about 1 mm, about 5 μm to about 750 μm or about 10 μm to about 500 μm (e.g., for irregularly shaped particles, the maximum measurable size of length, width or thickness). As further discussed below, the calcium oxide so formed can be further processed before being applied to the substrate for the carbonation reaction.

[0051] The capture assembly associated with the calciner preferably effectively captures at least 75%, at least 85%, at least 90%, at least 95%, at least 99% or at least 99.9% of the carbon dioxide released by the carbonate during the calcination process. In some embodiments, the calcination can be carried out by heating the carbonate to a temperature in the range of about 700°C to about 1200°C, about 750°C to about 1100°C, or about 800°C to about 1000°C. The released carbon dioxide can effectively form calcium oxide (CaO). At least a portion of the carbon dioxide captured by calcination can be used for industrial processes, enhanced oil recovery or storage. Non-limiting examples of capture technologies that can be implemented to capture carbon dioxide released in calcination can include oxy-fired calcination, calcium-based chemical looping, amine-based solvent technology, etc. Calcination for providing low-carbon CaO can be carried out on-site at the direct air capture device, and can therefore be part of an integrated system for continuous or batch processing. If desired, calcination can be carried out off-site or by a third party. Therefore, the carbonate content can be transported to a calcination site for regeneration of the calcium sorbent and carbon capture and then transported back to the direct air capture plant.

[0052] The CaO may remain in its dehydrated form, may be hydrated with water to form calcium hydroxide (Ca(OH)2), or may be a mixture of the two, all of which are interchangeably referred to as "calcium adsorbents" or "lime adsorbents". Thus, in addition to the calcination unit mentioned above, a slaking unit may be used to prepare an initial adsorbent and / or regenerate an adsorbent from a carbonation product. The calcium hydroxide and / or CaO may be further mixed with additional water to provide a calcium adsorbent in a suitable form for addition to one or more substrates. Thus, prior to addition to the substrate, the adsorbent may be any one or more of a paste, a slurry, a spray, or a suspension. Furthermore, in some embodiments, the calcium adsorbent may be prepared in a polymeric form, as a metal organic framework material (MOF), or another suitable mixture and / or molecular structure. The calcium adsorbent is preferably provided in any suitable form, whereby the calcium adsorbent can capture carbon dioxide from ambient air. For example, calcium hydroxide can capture carbon dioxide from the air when the relative humidity is above 40%, as the presence of water is generally believed to be key to the capture of carbon dioxide by calcium hydroxide to produce calcium carbonate. Carbon dioxide in the air can dissolve in water to form carbonic acid (H2CO3), which can decompose into HCO3 - and H + , thereby reacting with calcium to form calcium carbonate and capturing carbon dioxide.

[0053] In some embodiments, the calcium adsorbent added to one or more substrates may contain the calcium material itself and water, consist essentially of the calcium material itself and water, or consist essentially only of the calcium material itself and water. However, in other embodiments, one or more additional chemicals or materials may be included, and may be suitable for or configured to improve the carbon dioxide chemical adsorption properties of the calcium adsorbent and / or improve the adhesion of the calcium adsorbent to the substrate. Similarly, the calcium adsorbent may have a specific morphology, which may be suitable for or configured to improve the carbon dioxide chemical adsorption characteristics of the calcium adsorbent. Such improvements may include any one or more of reactivity, viscosity, porosity, surface area, morphological stability and electronegativity and other beneficial properties. In an exemplary embodiment, sodium hydroxide may be added to the adsorbent in particular. In other embodiments, potassium hydroxide, magnesium hydroxide, fumed silica, zeolite, magnetic particles and / or recycled regenerated adsorbents may be added. In addition to the above mixtures, the calcium adsorbent may be formed into powders, pellets, flakes, slurries, gels, honeycombs, and / or may be provided in other beneficial geometric shapes. Aging, drying, rehydrating, bending, flowing, vibrating, rolling, squeezing, charging, and other such manipulations may be applied to the sorbent as they have been shown to affect the reactivity and performance of the calcium sorbent applied to one or more substrates.

[0054] Applying the calcium adsorbent to the substrate can be carried out in a coating unit or device. The calcium adsorbent of the composition and / or form described above can be applied to one or more substrates in a relatively thin layer. For example, the average adsorbent layer thickness on a representative area of ​​the substrate can be less than 2.5 cm, less than 2 cm, less than 1.5 cm or less than 1 cm (e.g., as low as the minimum coating thickness achievable by a conventional coating method). In some embodiments, the average layer thickness can be in the range of about 0.01 mm to about 2.25 cm, about 0.01 mm to about 2 cm, about 0.01 mm to about 1.5 cm, about 0.01 mm to about 1 cm, about 0.01 mm to about 7 mm, about 0.01 mm to about 5 mm, about 0.02 mm to about 1 mm, or about 0.03 mm to about 0.5 mm. Although the foregoing ranges relate to a variety of useful embodiments according to the present disclosure, it should be understood that more specific ranges can be implemented based on the exact physical properties of the adsorbent coating material. For example, in some embodiments, the calcium adsorbent material can be provided in a substantially porous form, which provides an increased surface area for reacting with carbon dioxide. In such an embodiment, relatively thick coating can be used, while still providing high carbonation percentage, as discussed further below.For example, when using relatively thick coating, average layer thickness can be in the scope of about 0.5mm to about 2.25cm, about 0.75mm to about 2cm, about 1mm to about 1.5cm or about 1.5mm to about 1cm.In further exemplary embodiments, relatively thin coating can be used, and the process can be further simplified, because extra processing (as, in order to realize high porosity, as mentioned above) can be avoided, and substantially continuous coating can be applied with relatively small average thickness, while still reaching required carbonation percentage.In such an embodiment, when using relatively thin coating, average layer thickness can be in the scope of about 0.01mm to about 2mm, about 0.05mm to about 1.5mm or about 0.1mm to about 1mm.Average thickness can relate to the monolayer of calcium adsorbent, or can be the gross thickness of a plurality of layers (as, 2,3,4 or 5 layers) applied to substrate. Figure 1A and Figure 1B A representative substrate 10 is shown having a calcium adsorbent coating 20 applied thereto. Figure 1A As shown, coating 20 may cover less than the entire surface 11 of substrate 10, but if desired, the coating may cover substantially the entire surface. Figure 1B As shown, the thickness of coating 20 may be less than the thickness of the substrate; however, the substrate thickness may vary depending on the particular material used to form the substrate.

[0055] Preferably, the average adsorbent layer thickness is adapted or configured to provide a calcium adsorbent density within a defined range. As described above, useful calcium adsorbent densities may vary based on the average layer thickness used. Within all desired ranges, the calcium adsorbent density may be, for example, about 10 kg / m 2 (ksm or less), less than 5ksm, less than 2ksm, or less than 1ksm of exposed substrate area (e.g., at least 0.02ksm). In some embodiments, the calcium adsorbent density on the substrate may be in the range of about 0.05ksm to about 10ksm, about 0.1ksm to about 5ksm, about 0.2ksm to about 2ksm, or about 0.25ksm to about 1ksm. Various mechanisms can be used to manage the layer thickness, such as controlling the content of water mixed with the calcium adsorbent to form the coating mixture. This (or other factors) can be used to control the viscosity of the coating mixture, thereby controlling the coating thickness of the coating mixture. In some embodiments, this relatively thin nature of the calcium adsorbent layer can be particularly effective in allowing passive capture of carbon dioxide. Although calcium oxide captures carbon dioxide under ambient conditions, the reaction rate is limited by the thickness of the coating, and relatively thick layers essentially stop reacting below a certain depth. However, in some embodiments, the coating thickness can be increased by controlling one or more physical properties of the coating. For example, when the coating is provided in a relatively high porosity form, the coating thickness at the higher end of the above range may be particularly useful. Similarly, the substrate may have a three-dimensional structure that allows for greater layering of the adsorbent thereon. In an exemplary embodiment, the calcium adsorbent may be prepared substantially in the form of a foam exhibiting an at least partially open cell structure that effectively allows air to penetrate deeper into the layer thickness for reaction of carbon dioxide in the air with the adsorbent.

[0056] The present system and method can operate within the limited carbonation rate of adsorbent. In some embodiments, the carbonation rate can be maximized so that about 50% or more, about 60% or more, about 70% or more, or about 80% or more of the adsorbent by weight is carbonated before being removed from the substrate. For example, removal of the carbonation substrate can occur after the carbonation of the adsorbent reaches about 60% to about 98%, about 65% to about 95%, or about 75% to about 90% by weight. Since known treatments either require the use of other types of adsorbents / chemicals, or are configured to be used with adsorbents that cannot achieve such high levels of carbonation due to structural limitations (such as, required adsorbent layer thickness), it is expected that such high levels of carbonation cannot be achieved by optimizing known treatments. In other embodiments, when high throughput processing is required, the carbonation percentage can be minimized to increase the system throughput. For example, removal of the carbonation substrate can occur after the carbonation of the adsorbent reaches about 25% to about 75%, about 30% to about 65%, or about 35% to about 60% by weight. By utilizing such a concentration limit, the turnover rate of the adsorbent can be increased, thereby maximizing the total mass of carbon dioxide that can be removed by a given system. This is because the chemical adsorption rate can be significantly faster when the percentage of carbonation of the adsorbent is low, and the carbonation rate can slow significantly as the relative percentage of the adsorbent that has been carbonated increases.

[0057] By applying a determined calcium adsorbent coating thickness, coating density, and desired carbonation percentage, the calcium adsorbent layer applied to one or more substrates may be configured or adapted to provide a carbonation rate within defined parameters. It is expected that such a carbonation rate is not inherent to the calcium adsorbent, as the carbonation rate is a function of the above factors. In some embodiments, the calcium adsorbent coating formed on one or more substrates may be configured or adapted to exhibit a carbonation rate such that at least 25%, at least 30%, at least 35%, at least 40%, or 45% of the calcium adsorbent coating by weight is carbonated within a time of 96 hours or less, 84 hours or less, 72 hours or less, 60 hours or less, 48 ​​hours or less, 36 hours or less, or 24 hours or less (e.g., the shortest carbonation time is 1 hour). More specifically, the calcium adsorbent coating formed on one or more substrates may be configured or adapted to exhibit a carbonation rate such that about 25% to about 50%, about 25% to about 45%, or about 30% to about 45% by weight of the calcium adsorbent coating is carbonated within a period of about 2 hours to about 96 hours, about 4 hours to about 84 hours, about 6 hours to about 72 hours, about 8 hours to about 60 hours, about 10 hours to about 48 hours, or about 12 hours to about 36 hours. Such a carbonation rate can be achieved by controlling one or more of the above factors, thereby enabling a relatively high throughput system and method. This can be advantageous when the calcium adsorbent is regenerated, and such a high throughput can increase the total volume or mass of carbon dioxide removed from the air in a given period of time.

[0058] In some embodiments, it may be necessary to provide a more complete carbonation of the calcium adsorbent coating before removing the coating from the substrate. Such an embodiment is advantageous when the calcium carbonate adsorbent is not regenerated (i.e., it will be sealed in the form of calcium carbonate, which is removed from the substrate without calcination to release carbon dioxide) or the system space is large enough to allow a longer carbonation time. Therefore, in such an embodiment, the calcium adsorbent coating formed on one or more substrates can be configured to or suitable for showing a carbonation rate that makes at least 50%, at least 60%, at least 70%, at least 80%, or at least 90% of the calcium adsorbent coating by weight carbonated in a time of about 0.5 days to about 14 days, about 1 day to about 12 days, about 1.25 days to about 10 days, or about 1.5 days to about 8 days. The carbonation rate can be evaluated by sampling the calcium adsorbent coating at different times after the coating is formed and chemically analyzing the adsorbent (e.g., by mass spectrometry or similar analytical methods effective for identifying chemical components).

[0059] Applying the calcium adsorbent to one or more substrates may be accomplished by any suitable method or combination thereof. In some embodiments, the application may be accomplished by dipping the substrate directly into the calcium adsorbent or spraying the calcium adsorbent onto the substrate. In other embodiments, the application may be accomplished by using a brush, a scraper, a blowing mechanism, dripping, pouring, or any other method suitable for applying a thin layer of the adsorbent to the substrate. For example, Figure 2 As shown, the substrate 10 can be immersed in a reservoir 30 (e.g., in the form of a tank) containing a calcium adsorbent 25. A fixture 40 is attached to the substrate 10 for manipulating the substrate during the dipping process. Alternatively, when the calcium adsorbent 25 is dripped or sprayed onto the substrate, the substrate 10 can pass over the reservoir 30 so that excess adsorbent falls into the reservoir for recycling to the application assembly (e.g., a sprayer). One or more layers can be applied to the substrate. The application method can be adapted or configured to affect the physical properties of the applied adsorbent. The method of applying the calcium adsorbent to the substrate can be changed as needed to increase production volume; however, certain modes of applying the calcium adsorbent may be preferred in terms of increasing the reactivity of the calcium adsorbent with carbon dioxide. For example, blowing the adsorbent onto the substrate can effectively obtain a coating with increased porosity, which can improve the ability to perform chemical adsorption using a thicker layer, as described above. In some embodiments, the coating of the calcium adsorbent can be specifically characterized as a substantially continuous layer (or multiple layers) on the substrate. Thus, the coating may be referred to as being in the form of a film, sheet, membrane, etc. A "substantially" continuous coating may mean that while certain defects in the coating or layer (e.g., cracks, dents, and similar defects) are taken into account, the coating does not exist in the form of discrete fragments or particles that exist as separate elements (even though individual elements may be in physical contact with other individual elements). Rather, the coating or layer extends along the length of the substrate surface as an intact film, sheet, membrane, etc. In certain embodiments, the coating of the present disclosure may specifically exclude spherical lime-based adsorbents or other lime-based adsorbents in the form of granules. The use of such granular or spherical adsorbents may be disadvantageous because the additional complexity of forming the granules or pellets may require mixing the adsorbent with a filler, a binder, etc., and then spray drying or otherwise treating the mixture to form discrete solid particles or pellets. Such granular materials may also require additional processing to adhere to the substrate and more complex processing to remove the adhered particles for regeneration. Alternatively, such granules or pellets must be placed in a packed bed reactor so that air with carbon dioxide can be treated by the packed bed, which again introduces complexity that is not present in the method according to the present disclosure.

[0060] The substrate itself may not have a coating, or it may have adhesives, anti-adhesives, catalysts, polymers and other additives applied before the calcium adsorbent is applied to improve its performance, life, surface area and / or processability. The substrate surface may be two-dimensional (i.e., substantially flat) or three-dimensional (i.e., sheared, textured, shaped, curved, etc.) to improve the application, performance, reactivity, surface area and processability of the calcium adsorbent. It may be sought to increase the surface area to accelerate the carbonation reaction, and it may be sought to increase the adsorbent volume per unit of substrate material to reduce the cost associated with the substrate material. Plastic is a possible substrate because it is low in cost, flexible in structure, durable and does not react with calcium. In other embodiments, wood products, foam boards, steel or any such substrates suitable for this purpose.

[0061] When placed on a flat surface or in a suspended configuration, the substrate may be adapted to or configured to be substantially flat. In other embodiments, the substrate may be intentionally adapted to or configured to have a three-dimensional shape as described above. For example, the substrate may be shaped as a cylinder, a cone or other shapes, and it is advantageous that all exposed sides of the substrate are coated with calcium adsorbent to increase the surface area per unit of substrate material. In some exemplary embodiments, the substrate may be a curled configuration so as to have a substantially spiral cross-section. In other embodiments, the substrate may be adapted to or configured to have a porous network, wherein the pores are large enough to not only allow liquid adsorbent to flow through and coat the surface of the substrate, but also large enough to allow the carbonated adsorbent to be removed from the substrate. For example, a honeycomb structure such as commonly used in a catalytic converter (e.g., for the automotive industry or for the exhaust system of a power plant industry) may be used, and the pore size of the honeycomb structure may be appropriately adjusted to allow the effective removal of the carbonated adsorbent. This structure is usually made of ceramic, but metal honeycombs may also be used to improve durability.

[0062] The substrate can be rotated, moved, rotated, blown or otherwise operated to affect the drying of the calcium adsorbent on the substrate material. Similarly, a blower or the like can be used to remove excess adsorbent from the coating surface and ensure a substantially uniform and appropriately thin adsorbent coating on the substrate surface. The substrate can be replaced by a rod, tray, plate or other substrate that allows the application of a thin calcium adsorbent. In some embodiments, the calcium adsorbent can be deposited so that it has enough structural integrity to be suspended, upright or placed without any other substrate or material. A plurality of such substrates can be combined in a system to maximize its performance and minimize waste or loss of adsorbent material.

[0063] After the adsorbent is coated on one or more substrates, the coated substrate can be moved to a storage unit or device. The substrate material coated with the calcium adsorbent can be stored or otherwise positioned for contact with ambient air for a sufficiently long time to achieve the desired adsorbent carbonation percentage as described above. This time can be referred to as a reaction period or carbonation period. In some embodiments, the scope of the reaction period can be as little as a few hours or as much as a few months, or longer if necessary. During the reaction period, the adsorbent chemically absorbs carbon dioxide from ambient air or other concentrated carbon dioxide sources. Evaporation also occurs, both from the water added to the calcium adsorbent and from the water released in the reaction of calcium hydroxide and carbon dioxide to generate calcium carbonate and water. During the evaporation of water used to form the substrate mixture, the adsorbent layer will show an initial weight decrease, followed by an increase in weight due to carbonation.

[0064] The presently disclosed systems and methods advantageously provide for storage and transport of sorbent-coated substrates during carbonation in a manner that achieves particularly desired results. One or more substrates having calcium sorbent applied thereto may be arranged to be vertically attached to a conveyor system, suspended statically from above, supported by other substrates, or held by the sides or bottom of the substrate. This use of vertical space minimizes the land area used without a large amount of additional infrastructure and allows for drying on two or more sides on a conveyor system or the like. In some embodiments, the conveyor system may be adapted or configured to move the substrates through a storage unit for at least a portion or all of the duration of carbonation. This may be configured as a continuous conveyor line, a branching conveyor system, or multiple separate conveyor systems. In addition to or in lieu of vertically suspended storage, horizontally stacked substrates may also be used during and after the initial drying process, and on or off the conveyor system.

[0065] In one exemplary embodiment, the calcium adsorbent may be first applied to a substantially vertical hanging substrate to allow for two-sided application (see Figure 2 ), and after the initial stage of carbonation, the partially carbonated sorbent can be removed and placed in a substantially horizontal delivery system, which can effectively expose the surface area of ​​the sorbent attached to the substrate material to ambient air, thereby accelerating carbonation. In another exemplary embodiment, the calcium sorbent can be applied alone to a vertical substrate, and after the carbonation period is sufficiently completed, at least a portion of the carbonated sorbent can be removed and calcined to regenerate the sorbent.

[0066] The storage unit or device may include suitable covers suitable for or configured to protect the calcium adsorbent from weather (e.g., rain) that may disrupt the carbonation process. The storage unit or device may or may not be close to air, depending on the climate of the area. The temperature, relative humidity, and airflow of the storage space may be controlled to optimize carbonation, or they may fluctuate with ambient conditions. Therefore, the storage unit or device may include suitable climate control elements, air inlets, etc. suitable for or configured to provide ambient air inflow for carbon dioxide removal. For example, the storage unit or device may include one or more air movers (e.g., fans, blowers, etc.) configured or suitable to increase air circulation in the storage unit or device and ensure that the carbon dioxide concentration in the air close to the calcium adsorbent is not lower than a range that may reduce process efficiency (e.g., the average ambient air CO2 content of the air entering the device is -5%, -10%, -15% or -20%). As another example, the storage unit or device may include one or more heaters and / or one or more coolers configured or suitable to adjust the temperature to a desired range to improve process efficiency. As yet another example, the storage unit or device may include one or more humidity regulators that may be configured or adapted to maintain the relative humidity (RH) in the storage unit or device within a desired range suitable for improving process efficiency (e.g., greater than 40% RH, greater than 50% RH, or greater than 60% RH, such as within a range of about 45% to about 90%, about 45% to about 80%, or about 50% to about 75% RH). In addition, in some embodiments, excess carbon dioxide (or other gas) above that present in ambient air may be fed into the storage unit to accelerate carbonation. In some embodiments, the storage unit or device may incorporate natural topographical features, such as canyons, waterways, cliffs, or caves, so that airflow, air temperature, and / or air humidity are more suitable for process performance.

[0067] After the calcium adsorbent has achieved sufficient carbonation within the desired range, the captured carbon dioxide can be further processed for storage. In some embodiments, the carbonated adsorbent can be removed from the substrate material for further processing. In other embodiments, the substrate material may be suitable or configured to be stored geologically with the carbonated adsorbent, or the substrate may be suitable for processing with the carbonated adsorbent through a calciner. Thus, the substrate may be reusable or may be sacrificial. In the case of removal, removing at least a portion of the carbonated form of the calcium adsorbent from one or more substrates may include subjecting one or more substrates to a force sufficient to break the coating of the calcium adsorbent material and dissociate the coating of the calcium adsorbent material from one or more substrates. Fracture may mean breaking into multiple pieces for ease of processing, and breaking the coating may increase the ability of the coating to easily dissociate from the substrate.

[0068] Flexible substrates can be used so that the bending / flexing of the substrate can be sufficient to remove the basically fragile carbonated sorbent. Therefore, subjecting the substrate to the force sufficient to fracture and dissociate the coating can include any force that causes the substrate to bend and / or flex. Alternatively or additionally, the force that the substrate may be subjected to can include shaking, scraping, blowing, vibration, rolling, extrusion rolling, impact pulse, electrostatic pulse, electromagnetic pulse, magnetic force and / or a variety of other methods for removing the carbonated sorbent from the substrate material. Mechanical force may be desirable in some embodiments because various forms of mechanical force can be applied in a cost-effective manner. In other embodiments, sound or impact force / pulse can be applied more easily. In some embodiments, the removal of sorbent can be enhanced by various compositions and / or surface treatments of the substrate. Once removed, additional time can be given to the sorbent material to be carbonated, assuming that additional surface area has been newly exposed, or it can be processed immediately.

[0069] The carbonated adsorbent can be regenerated by a calciner in substantially the same manner as the above-mentioned preparation of the original calcium adsorbent material for reuse. After carbonation, the adsorbent material of the initial first chemical composition (e.g., calcium hydroxide and / or calcium oxide) has been converted into a different chemical composition, namely calcium carbonate. Calcium carbonate can be processed by a calciner with carbon capture. By heating calcium carbonate again to a temperature higher than about 800° C., carbon dioxide is released and then captured for storage and utilization. The captured carbon dioxide is substantially or entirely carbon dioxide extracted from ambient air. In addition, calcium oxide is formed again and can be sent back as an input for calcium adsorbent, thereby reducing the demand for additional limestone input.

[0070] The re-calcination (or regeneration) portion of the process has similarities to the calcium cycle. Unlike the calcium cycle, a carbonator is not required because carbonation occurs through long-term exposure to air. The characteristics of the calcium cycle are well known, and it is known that calcium oxide will continue to chemically adsorb carbon dioxide when it circulates from calcium oxide to calcium carbonate and then back to calcium oxide, but it will also lose its reactivity after a certain number of cycles. For example, after as few as five cycles of continuous use of a calciner and a carbonator, the carbonation conversion rate can drop below 50%. However, the system and method disclosed in the present application can alleviate this adsorbent deactivation. In particular, by at least partially slaking the calcium oxide, water can promote the reaction between calcium oxide and carbon dioxide. In addition, the removal of the carbonation reactor (usually operated at about 650°C) eliminates wear and sintering problems. Further, the residence time of the reaction of calcium hydroxide and carbon dioxide in the system and method of the present application is significantly longer than the residence time of calcium oxide and carbon dioxide in a typical high-temperature carbonator. The cycle between carbonation and calcination can be from a few cycles to hundreds of cycles, thereby reducing the cost of limestone.

[0071] Insofar as deactivation of the calcium adsorbent may occur so that the efficiency drops to a specified level, the deactivated adsorbent may be disposed of in any one or more forms of CaO, Ca(OH)2 and CaCO3. The waste material may be used as a product for industries such as cement, agriculture or road aggregates, where CaO and limestone of similar chemical properties are used as inputs. Alternatively, the waste may be processed for the disposal of the material. Insofar as the disposal of CaCO3 is concerned, it may also be used as a mineral to sequester carbon dioxide from the air, isolating it from the atmosphere for thousands of years in the form of stone. Therefore, at least a portion of the calcium carbonate removed from the substrate after carbonation has been carried out may be disposed of in a manner that allows the captured carbon dioxide to be sequestered. In some cases, the calcium adsorbent may skip the re-calcination stage after the first carbonation and be immediately stored underground as a stable, non-toxic mineral CaCO3 formed during the carbonation process. Due to the passive low-input system developed herein, this mineral carbon dioxide storage is potentially attractive in areas where limestone costs are low and geological conditions are insufficient for traditional carbon dioxide sequestration.

[0072] Figure 3 Exemplary embodiments of overall systems and methods according to the present disclosure are provided. As shown therein, the exemplary systems and methods can use relatively tall substrates (e.g., "sheets") that are immersed in a reservoir (i.e., "dip tank") containing a liquid calcium sorbent (e.g., in the form of calcium hydroxide) as they are transported by a vertical conveyor. These substrates are suspended from the ceiling and the conveyor transports them during the carbonation process until the carbonated sorbent is removed for further processing.

[0073] exist Figure 3In an embodiment of the present invention, the coating system 32 may include an immersion unit 35 for immersing a substrate 10 (e.g., a hanging sheet) into a reservoir 30 (e.g., an immersion tank). The immersion unit 35 may include a portion of a vertical conveyor 50 that is oriented at an angle to allow the substrate 10 to move downward into the reservoir 30 and then move upward out of the reservoir. The coating system 32 may include other components in addition to the reservoir 30, such as a sprayer or a dropper assembly, for applying the calcium adsorbent by a non-immersion method. In other embodiments, the immersion unit 35 may include additional components that are configured to individually lower a single substrate 10 into the reservoir 30. The substrate 10 that leaves the immersion unit is in the form of a coated substrate 52 (e.g., a lime-coated sheet) on which a calcium adsorbent coating is applied. The coated substrate 52 is then placed in a storage unit 54. The storage unit 54 may consist essentially of a conveyor 50 located in a shielded position between the immersion unit 35 and the collection unit 60. Alternatively, the storage unit 54 can be a building or one or more rooms in a building, where the coated substrate 52 can undergo carbonation, wherein ambient CO2 from the air reacts with the calcium adsorbent and water evaporates from the calcium adsorbent. After sufficient carbonation has occurred, the coated substrate 52 is moved to a collection unit 60 (e.g., a lime removal unit). There, the calcium carbonate adsorbent is removed from the substrate 10. The substrate 10 is released for reuse in the impregnation unit 35, and the calcium carbonate adsorbent (which may include CaCO3 and unreacted Ca(OH)2) moves along a horizontal conveyor 65, during which the partially carbonated calcium adsorbent can undergo further carbonation, so that at least a portion of the unreacted calcium hydroxide is carbonated. All or part of the calcium carbonate adsorbent can be removed for disposal, so that the carbon dioxide removed from the air is sequestered in the formed calcium carbonate. All or part of the calcium carbonate sorbent may also be conveyed to the calciner 70 where the carbon dioxide may be released to again form calcium oxide which may be removed in the solids separator 75 to provide the calcium oxide to the lime slaker 80 to form a calcium hydroxide slurry for input into the reservoir 30 for use as a calcium sorbent.

[0074] Figure 3 A fully implementable system and method for carbon dioxide capture is shown, but it should be understood that only some of the components and steps shown may be implemented to achieve various embodiments of the present disclosure. Figure 3 The technical personnel using the present disclosure can immediately recognize various combinations of the components and steps shown in the figure to obtain different embodiments. For example, in one or more embodiments, Figure 3 The methods and systems shown in can be implemented under one or more of the following conditions.

[0075] The calciner 70 and solid separator 75 may not be present in the system. Instead, the calcium oxide may be directly input into the lime slaker 80. In such an embodiment, the lime removed from the substrate in the collection unit 60 may be exported for sequestration and / or transported to a third party for re-calcination and carbon capture. Likewise, the lime slaker 80 may not be present and the calcium hydroxide may be directly obtained for input into the reservoir 30.

[0076] The reservoir 30 may be replaced by any other component suitable for applying the calcium adsorbent to the substrate 10 .

[0077] • The "sheet" may be replaced by any other suitable substrate material otherwise described herein.

[0078] The lime coated flakes 52 can be circulated through a vertical conveyor for carbonation without any intermediate treatment in a collection unit 60.

[0079] The CaCO3 and Ca(OH)2 removed from the collection unit 60 can be directly sent for re-calcination without additional carbonation.

[0080] The process can be substantially continuous in that the application of the calcium sorbent, the carbonation of the coated substrates, and the removal of the carbonated sorbent in the collection unit 60 can be performed uninterrupted except for necessary maintenance or planned shutdowns. For example, the system can be large enough that a single substrate can be cycled from exiting the coating system 32 to reentering the coating system only for a length of time sufficient for the desired level of carbonation to occur. This can be on the order of hours to days. In this way, the system can operate continuously.

[0081] The vertical conveyor may include a docking station at some point between the coating system 32 and the collection unit 60. In this manner, coated substrates 52 may be unloaded at the docking station for carbonation to occur while other substrates are being processed through the system. The docking station may be intermittently emptied completely or partially of coated substrates that have undergone carbonation and refilled with newly coated substrates.

[0082] • The process can be operated in batch mode, where substrates are coated in batches, stored in batches for carbonation, and then processed in batches for lime removal.

[0083] The process can be operated through multiple coating and carbonation steps without removing the coating from the substrate. For example, a substrate can be coated with a relatively thin layer of calcium adsorbent material, treated to allow carbonation to occur, coated again to add an additional relatively thin layer of calcium adsorbent material on the carbonated layer, and so on, until a relatively thick coating of multiple individual carbonated layers is present on the substrate. The coated substrate can then be de-coated.

[0084] Further exemplary embodiments are Figure 4 and Figure 5 Reference Figure 4 , Figure 3 The core system shown can remain essentially the same, but the vertical transport system can be replaced with a stationary sheet. In such an embodiment, the calcium sorbent can be applied through a pipe and drip irrigation system so that the substrate remains stationary while the calcium sorbent moves through the system first in the form of calcium hydroxide and second in the form of carbonated lime. Figure 4 , the calcium sorbent may be pumped or otherwise delivered from the reservoir 30 via one or more lines 100 to one or more drip tubes 110 including one or more perforations 115 for dripping new calcium sorbent onto the substrate 200. After the calcium sorbent undergoes carbonation, the carbonated lime may be removed from the substrate 200 (e.g., by a vibration system 155 integrated with the suspension unit 150) such that the carbonated lime falls onto a horizontal conveyor 165. The conveyor may be configured to deliver the carbonated lime to a calciner 70 with carbon capture, which may be connected to a solids separator 75 and a lime slaker 80 to deliver the calcium sorbent to the reservoir 30, similar to Figure 3 CO2 and material flows are not shown in Figure 4 , but it should be understood that such material flow can be Figure 3 The relevant descriptions are basically the same.

[0085] Can be improved Figure 3 The embodiments of the present invention provide further exemplary embodiments for implementing the systems and methods described herein. Figure 5 As shown, the Figure 4 The invention also provides an embodiment of the present invention, which is a drip irrigation system of the present invention, but utilizes a gravity-based collection system 190 instead of a horizontal conveyor. After the carbonated sorbent is removed from the substrate 200, it falls onto the inclined surface of the gravity-based collection system 190, so that the solid product is collected at a high enough density to allow easy transport back to the calciner 70.

[0086] The present system and method can achieve net carbon removal from the atmosphere because the net CO2 captured from the air by the calcium sorbent is greater than any CO2 emissions in the process. The net carbon flow in an exemplary embodiment of the present disclosure is shown in the table below for a system with a 90% carbon capture calciner and an 85% calcium sorbent carbonation rate.

[0087]

[0088] Experimental data indicate that >70% carbonation can be achieved using 0.3 kg of calcium sorbent per square meter of exposed area in approximately 3 days. This rate and conversion rate allows for approximately 100,000 metric tons (MT) of net direct air capture using less than 25 acres of land. This land use intensity is far less than that required to capture billions of tons of CO2 from air, does not impact other land uses, and does not deplete suitable areas near limestone and CO2 storage.

[0089] Many modifications and other embodiments of the present invention will occur to those skilled in the art having the benefit of the teachings presented in the foregoing description and the associated drawings. Therefore, it should be understood that the present invention is not limited to the specific embodiments disclosed, and modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are used herein, they are used in a general and descriptive sense only and not for the purpose of limitation.

[0090] As used herein, the words "approximately" and "substantially" are understood to mean that values ​​listed as "approximately" a value or "substantially" a value may vary by an industry-recognized level of tolerance from the specified value. When industry-recognized tolerances are not available, it is understood that such terms may mean that acceptable values ​​may vary by ±3%, ±2%, or ±1% from the specifically listed value. Likewise, in some embodiments, the listed values ​​may be exact, if desired, and variations above or below the listed values ​​may be expressly excluded.

Claims

1. A method for direct air capture of carbon dioxide, the method comprising: applying a calcium sorbent material on a flexible substrate to define a layer of the calcium sorbent material on a surface of the substrate, the layer of calcium sorbent material defining a substantially continuous coating along the surface of the substrate, the substantially continuous coating having an average thickness of 0.01 mm to 5 mm and a density of 0.1 kg / m2 to 5 kg / m2; contacting the substrate having a substantially continuous coating of calcium sorbent material with air containing carbon dioxide for a sufficient period of time to react the calcium sorbent with the carbon dioxide, thereby capturing at least a portion of the carbon dioxide from the air and converting at least a portion of the calcium sorbent to a carbonated form; removing at least a portion of the carbonated form of the calcium sorbent from the substrate by subjecting the substrate to a force effective to one or both of bend and flex the substrate such that the substantially continuous coating of the calcium sorbent material breaks and releases from the substrate; and Processing the calcium sorbent in a carbonated form allows the captured carbon dioxide from the air to be ready for storage or other uses.

2. The method of claim 1, wherein the substrate is configured as a substantially flat sheet.

3. The method of claim 1, wherein the substantially continuous coating of calcium adsorbent material is configured to exhibit a carbonation rate such that at least 25% by weight of the calcium adsorbent material is carbonated in 96 hours or less.

4. The method of claim 1, wherein the substantially continuous coating of calcium adsorbent material is configured to exhibit a carbonation rate such that at least 50% by weight of the calcium adsorbent material is carbonated within a period of 1 day to 14 days.

5. The method of claim 1 , wherein contacting the substrate having the substantially continuous coating of calcium adsorbent material with air containing carbon dioxide comprises suspending the substrate having the substantially continuous coating of calcium adsorbent material in a position where the substantially continuous coating of calcium adsorbent material contacts the air.

6. The method of claim 1, wherein treating the carbonated form of the calcium sorbent comprises granulating the carbonated form of the calcium sorbent to seal the carbonated form of the calcium sorbent.

7. The method of claim 1, wherein treating the carbonated form of the calcium sorbent comprises further contacting the carbonated form of the calcium sorbent with ambient air for a time sufficient to increase the carbonation percentage.

8. The method of claim 1, wherein treating the carbonated form of the calcium adsorbent comprises: calcining the carbonated form of the calcium sorbent to release carbon dioxide therefrom and form calcium oxide; and The carbon dioxide released from the calcium sorbent is captured.

9. The method of claim 8, further comprising slaking the calcium oxide to form a calcium sorbent material for preparing a substantially continuous coating.

10. The method of claim 8, further comprising removing a portion of the carbonated form of the calcium sorbent prior to calcining and adding supplemental limestone during calcining.

11. The method of claim 1 , wherein preparing the substantially continuous coating of calcium adsorbent material comprises immersing the substrate in a reservoir of calcium adsorbent material.

12. The method of claim 1, wherein preparing the substantially continuous coating of calcium adsorbent material comprises dripping, pouring, or spraying calcium adsorbent material onto the substrate.

13. A system for direct air capture of carbon dioxide, the system comprising: A flexible substrate substantially configured as a sheet having a surface, a coating system configured to apply a liquid calcium adsorbent material to the substrate to form a substantially continuous coating of the calcium adsorbent material on the surface of the substrate, such that the substantially continuous coating of the calcium adsorbent material has an average thickness of 0.01 mm to 5 mm and a density of 0.1 kg / m2 to 5 kg / m2; a storage unit configured to position the substrate for a period of time wherein the substrate is in contact with air such that carbon dioxide in the air reacts with the calcium adsorbent material to form carbonated calcium adsorbent material; as well as a collection unit configured to remove and collect carbonated calcium adsorbent material from the substrate, the collection unit being configured to subject the substrate to a force effective to one or both of bend and flex the substrate such that the substantially continuous coating of calcium adsorbent material is broken and released from the substrate.

14. The system of claim 13, wherein the coating system comprises one or more reservoirs of liquid calcium sorbent material.

15. The system of claim 13, wherein the coating system further comprises a dipping unit configured to dip the substrate into one or more reservoirs of liquid calcium sorbent material.

16. The system of claim 13, wherein the coating system comprises a suspension unit configured to maintain one or more substrates in a substantially vertical position.

17. The system of claim 16, wherein the coating system further comprises one or more components configured to drip or pour a calcium sorbent material onto the substrate.

18. The system of claim 16, further comprising a calciner configured to receive the carbonated calcium sorbent material and convert the carbonated calcium sorbent material into calcium oxide and carbon dioxide.

19. The system of claim 18, further comprising a solid separator configured to separate the calcium oxide from the carbon dioxide.

20. The system of claim 19, further comprising a unit configured to receive calcium oxide and form calcium hydroxide for use as a calcium adsorbent material.