Coated abrasive article and method of making a coated abrasive article
By using patterned base rubber and re-rubber coatings in coated abrasive products, combined with grinding aids, the problems of sand loss and filling are solved, grinding efficiency and surface quality are improved, and the preparation process is simplified.
Patent Information
- Application Number
- CN202080085085.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-09
- Filing Date
- 2020-12-07
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-12-07
AI Technical Summary
Existing coated abrasive products have problems with sand loss and filling during the grinding process, which affects efficiency and surface quality. Moreover, the preparation of patterned coatings is complicated and increases costs.
Using patterned primer and resize coatings to deposit abrasive particles uniformly or patternedly on the backing by spraying or other methods, combined with grinding aids to improve grinding efficiency and anti-packing properties, and optimized through specific pattern designs Abrasive properties.
It effectively reduces sand loss and filling phenomena, improves grinding efficiency and surface quality, reduces preparation complexity and cost, and optimizes abrasive performance through patterned design.
Smart Images

Figure CN114901430B_ABST
Abstract
Description
Background Art
[0001] Coated abrasive articles can be widely used in the manufacturing process of articles for grinding, dressing or grinding various materials and surfaces. Generally speaking, coated abrasive articles include a backing, a first cured resin adhesive layer (bottom layer) applied to one major surface of the backing, abrasive particles, a second cured resin adhesive layer (size layer) and an optional third cured resin adhesive layer (top layer). In some cases, a grinding aid is used to improve grinding performance and is generally used as an additive to form at least one of the aforementioned resin adhesive layers. BRIEF DESCRIPTION OF THE DRAWINGS
[0002] Figure 1A is a schematic diagram of an exemplary coated abrasive article according to the present disclosure.
[0003] Figure 1B is a top view of an exemplary coated abrasive article.
[0004] Figure 2A and Figure 2B Methods and results of pattern coating an abrasive article according to embodiments described herein are shown.
[0005] Figure 3 is a diagrammatic view of a method of making a patterned coated abrasive article according to embodiments described herein.
[0006] FIG. 4A to FIG. 4D A patterned coated abrasive article according to embodiments described herein is shown.
[0007] Figure 5 Methods of using patterned coated abrasive articles according to embodiments described herein are shown.
[0008] Figure 6 Coated abrasive articles according to embodiments described herein are shown.
[0009] 7A to 7I Coated abrasive articles prepared according to the Examples are shown.
[0010] Reference symbols used repeatedly in the specification and drawings are intended to represent the same or similar features or elements of the present disclosure. It should be understood that those skilled in the art can design many other modifications and embodiments that fall within the scope and essence of the principles of the present disclosure. The drawings may not be drawn to scale. DETAILED DESCRIPTION
[0011] Coated abrasive articles are known in the art and generally include abrasive grains embedded in a make coat on a backing and coated with a size coat that reduces shelling of the abrasive grains from the backing. A top coat or other functional layers (including functional layers and primer or laminating layers) may also be added to add functionality and / or alter parameters of the coated abrasive article.
[0012] Typically, patterned coated abrasive articles exhibit better grinding efficiency than non-patterned coated abrasive articles. This may be due to more efficient removal of chips from the workpiece, judicious engineering of the grinding zone, or enhanced effects of lubricants and / or grinding aids on the working surface.
[0013] As used herein, "pattern" on a coated abrasive article refers to the intentional placement of material on a backing so that a portion of the backing or a portion of a previous layer remains uncoated. Therefore, a patterned primer coat covers some but not all of the backing so that a portion of the backing remains uncoated. Similarly, a patterned layer of abrasive particles may result in some but not all of the primer coat being coated by abrasive particles. Patterns include intentional designs with or without repeating units. The pattern may extend from the center of the abrasive disc or the central axis of the abrasive belt to the edge of the abrasive disc or the abrasive belt. The patterned coating is intended to include any suitable method for forming a well-defined area of a given material coating and an open area without a given material coating. Therefore, a patterned abrasive area may be designed independently of any pattern present on a fabric substrate to optimize both abrasive performance, dust removal, and anti-stuffing properties. The pattern may include lines, swirls, polygons, letters, or numbers. In addition, other text or product information may also be provided on the coated abrasive article. The pattern may also include a color so that a portion of the final coated abrasive article has a first color, and a portion of the final coated abrasive article has a second color.
[0014] It is also known in the art that abrasive particles can be pattern coated and / or aligned on the backing surface. In some embodiments, patterned drop coating can be achieved using alignment tools by methods similar to those described in PCT patent application publications 2016 / 205133 (Wilson et al.), 2016 / 205267 (Wilson et al.), 2017 / 007703 (Wilson et al.), 2017 / 007714 (Liu et al.). Transfer coating using tools with patterned cavities can be similar to transfer coating described in U.S. Patent Application Publication 2016 / 0311081A1 (Culler et al.). In some embodiments, abrasive particles can be applied to the primer layer by patterned mesh or screen.
[0015] Alignment of the abrasive particles can be accomplished using electrostatic or magnetic coatings as described in PCT Patent Application Publications WO2018 / 080703 (Nelson et al.), WO2018 / 080756 (Eckel et al.), WO2018 / 080704 (Eckel et al.), WO2018 / 080705 (Adefris et al.), WO2018 / 080765 (Nelson et al.), WO2018 / 080784 (Eckel et al.), WO2018 / 136271 (Eckel et al.), WO2018 / 134732 (Nienaber et al.), WO2018 / 080755 (Martris et al.), and WO2018 / 080766 (Nelson et al.). inez et al.), WO2018 / 080799 (Nienaber et al.), WO2018 / 136269 (Nienaber et al.), WO2018 / 136268 (Jesme et al.), WO2019 / 207415 (Nienaber et al.), WO2019 / 207417 (Eckel et al.), WO2019 / 207416 (Nienaber et al.), and U.S. Provisional Application No. 62 / 914,778 filed on October 14, 2019, U.S. Provisional Application No. 62 / 875,700 filed on July 18, 2019, and U.S. Provisional Application No. 62 / 924,956 filed on October 23, 2019.
[0016] The terms "cured", "curing" and "curable" refer to linking polymer chains together by covalent chemical bonds (usually by cross-linking molecules or groups) to form a network. Therefore, in this disclosure, the terms "cured" and "cross-linked" can be used interchangeably.
[0017] Figure 1A and Figure 1B Shown are views of coated abrasive articles according to embodiments described herein.
[0018] Reference now Figure 1A , the coated abrasive article 100 includes a backing 110 having a first major surface 112 and a second major surface 114 opposite the first major surface 112. A make layer 120 is disposed on and bonded to the first major surface 112. Abrasive particles 130 and abrasive particles 130 are bonded to the make layer 120. A size layer 140 is disposed above and bonded to the make layer 120 and abrasive particles 130. An optional top layer or other functional layer is disposed above and bonded to the size layer 140.
[0019] Reference now Figure 1BOne exemplary form of a coated abrasive article is a coated grinding disc 150. However, other coated abrasive articles, such as abrasive belts, are also contemplated.
[0020] Exemplary suitable materials for backing include polymer films, metal foils, woven fabrics, knitted fabrics, paper, vulcanized fibers, nonwoven fabrics, foams, silk screens, nets, laminates, combinations thereof, and processed forms thereof. Coated abrasive articles may be in the form of sheets, discs, belts, pads, or rolls. Backing may be rigid, semi-rigid, or flexible. In some embodiments, backing should be sufficiently flexible to allow coated abrasive articles to be formed into rings to prepare the abrasive belts that can be run on suitable grinding equipment. For applications requiring the hardness of backing, flexible backing may also be used by fixing the flexible backing to the rigid support pads installed on the grinding tool. For the application of hand-off grinding considering hardness and cost, vulcanized fiber backing is usually preferred. In some embodiments, backing may be circular and may include continuous, uninterrupted discs, and in other embodiments, it may have a central mandrel hole for installation. Equally, the circular backing may be flat, or it may have a depressed central hub, such as a depressed central disc of type 27. In some embodiments, the backing has mechanical or adhesive fasteners securely attached to a major surface opposite the abrasive layer.
[0021] The base coat, the size coat, and the optional super coat comprise resin binders that may be the same or different. Exemplary suitable binders may be prepared from corresponding binder precursors such as thermally curable resins, radiation curable resins, and combinations thereof.
[0022] The binder precursor (e.g., primer layer precursor and / or size layer precursor) may include, for example, glue, phenolic resin, aminoplast resin, urea-formaldehyde resin, melamine-formaldehyde resin, urethane resin, multifunctional (meth)acrylate polymerizable in a free radical manner (e.g., aminoplast resin having side chain α,β-unsaturated groups, acrylated urethane, acrylated epoxy resin, acrylated isocyanurate), epoxy resin (including bis-maleimide and fluorene-modified epoxy resin), isocyanurate resin, and mixtures thereof. Among these materials, phenolic resin is preferred, especially when used in combination with a vulcanized fiber backing.
[0023] Generally speaking, phenolic resins are formed by the condensation of phenol and formaldehyde, and are generally classified as resol or novolac phenolic resins. Novolac phenolic resins are acid catalyzed and have a molar ratio of formaldehyde to phenol of less than 1:1. Resole / resol phenolic resins may be catalyzed with an alkaline catalyst and have a molar ratio of formaldehyde to phenol of greater than or equal to one, typically between 1.0 and 3.0, so that hydroxymethyl side groups are present. Alkaline catalysts suitable for catalyzing the reaction between the aldehyde and phenol components of resol phenolic resins include sodium hydroxide, barium hydroxide, potassium hydroxide, calcium hydroxide, organic amines, and sodium carbonate, all as catalyst solutions dissolved in water.
[0024] Resols are typically applied as solutions with water and / or organic solvents (e.g., alcohols). Typically, the solution contains about 70% to about 85% solids by weight, but other concentrations may be used. If the solids content is very low, more energy is required to remove the water and / or solvent. If the solids content is very high, the viscosity of the resulting phenolic resin is too high, which typically results in processing problems.
[0025] Phenolic resins are well known and readily available from commercial sources. Examples of commercially available resol phenolic resins that can be used to practice the present disclosure include those sold by Durez Corporation under the trade name VARCUM (e.g., 29217, 29306, 29318, 29338, 29353); those sold by Ashland Chemical Co., Bartow, Florida, under the trade name AEROFENE (e.g., AEROFENE 295); and those sold by Kangnam Chemical Company Ltd. of Seoul, South Korea under the trade name PHENOLITE (e.g., PHENOLITE TD-2207).
[0026] The binder precursor may also contain optional additives such as, for example, fillers (including grinding aids), fibers, lubricants, wetting agents, surfactants, pigments, dyes, coupling agents, resin curing agents, plasticizers, antistatic agents, and suspending agents. Examples of fillers suitable for use in the present invention include: wood pulp, vermiculite, and combinations thereof; metal carbonates such as calcium carbonate (e.g., chalk, calcite, marl, travertine, marble, and limestone), calcium magnesium carbonate, sodium carbonate, and magnesium carbonate; silicates such as amorphous silica, quartz, glass beads, glass bubbles, and glass fibers; silicates such as talc, clay (montmorillonite), feldspar, mica, calcium silicate, calcium metasilicate, sodium aluminosilicate, sodium silicate; metal sulfates such as calcium sulfate, barium sulfate, sodium sulfate, sodium aluminum sulfate, aluminum sulfate; gypsum; vermiculite; wood flour; aluminum trihydrate; metal oxides such as calcium oxide (lime), aluminum oxide, titanium dioxide, and metal sulfites such as calcium sulfite.
[0027] The binder precursor may be applied by any known coating method including, for example, roll coating, extrusion die coating, curtain coating, knife coating, gravure coating, and spray coating.
[0028] The basis weight of the make coat used may depend, for example, on the intended use, the type and grade of abrasive grains, and the nature of the coated abrasive disc being prepared, but will typically range from 1 gram per square meter (gsm), 2 gsm, 5 gsm, 10 gsm, or 15 gsm to 20 gsm, 25 gsm, 100 gsm, 200 gsm, 300 gsm, 400 gsm, or even 600 gsm.
[0029] Figure 2A is a method of making a patterned coated abrasive article according to embodiments described herein. Method 200 can be used to provide a patterned coated abrasive article.
[0030] Details regarding the general manufacture of coated abrasive articles can be found, for example, in U.S. Pat. Nos. 4,734,104 (Broberg), 4,737,163 (Larkey), 5,203,884 (Buchanan et al.), 5,152,917 (Pieper et al.), 5,378,251 (Culler et al.), 5,417,726 (Stout et al.), 5,436,063 (Follett et al.), 5,496,386 (Broberg et al.), and 5,514,677 (Follett et al.). ), 5,609,706 (Benedict et al.), 5,520,711 (Helmin), 5,954,844 (Law et al.), 5,961,674 (Gagliardi et al.), 4,751,138 (Bange et al.), 5,766,277 (DeVoe et al.), 6,077,601 (DeVoe et al.), 6,228,133 (Thurber et al.), and 5,975,988 (Christianson).
[0031] As described above, it may be helpful to have abrasive articles with abrasive particles applied in a pattern. It is contemplated that in some embodiments, it may be more effective to apply some layers uniformly in a coated abrasive article, and only a subset of these layers have the desired pattern. It may also be helpful to apply a pattern in all or nearly all layers. However, applying a pattern in a subset of layers may provide a functional difference in grinding efficiency, or this may be used to associate an abrasive article with a specific manufacturer or detect counterfeit products from different manufacturers. In addition, pattern coatings may require special tools. Therefore, reducing the number of coatings that require a pattern can reduce manufacturing costs. However, when only a subset of the coating is patterned, improvements in pattern coatings can still be seen. For example, a patterned primer coating with a full-coat helps resist sanding.
[0032] In frame 210, a backing is provided. Exemplary suitable materials for backing include polymer films, metal foils, woven fabrics, knitted fabrics, paper, vulcanized fibers, nonwoven fabrics, foams, screens, nets, laminates, combinations thereof, and processed forms thereof. Optionally, the coated abrasive article may also include, for example, a backing (i.e., a coating on the main surface of the backing opposite to the main surface with the abrasive coating), a pre-sizing layer or bonding layer (i.e., a coating between the abrasive coating and the main surface to which the abrasive coating is fixed) and / or an impregnant covering the two main surfaces of the backing. The backing may also have an applied laminate, such as described in, for example, co-owned pending U.S. provisional applications 62 / 945242 and 62 / 945244, both of which were filed on December 9, 2019.
[0033] In frame 220, primer coating is provided. Primer coating can be applied as a curable primer layer deposited on the main surface of the backing. Primer coating can be applied by any suitable method, and these methods include for example spraying, curtain coating, slot coating, roller coating and / or scraper coating. Coating weight will depend on application, and will be apparent to those skilled in the art. In one embodiment, primer coating precursor is applied on the backing with pattern, as indicated by frame 222. For example, primer coating precursor can be sprayed by mask so that primer coating precursor contacts and covers the backing substrate with required pattern. However, in other embodiments, primer coating precursor is applied as uniform coating, as indicated in frame 224, so that the whole backing substrate receives the substantially uniform coating of primer coating precursor. In some embodiments, other methods are also possible, including concave coating, flexographic printing, patterned roller coating, screen printing or stencil printing.
[0034] In block 230, abrasive particles are provided. As discussed herein, the abrasive particles may include crushed abrasive particles, plate-like abrasive particles, and / or shaped abrasive particles. In some embodiments, applying the abrasive particles may include providing abrasive particles of a first size and a second size. In some embodiments, providing the abrasive particles may also include providing multiple types of abrasive particles, such as shaped abrasive particles and crushed abrasive particles.
[0035] In some preferred embodiments, at least some of the abrasive particles may be deposited according to a predetermined pattern. Examples of patterns include rectangular grids, parallel strips, hexagonal grids, arrays of parallel wavy lines, checkerboards, spirals, and partially filled circles. Some example patterns are shown in U.S. Provisional Application 62 / 945242 filed on December 9, 2019.
[0036] In the embodiment of applying a patterned make coat precursor in block 220, it may not be necessary to deposit abrasive particles in a pattern, because particles landing on the backing area without make coat precursor will not adhere to the backing. Therefore, the abrasive can be applied uniformly on the make coat precursor, as indicated in block 234.
[0037] However, it is also clearly contemplated that, whether the make coat is applied uniformly or in a pattern, applying the abrasive particles in a pattern may be beneficial, as indicated by block 232. For example, the particles may be applied more densely in different areas of the abrasive article. In addition, particles of different sizes can be applied in different patterns. Furthermore, shaped abrasive particles can be applied to the same article in a different pattern than crushed abrasive particles. As used herein, the term "pattern" refers to the overall pattern formed by the abrasive particles, rather than the individual abrasive particles that make up the pattern.
[0038] After or during deposition of the abrasive grains, the curable make layer precursor is sufficiently cured (eg, using heat and / or electromagnetic radiation) such that the make layer and abrasive grains are secured to the backing.
[0039] In frame 240, a size coat is applied. In some embodiments, applying a size coat may include applying a size coat precursor, which is later cured to produce a size coat. The size coat may be applied on a completely or at least partially cured primer layer. Coating may be achieved by any suitable method, including, for example, spraying, curtain coating, slot coating, roller coating and / or blade coating. The coating weight will depend on the application, and will be apparent to those skilled in the art. The curable size coat precursor may be cured, for example, using heat and / or electromagnetic radiation. In one embodiment, the size coat is applied in a pattern, as indicated by frame 242. The size coat may be applied as a pattern, regardless of whether the primer coating or abrasive grains are pattern-coated. For example, the size coat can be applied in a pattern to indicate the manufacturer or grade of the abrasive article. In addition, as indicated by frame 244, the size coat may be applied as a uniform coating on a pattern-coated layer of abrasive grains and / or a pattern-coated primer coating. Due to the relative size of the abrasive grains compared to the abrasive article, a uniformly applied size coat can at least partially obscure the patterning of the abrasive grains, thereby producing an abrasive article that appears similar to a non-patterned coated abrasive article.
[0040] In frame 250, additional functional layers may be provided. Functional layers may be applied as a supplement to the top coat, or as a top coat. Functional layers may be deposited in patterns, as indicated by frame 252, which may be the same or different from any abrasive grain pattern layer. Additionally, in some embodiments, functional layers may be applied in uniform coatings, as indicated by frame 254. For example, it may be desirable, for example, to deposit a grinding aid uniformly on the article. Additionally, functional layers may also include a grinding aid and / or an anti-clogging material. For example, a top coat may be applied in patterns to indicate the manufacturer or grade of the abrasive article.
[0041] Grinding aids are defined as particulate materials that, when added to an abrasive article, have a significant effect on the chemical and physical processes of grinding. Specifically, it is believed that grinding aids can: (1) reduce friction between the abrasive particles and the workpiece being ground; (2) prevent abrasive particles from "blocking," i.e., preventing metal particles from being welded to the tops of the abrasive particles; (3) reduce the interface temperature between the abrasive particles and the workpiece; (4) reduce grinding forces; and / or (5) have a synergistic effect of the above mechanisms. In general, the addition of grinding aids can increase the useful life of coated abrasive articles. Grinding aids encompass a wide variety of different materials and can be inorganic or organic.
[0042] Exemplary grinding aids may include inorganic halide salts, halogenated compounds and polymers, and organic and inorganic sulfur-containing materials. Exemplary grinding aids may be organic or inorganic, including waxes, halogenated organic compounds, such as chlorinated waxes, such as tetrachloronaphthalene, pentachloronaphthalene, and polyvinyl chloride; halide salts, such as sodium chloride, potassium cryolite, sodium cryolite, ammonium cryolite, potassium tetrafluoroborate, sodium tetrafluoroborate, silicon fluoride, potassium chloride, magnesium chloride; and metals and their alloys, such as tin, lead, bismuth, cobalt, antimony, cadmium, iron and titanium. Examples of other grinding aids include sulfur, organic sulfur compounds, graphite and metal sulfides, materials containing organic and inorganic phosphates. Combinations of different grinding aids may be used.
[0043] Preferred grinding aids include halide salts, especially potassium tetrafluoroborate (KBF4), cryolite (Na3AlF6) and ammonium cryolite [(NH4)3AlF6]. Other halide salts that can be used as grinding aids include sodium chloride, potassium cryolite, sodium tetrafluoroborate, silicon fluoride, potassium chloride and magnesium chloride. Other preferred grinding aids are those in U.S. Pat. No. 5,269,821 (Helmin et al.), which describes grinding aid agglomerates composed of water-soluble and water-insoluble grinding aid particles. Other useful grinding aid agglomerates are those in which a plurality of grinding aid particles are bound together with a binder to form an agglomerate. Agglomerates of this type are described in U.S. Pat. No. 5,498,268 (Gagliardi et al.).
[0044] Examples of halogenated polymers that can be used as grinding aids include: polyvinyl halides (e.g., polyvinyl chloride) and polyvinyl diene halides, such as those disclosed in U.S. Pat. No. 3,616,580 (Dewell et al.); highly chlorinated paraffins, such as those disclosed in U.S. Pat. No. 3,676,092 (Buell); fully chlorinated hydrocarbon resins, such as those disclosed in U.S. Pat. No. 3,784,365 (Caserta et al.); and fluorocarbons, such as polytetrafluoroethylene and polychlorotrifluoroethylene as disclosed in U.S. Pat. No. 3,869,834 (Mullin et al.).
[0045] Inorganic sulfur-containing materials that can be used as grinding aids include elemental sulfur, ferrous sulfide, copper sulfide, molybdenum sulfide, potassium sulfate, etc., as variously disclosed in U.S. Pat. Nos. 3,833,346 (Wirth), 3,868,232 (Sioui et al.), and 4,475,926 (Hickory). Organic sulfur-containing materials (e.g., thiourea) used in the present invention include those mentioned in U.S. Pat. No. 3,058,819 (Paulson).
[0046] The present disclosure also encompasses the use of combinations of different grinding aids, and in some cases this may produce a synergistic effect.The examples of grinding aids mentioned above are intended as representative descriptions of grinding aids, and they are not intended to be inclusive of all grinding aids.
[0047] The coated abrasive article may also include grinding aid particles arranged randomly, in a single predetermined pattern or in a plurality of different patterns. At least a portion of the grinding aid particles may be positioned so that the pattern formed by these grinding aid particles includes a plurality of parallel lines and / or a grid pattern. For example, at least a portion of the grinding aid particles may be positioned so that the pattern formed by these grinding aid particles includes a plurality of circles (hollow or filled). Similarly, at least a portion of the grinding aid particles may be arranged in a spiral, a chessboard or a strip (in any orientation). The pattern of the grinding aid particles may be the same or different from the pattern of the abrasive particles. The grinding aid particles (whether patterned or not) may be deposited as a part of the abrasive particle deposition discussed above with respect to step 230, or may be deposited as a part of the top coat, and may be applied as a part of the functional coating described in frame 250.
[0048] Figure 2B 260, showing the results of including patterns in different applied layers on a backing. Flowchart 260 assumes that a single pattern is applied at any of the layers, and that the same pattern is applied for multiple layers. However, it is expressly contemplated that the pattern of abrasive particles may differ, for example, from a patterned size coat. Additionally, Figure 2B Only the abrasive article 270 resulting from the application of a patterned or uniformly coated make layer 262, abrasive grain layer 264, or size layer 266 is shown. However, it is expressly contemplated that a supersize layer or additional functional layer is also contemplated and can be treated similarly to the size layer 266.
[0049] Figure 3 is a diagrammatic view of a method of making a patterned coated abrasive article according to embodiments described herein. Figure 3 A diagram 300 is shown illustrating the deposition of different layers on a backing 320. Each layer is deposited by one of several dispensers 310. However, while several dispensers 310 are discussed, it is contemplated that in some embodiments, one dispenser 310 may dispense multiple layers of material.
[0050] The abrasive article has a backing 320 that may have undergone one or more pretreatments or received one or more primer layers. Primer layers and pretreatments may change the properties of the backing 320, for example, changing the hardness of the backing 320 to make it harder or less hard than it would be without the pretreatment or primer layer.
[0051] The first dispenser 310 dispenses a primer coating 330 or a primer coating precursor that can be cured into the primer coating 330 onto the backing 320. The primer coating 330 can be deposited directly onto the backing 320, or can be deposited onto a laminate that is deposited directly onto the backing 320, as described in, for example, U.S. Provisional Applications 62 / 945242 and 62 / 945244, both filed on December 9, 2019. In one embodiment, the primer coating 330 or the primer coating precursor can be deposited on the backing 320 as a uniform coating or as a uniform layer on the surface of the backing 320. In another embodiment, the primer coating 330 or the primer coating precursor can be deposited in a pattern so that some portions of the backing 320 do not receive the primer coating 330 or the primer coating precursor.
[0052] The second dispenser 310 dispenses abrasive particles 340. The abrasive particles 340 may be shaped abrasive particles, formed abrasive particles, crushed abrasive particles, and / or plate-shaped abrasive particles. Dispensing abrasive particles 340 from the second dispenser 310 may include dispensing a first group of abrasive particles 340 and a second group of abrasive particles 340.
[0053] Abrasive particles 340 may be dispensed by dispenser 310 in a pattern such that some areas of the applied make coat 330 or some areas of the applied backing 320 remain uncovered. Figure 2B As shown, abrasive particles 340 can be deposited in a pattern regardless of whether make coat 330 is deposited in a pattern. However, if make coat 330 is applied in a pattern and abrasive particles 340 are applied uniformly, only abrasive particles 340 embedded within the pattern of make coat 330 will adhere to and become incorporated into the final abrasive article.
[0054] It is also envisioned that, although Figure 3 Only one type and size of abrasive particles 340 are shown, but in some embodiments, a first group of abrasive particles and a second group of abrasive particles are deposited. For example, the first group of abrasive particles and the second group of abrasive particles can be different in type, selected from shaped abrasive particles, formed abrasive particles, crushed abrasive particles, plate-like abrasive particles, or agglomerated abrasive particles. Additionally or alternatively, the first group of abrasive particles and the second group of abrasive particles can be different in size, composition, or deposition pattern.
[0055] Size coat 350 or size coat precursor is deposited on top of abrasive grains 340. Many size coats impart color to abrasive grains, either naturally or by including pigments. Thus, pattern-coating size coat 350 can produce a visual pattern that is clearly visible to a user of the abrasive article. Although the pattern of abrasive grains 340 can be detected, in some embodiments, abrasive grains 340 are small enough that the pattern is not easily visible. Because the pattern of abrasive grains 340 can change the quality or behavior of an abrasive article, a patterned size coat can help indicate one or more attributes on an abrasive article to a user, such as the grade or size of the abrasive grains.
[0056] One or more supersize coatings 360 may be applied over the size coat 350. The supersize coating may impart additional functionality to the abrasive article, such as grinding aids, lubricants, or other particles. The supersize coating 360 may also impart color or visual indications to the final abrasive article.
[0057] FIG. 4A to FIG. 4D Patterned coated abrasive articles according to embodiments described herein are shown. 4A and 4B show patterned coated abrasive discs coated with a supersize layer. Figure 4C A web abrasive with a uniformly applied size coat is shown. Figure 4D A web abrasive having a size coat with a patterned coating is shown.
[0058] Whether crushed or shaped, the abrasive particles used in the embodiments herein should have sufficient hardness and surface roughness to be used as abrasive particles in the grinding process. Preferably, the abrasive particles have a Mohs hardness of at least 4, at least 5, at least 6, at least 7 or even at least 8.
[0059] Useful abrasive materials include, for example, fused alumina, heat treated alumina, white fused alumina, ceramic alumina materials (such as those commercially available as 3M CERAMIC ABRASIVE GRAIN from 3M Company, St. Paul, Minnesota), black silicon carbide, green silicon carbide, titanium diboride, boron carbide, tungsten carbide, titanium carbide, cubic boron nitride, garnet, fused alumina zirconia, sol-gel derived ceramics (e.g., alumina ceramics doped with chromium oxide, ceria, zirconium oxide, titanium dioxide, silicon dioxide and / or tin oxide), silica (e.g., quartz, glass beads, glass bubbles and glass fibers), feldspar or flint. Examples of sol-gel derived comminuted ceramic particles can be found in US Pat. Nos. 4,314,827 (Leitheiser et al.), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), 4,770,671 (Monroe et al.), and 4,881,951 (Monroe et al.).
[0060] As previously described, the abrasive particles can be shaped (e.g., precisely shaped) or random (e.g., crushed). Shaped abrasive particles and precisely shaped abrasive particles can be prepared, for example, by a molding process using the sol-gel technology described in the following patents: U.S. Patents 5,201,916 (Berg), 5,366,523 (Rowenhorst (Re 35,570)) and 5,984,988 (Berg). U.S. Patent 8,034,137 (Erickson et al.) describes aluminum oxide particles that have been formed into a specific shape and then crushed to form fragments that retain a portion of their original shape features. Exemplary shapes of abrasive particles include crushed, pyramids (e.g., 3-, 4-, 5-, or 6-sided pyramids), truncated pyramids (e.g., 3-, 4-, 5-, or 6-sided truncated pyramids), cones, truncated cones, rods (e.g., cylindrical, worm-like), and prisms (e.g., 3-, 4-, 5-, or 6-sided prisms).
[0061] Abrasive particles can be independently sized according to a specified nominal grade recognized by the abrasive industry. Illustrative abrasive industry recognized classification standards include those issued by ANSI (American National Standards Institute), FEPA (European Abrasive Manufacturers Federation) and JIS (Japanese Industrial Standards). ANSI grade designations (i.e., specified nominal grades) include, for example: ANSI 4, ANSI 6, ANSI 8, ANSI 16, ANSI 24, ANSI 36, ANSI 46, ANSI 54, ANSI 60, ANSI 70, ANSI 80, ANSI 90, ANSI 100, ANSI 120, ANSI 150, ANSI 180, ANSI 220, ANSI 240, ANSI 280, ANSI 320, ANSI 360, ANSI 400 and ANSI 600. FEPA grade numbers include F4, F5, F6, F7, F8, F10, F12, F14, F16, F20, F22, F24, F30, F36, F40, F46, F54, F60, F70, F80, F90, F100, F120, F150, F180, F220, F230, F240, F280, F320, F360, F400, F500, F600, F800, F1000, F1200, F1500, F2000, P12, P16, P20, P24, P30, P36, P40, P50, P60, P80, P100, P120, P150, P180, P220, P240, P280, P320, P360, P400, P500, P600, P800, P1000, P1200, P1500, P2000, and P2500. JIS grade numbers include: JIS8, JIS12, JIS16, JIS24, JIS36, JIS46, JIS54, JIS60, JIS80, JIS100, JIS150, JIS180, JIS220, JIS240, JIS280, JIS320, JIS360, JIS400, JIS600, JIS800, JIS1000, JIS1500, JIS2500, JIS4000, JIS6000, JIS8000 and JIS10,000.
[0062] Examples of shaped abrasive particles can be found in U.S. Pat. Nos. 5,201,916 (Berg), 5,366,523 (Rowenhorst (Re 35,570)), and 5,984,988 (Berg). U.S. Pat. No. 8,034,137 (Erickson et al.) describes aluminum oxide crushed abrasive particles that have been formed into a specific shape and then crushed to form fragments that retain a portion of their original shape characteristics. In some embodiments, the shaped alpha alumina particles are precisely shaped particles (i.e., the particles have a shape that is at least partially determined by the shape of the cavity in the production tool used to make them). Details regarding such precisely shaped abrasive particles and methods for making them can be found, for example, in U.S. Pat. Nos. 8,142,531 (Adefris et al.), 8,142,891 (Culler et al.), and 8,142,532 (Erickson et al.); and U.S. Patent Application Publications 2012 / 0227333 (Adefris et al.), 2013 / 0040537 (Schwabel et al.), and 2013 / 0125477 (Adefris).
[0063] In those embodiments where the abrasive particles are shaped as triangular plates (or triangular truncated pyramids), they may have a major surface with a vertex of 90 degrees (corresponding to a right triangle), or they may have a major surface with a vertex greater than 90 degrees (corresponding to an obtuse triangle), but this is not required. Examples include at least 91 degrees, at least 95 degrees, at least 100 degrees, at least 110 degrees, at least 120 degrees, or even at least 130 degrees.
[0064] In some preferred embodiments, the abrasive particles include plate-shaped crushed abrasive particles. Such abrasive particles can be obtained from commercial suppliers by known methods, and / or by sorting such crushed abrasive particles by shape; for example, using a shape sorting table known in the art.
[0065] Examples of suitable abrasive particles include crushed abrasive particles comprising: fused alumina, heat treated alumina, white fused alumina, ceramic alumina materials (such as those commercially available from 3M Company of St. Paul, Minnesota as 3MCERAMIC ABRASIVE GRAIN), brown alumina, blue alumina, silicon carbide (including green silicon carbide), titanium diboride, boron carbide, tungsten carbide, garnet, titanium carbide, diamond, cubic boron nitride, fused zirconium corundum, iron oxide, chromium oxide, zirconium oxide, titanium dioxide, quartz, feldspar, flint, corundum, sol-gel ceramics (e.g., alpha alumina), and combinations thereof. Additional examples include crushed abrasive composites of abrasive particles (these abrasive particles may be plate-like or not) in a binder matrix, such as those described in U.S. Pat. No. 5,152,917 (Pieper et al.). Many such abrasive particles, agglomerates, and composites are known in the art.
[0066] Preferably, the crushed abrasive particles include ceramic crushed abrasive particles, such as, for example, sol-gel derived polycrystalline alpha alumina particles. Ceramic crushed abrasive particles composed of crystallites of alpha alumina, magnesium aluminum spinel, and rare earth hexagonal aluminate can be prepared using sol-gel alpha alumina particle precursors according to the methods described in, for example, U.S. Pat. No. 5,213,591 (Celikkaya et al.) and U.S. Published Patent Applications 2009 / 0165394 A1 (Culler et al.) and 2009 / 0169816 A1 (Erickson et al.).
[0067] Examples of sol-gel prepared abrasive particles from which crushed abrasive particles can be separated and methods for preparing the same can be found in U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), 4,770,671 (Monroe et al.), and 4,881,951 (Monroe et al.). It is also contemplated that crushed abrasive particles may include abrasive agglomerates such as those described in, for example, U.S. Pat. Nos. 4,652,275 (Bloecher et al.) or 4,799,939 (Bloecher et al.). In some embodiments, crushed abrasive particles may be surface treated with a coupling agent (e.g., an organosilane coupling agent) or other physical treatment (e.g., iron oxide or titanium oxide) to enhance adhesion of crushed abrasive particles to a binder. Crushed abrasive particles may be treated before they are combined with a binder, or they may be surface treated in situ by including a coupling agent into the binder.
[0068] Additional details regarding methods of preparing sol-gel derived abrasive particles can be found, for example, in U.S. Pat. Nos. 4,314,827 (Leitheiser), 5,152,917 (Pieper et al.), 5,435,816 (Spurgeon et al.), 5,672,097 (Hoopman et al.), 5,946,991 (Hoopman et al.), 5,975,987 (Hoopman et al.), and 6,129,540 (Hoopman et al.), and in U.S. Published Patent Application 2009 / 0165394 Al (Culler et al.).
[0069] The surface coating on various abrasive particles can be used to improve the adhesion between the abrasive particles and the binder in the abrasive article, or can be used to assist in electrostatic deposition. In one embodiment, the surface coating described in U.S. Pat. No. 5,352,254 (Celikkaya) can be used in an amount of 0.1% to 2% of the surface coating relative to the weight of the abrasive particles. Such surface coatings are described in U.S. Pat. Nos. 5,213,591 (Celikkaya et al.), 5,011,508 (Wald et al.), 1,910,444 (Nicholson), 3,041,156 (Rowse et al.), 5,009,675 (Kunz et al.), 5,085,671 (Martin et al.), 4,997,461 (Markhoff-Matheny et al.), and 5,042,991 (Kunz et al.). In addition, the surface coating can prevent the shaped abrasive particles from blocking. The term "capping" is used to describe the phenomenon whereby metal particles from the workpiece being ground fuse to the top of the crushed abrasive particles. Surface coatings that perform the above functions are known to those skilled in the art.
[0070] The crushed abrasive particles used in the practice of the present disclosure are preferably selected to have a length and / or width in the range of 0.1 microns to 3500 microns, more typically in the range of 100 microns to 3000 microns, and more typically in the range of 100 microns to 2600 microns, although other lengths and widths may be used.
[0071] Crushed abrasive particles can be selected to have a thickness in the range of 0.1 micron to 1600 microns, more typically 1 micron to 1200 microns, but other thicknesses can be used. In some embodiments, plate-shaped crushed abrasive particles can have an aspect ratio (ratio of length to thickness) of at least 2, 3, 4, 5, 6 or more.
[0072] The length, width and thickness of the abrasive particles can be determined on a single or average basis as desired. Suitable techniques may include inspecting and measuring individual particles, and using automatic image analysis techniques (e.g., using a dynamic image analyzer, such as the CAMSIZER XT image analyzer from Retsch Technology Gmbh, Haan, Germany), according to test method ISO 13402-2:2006 "Particle size analysis - Image analysis method - Part 2: Dynamic graphic analysis method".
[0073] Figure 5 Methods of using patterned coated abrasive articles according to embodiments described herein are shown. Figure 5 Can be used with Figure 6 The abrasive article 600 is mentioned in conjunction with the above. Figure 6 As shown, when viewed from the side, at least some of the shaped abrasive particles have an asymmetric profile. This allows each abrasive particle 630 to have a cutting face. In some embodiments, as described in, for example, 62 / 924,956 filed on October 23, 2019, the shaped abrasive particles are oriented so that the cutting faces of at least some of the abrasive particles 630 are aligned and the cutting tips are oriented away from the backing. The abrasive particles 630 can be embedded in the primer coating 620 so that the particles 630 are aligned perpendicular to the backing 610, or so that there is an inclination angle 660. A size coating 640 may also be present.
[0074] The method 500 can be used to abrade a variety of different workpieces. While in contact, one of the abrasive article and the workpiece is moved relative to each other in a use direction, and a portion of the workpiece is removed.
[0075] Examples of workpiece materials include metals, metal alloys, steel, steel alloys, aluminum exotic metal alloys, ceramics, glass, wood, wood-like materials, composite materials, painted surfaces, plastics, reinforced plastics, stone, and / or combinations thereof. The workpiece may be flat or have a shape or contour associated therewith. Exemplary workpieces include metal parts, plastic parts, particle board, camshafts, crankshafts, furniture, and turbine blades.
[0076] Abrasive articles according to the present invention can be used to grind a workpiece. The methods of grinding range from rough grinding (i.e., high pressure and high removal volume) to polishing (e.g., polishing a medical implant with an emery belt), wherein the latter is generally made with a finer grade of abrasive particles. One such method comprises the steps of bringing an abrasive article (e.g., a coated abrasive article, a nonwoven abrasive article, or a bonded abrasive article) into frictional contact with a surface of a workpiece, and moving at least one of the abrasive article or the workpiece relative to the other to grind at least a portion of the surface.
[0077] In block 510, an abrasive article is provided. In one embodiment, the abrasive article includes a plurality of abrasive particles designed to have a first use orientation and a second use orientation. For example, referring to Figure 6 , moving the abrasive article in a first use direction refers to moving the abrasive article in direction 650 so that the cutting face 630 first encounters the workpiece. The second use direction refers to moving the abrasive article in direction 660. According to various embodiments, a method of using an abrasive article such as an abrasive belt or abrasive disk includes contacting shaped abrasive particles with a workpiece or substrate.
[0078] According to various embodiments, the depth of cut in the substrate or workpiece may be at least about 10 μm, at least about 20 μm, at least about 30 μm, at least about 40 μm, at least about 50 μm, or at least about 60 μm.A portion of the substrate or workpiece is removed by the abrasive article as chips.
[0079] In block 520, the abrasive article is moved against the workpiece in a first direction, which is indicated as, for example, Figure 6 Direction 650.
[0080] According to various embodiments, the abrasive articles described herein can have several advantages when moving in a preferred direction of use. For example, the amount of material removed from the workpiece, the depth of cut in the workpiece, the surface roughness of the workpiece, or a combination thereof, is greater in a first direction than in any other second direction at the same applied force, cutting speed, or a combination thereof.
[0081] For example, at least about 10%, or at least about 15%, at least about 35%, at least about 40%, at least about 45%, at least about 50%, at least about 55%, at least about 60%, at least about 65%, at least about 70%, at least about 75%, at least about 80%, at least about 85%, at least about 90%, at least about 95%, at least about 100%, at least about 120%, at least about 130%, at least about 140%, at least about 150% more material is removed from the substrate or workpiece in the first use direction. In some embodiments, about 15% to about 500% more, or about 30% to about 70%, or about 40% to about 60%, or less than, equal to, or greater than about 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, 110%, 120%, 130%, 140%, 150%, 160%, 170%, 180%, 190%, 200%, 210%, 220%, 230%, 240%, 250%, 260%, 270%, 280%, 290%, 300%, 310%, 320%, 330%, 340%, 350%, 360%, 370%, 380%, 390%, 400%, 410%, 420%, 430%, 440%, 450%, 460%, 470%, 480%, 490%, 500%, 510%, 510%, 520%, 530%, 540%, 550%, 560%, 570%, 580%, 590%, 591%, 592%, 600%, 610%, 611%, 620%, 630%, 640%, 650%, %, 105%, 110%, 115%, 120%, 125%, 130%, 135%, 140%, 145%, 150%, 155%, 160%, 165%, 170%, 175%, 180%, 185%, 190%, 195%, 200%, 205%, 210%, 215%, 220%, 225%, 230%, 235 %, 240%, 245%, 250%, 255%, 260%, 265%, 270%, 275%, 280%, 285%, 290%, 295%, 300%, 305%, 310%, 315%, 320%, 325%, 330%, 335%, 340%, 345%, 350%, 355%, 360%, 365%, 370 %, 375%, 380%, 385%, 390%, 395%, 400%, 405%, 410%, 415%, 420%, 425%, 430%, 435%, 440%, 445%, 450%, 455%, 460%, 465%, 470%, 475%, 480%, 485%, 490%, 495%, or about 500% of the material removed. The amount of material removed can refer to an initial cut amount (e.g., the first cut amount of a cutting cycle) or a total cut amount (e.g., the sum of the amounts of material removed within a set number of cutting cycles).
[0082] As another example, the depth of cut in the substrate or workpiece may be at least about 10%, or at least about 30%, at least about 35%, at least about 40%, at least about 45%, at least about 50%, at least about 55%, at least about 60%, at least about 65%, at least about 70%, at least about 75%, at least about 80%, at least about 85%, at least about 90%, at least about 95%, at least about 100%, at least about 120%, at least about 130%, at least about 140%, or at least about 150% deeper in the first use direction. In some embodiments, the depth in the first use direction is about 10% to about 500%, or about 30% to about 70%, or about 40% to about 60%, or less than, equal to, or greater than about 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100% , 105%, 110%, 115%, 120%, 125%, 130%, 135%, 140%, 145%, 150%, 155%, 160%, 165%, 170%, 175%, 180%, 185%, 190%, 195%, 200%, 205%, 210%, 215%, 220%, 225%, 230%, 235 %, 240%, 245%, 250%, 255%, 260%, 265%, 270%, 275%, 280%, 285%, 290%, 295%, 300%, 305%, 310%, 315%, 320%, 325%, 330%, 335%, 340%, 345%, 350%, 355%, 360%, 365%, 37 0%, 375%, 380%, 385%, 390%, 395%, 400%, 405%, 410%, 415%, 420%, 425%, 430%, 435%, 440%, 445%, 450%, 455%, 460%, 465%, 470%, 475%, 480%, 485%, 490%, 495% or about 500%.
[0083] For another example, the arithmetic mean roughness value (Sa) of a workpiece or substrate cut by moving the abrasive article in a first use direction may be higher than that of a corresponding substrate or workpiece cut under exactly the same conditions but in a second movement direction. For example, when cutting a workpiece or substrate in a first direction, the surface roughness may be about 30% higher, or about 40% higher, about 50% higher, about 60% higher, about 70% higher, about 80% higher, about 90% higher, about 100% higher, about 110% higher, about 120% higher, about 130% higher, about 140% higher, about 150% higher, about 160% higher, about 170% higher, about 180% higher, about 190% higher, about 200% higher, about 210% higher, about 220% higher, about 230% higher, about 240% higher, about 250% higher, about 260% higher, about 270% higher, about 280% higher, about 290% higher, about 300% higher, about 310% higher, about 320% higher, about 330% higher, about 340% higher, about 350% higher, about 360% higher, about 370% higher, about 380% higher, about 390% higher, about 400% higher, about 410% higher, about 420% higher, about 430% higher, about 440% higher, about 450% higher, about 460% higher, about 470% higher, about 480% higher, about 490% higher, about 500% higher, about 510% higher, about 520% higher, about 530% higher, about 540% higher, about 550% higher, about 560% higher, about 57 0%, about 260% higher, about 270% higher, about 280% higher, about 290% higher, about 300% higher, about 310% higher, about 320% higher, about 330% higher, about 340% higher, about 350% higher, about 360% higher, about 370% higher, about 380% higher, about 390% higher, about 400% higher, about 410% higher, about 420% higher, about 430% higher, about 440% higher, about 450% higher, about 460% higher, about 470% higher, about 480% higher, about 490% higher, or about 500% higher. The arithmetic mean roughness value may be in the range of about 1000 to about 2000, about 1000 to about 1100, or less than, equal to, or greater than about 1000, 1050, 1100, 1150, 1200, 1250, 1300, 1350, 1400, 1450, 1500, 1550, 1600, 1650, 1700, 1750, 1800, 1850, 1900, 1950, or about 2000.
[0084] Alternatively, as shown at block 530, the abrasive article can be moved in a second direction 660 that is different from the use direction 650. Figure 6A second orientation 660 is shown that is 180 degrees different from the first orientation 650, but the second orientation 660 may be rotated from about 1 degree to 360 degrees, from about 160 degrees to about 200 degrees, less than, equal to, or greater than about 1 degree, 5 degrees, 10 degrees, 15 degrees, 20 degrees, 25 degrees, 30 degrees, 35 degrees, 40 degrees, 45 degrees, 50 degrees, 55 degrees, 60 degrees, 65 degrees, 70 degrees, 75 degrees, 80 degrees, 85 degrees, 90 degrees, 95 degrees, 100 degrees, 105 degrees, 110 degrees, 115 degrees, 120 degrees, 125 degrees, 130 degrees, 135 degrees, 140 degrees relative to the use orientation 650. , 145 degrees, 150 degrees, 155 degrees, 160 degrees, 165 degrees, 170 degrees, 175 degrees, 180 degrees, 185 degrees, 190 degrees, 195 degrees, 200 degrees, 205 degrees, 210 degrees, 215 degrees, 220 degrees, 230 degrees, 240 degrees, 250 degrees, 260 degrees, 265 degrees, 270 degrees, 275 degrees, 280 degrees, 285 degrees, 290 degrees, 295 degrees, 300 degrees, 305 degrees, 310 degrees, 315 degrees, 320 degrees, 325 degrees, 330 degrees, 335 degrees, 340 degrees, 350 degrees, 355 degrees or about 360 degrees.
[0085] Although it may be desirable to move the abrasive article in the first use direction 650, there are some reasons to move the abrasive article in the second direction 660. For example, it may be beneficial to polish the substrate or workpiece by bringing the substrate or workpiece into contact with the abrasive article and moving the abrasive article in the second direction 660. While not intending to be bound by any particular theory, the inventors hypothesize that movement in the second direction may expose the substrate or workpiece to angles other than the tilt angle of the abrasive article, which may be more suitable for polishing applications.
[0086] Coated abrasive articles prepared according to the method of the present disclosure can be used for example to grind workpieces. Examples of workpiece materials include metals, metal alloys, exotic metal alloys, ceramics, glass, wood, imitation wood materials, composite materials, painted surfaces, plastics, reinforced plastics, stone materials and / or combinations thereof. The workpiece can be flat or have a shape or profile associated therewith. Exemplary workpieces include metal parts, plastic parts, particle boards, camshafts, crankshafts, furniture and turbine blades. The force applied during the grinding process is generally in the range of about 1 kilogram to about 100 kilograms.
[0087] The coated abrasive article prepared according to the method of the present disclosure can be used manually and / or in combination with a machine. During grinding, at least one of the coated abrasive article and the workpiece is moved relative to the other. Grinding can be performed under wet or dry conditions. Exemplary liquids for wet grinding include water, water containing conventional rust-inhibiting compounds, lubricants, oils, soaps, and cutting fluids. The liquid may also contain, for example, a defoaming agent, a degreasing agent.
[0088] All cited references, patents, and patent applications incorporated by reference in this application are incorporated in a consistent manner. In the event of inconsistencies or conflicts between the incorporated references and this application, the information in this application shall prevail. The foregoing description given to enable one of ordinary skill in the art to practice the disclosure protected by the claims should not be construed as limiting the scope of the disclosure, which is defined by the claims and all equivalents thereof.
[0089] The present invention provides a coated abrasive product. The coated abrasive product includes a backing having a first major surface and a second major surface opposite to each other. The coated abrasive product includes a primer layer bonded to the first major surface. The coated abrasive product also includes abrasive particles directly bonded to the primer layer. The abrasive particles are at least partially embedded in the primer layer. The coated abrasive product also includes a secondary layer directly bonded to the primer layer and the abrasive particles. One of the primer layer and the secondary layer includes a patterned coating.
[0090] The article may be implemented such that the patterned coating includes any of lines, swirls, polygons, letters, or numbers.
[0091] The article may be implemented such that the make layer comprises a patterned coating, and wherein the size layer comprises a uniform coating such that for a portion of the backing, the size layer directly contacts the backing.
[0092] The article may be implemented such that both the make layer and the size layer include a patterned coating.
[0093] The article may be implemented such that the size coat comprises a patterned coating, and wherein the coated abrasive article comprises a first color and a second color, and wherein the first color is the color of the size coat.
[0094] The article may further include a supersize coating.
[0095] The article may be implemented such that the supersize coating includes a supersize pattern.
[0096] The article may be implemented such that the primer layer includes a cured resin.
[0097] The article may be realized such that the size layer includes a cured resin.
[0098] The article may be implemented such that the backing comprises a polymer film, a metal foil, a woven fabric, a knitted fabric, paper, vulcanized fibers, a nonwoven, a foam, a screen, a mesh, or a combination thereof.
[0099] The article may be implemented such that it further comprises a laminate applied directly to the first major surface of the backing, and wherein the primer layer is bonded to the laminate.
[0100] The article may be realized such that the backing is pretreated with a backsize, presize, or impregnant.
[0101] The article can be realized such that the abrasive particles are shaped abrasive particles.
[0102] The article can be realized such that at least some of the shaped abrasive particles are aligned relative to each other.
[0103] The article can be implemented such that at least some of the shaped abrasive particles are aligned such that the cutting surface of each of the shaped abrasive particles is aligned and such that the base of each of the shaped abrasive particles is embedded within the make layer.
[0104] The article may be implemented such that the abrasive particles are magnetically coated.
[0105] The article may be implemented such that the patterned coating includes repeating units.
[0106] The article may be implemented such that the patterned coating extends from the center of the abrasive article to the edge of the abrasive article.
[0107] The article may be realized such that the abrasive article is an abrasive disk or an abrasive belt.
[0108] A method for preparing a coated abrasive article. The method includes depositing a curable primer layer precursor on the major surface of a backing. The method also includes depositing a plurality of abrasive grains onto the curable primer layer precursor. The method also includes at least partially curing the curable primer layer precursor. The method also includes depositing a curable size layer precursor on the plurality of abrasive grains. The method also includes at least partially curing the curable size layer precursor. One of the curable primer layer precursor and the curable size layer is deposited on the major surface of the backing in a pattern.
[0109] The method may be implemented such that the pattern comprises repeating units.
[0110] The method may be implemented such that the pattern comprises lines, swirls, polygons, letters or numbers.
[0111] The method may be implemented such that the pattern comprises a first color and a second color.
[0112] The method may be implemented such that the first color is the color of the cured size coat.
[0113] The method may be implemented such that the method further comprises depositing a super glue layer.
[0114] The method may be implemented such that the superfill layer is deposited in a superfill pattern, and wherein the second color comprises a superfill color.
[0115] The method may be implemented such that the plurality of abrasive grains are deposited such that only a first portion of each abrasive grain is embedded within the curable make layer precursor and a second portion of each abrasive grain is free of the make layer precursor.
[0116] The method can be implemented such that the backing comprises a polymer film, a metal foil, a woven fabric, a knitted fabric, paper, vulcanized fibers, a nonwoven, a foam, a screen, a mesh, or a combination thereof.
[0117] The method can also include depositing a laminate coated directly onto the first major surface of the backing, and wherein the make layer is bonded to the laminate.
[0118] The method may further include pretreating the backing with a backsize, presize or impregnant.
[0119] The method may be implemented such that the abrasive particles are deposited in a particle pattern.
[0120] The method may be implemented such that the particle pattern differs from the pattern.
[0121] The method may be implemented such that the abrasive particles include crushed abrasive particles, plate-shaped abrasive particles, shaped abrasive particles, or formed abrasive particles.
[0122] The method can be implemented such that the abrasive particles are shaped abrasive particles, and wherein each of the shaped abrasive particles includes at least one polygonal face.
[0123] The method can be implemented such that each of the shaped abrasive particles includes at least one asymmetric face.
[0124] The method can be implemented such that the abrasive particles are magnetically coated.
[0125] The method can be implemented such that the abrasive particles are aligned on the backing such that at least one polygonal face of some of the shaped abrasive particles are aligned relative to each other.
[0126] The method can be implemented such that at least one polygonal face of some of the shaped abrasive particles are aligned relative to the backing.
[0127] The method can be implemented such that the abrasive particles are angled relative to the backing.
[0128] Example
[0129] Unless otherwise indicated, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight.
[0130] Unless otherwise noted, all other reagents were obtained or purchased from fine chemical suppliers such as Sigma-Aldrich Company, St. Louis, Missouri, or may be synthesized by known methods.
[0131] Abbreviations of units used in the examples:
[0132] ℃: Celsius
[0133] diameter
[0134] cm: centimeters
[0135] in: inches
[0136] g: grams
[0137] g / m 2 : grams per square meter
[0138] rpm: revolutions per minute
[0139] mm: millimeters
[0140] wt.%: weight %
[0141]
[0142]
[0143] Process of preparing mesh abrasive
[0144] Cut the mesh backing into small discs of 6 inches or 3.5 inches in diameter before use.
[0145] A uniform primer coating was achieved by applying 2.36 g of primer resin to a diameter of 6 inches on a mesh backing or apply 1.32g of primer resin to a is achieved on a 3.5-inch mesh backing.
[0146] The patterned primer coating is achieved by applying the primer resin to the mesh backing with a 3M manual rubber roller through a patterned stencil described in U.S. Provisional Application 62 / 945,242 filed on December 9, 2019.
[0147] Mineral drop coating is achieved by laying down abrasive mineral grit onto a base resin layer.
[0148] Curing process: The web abrasive samples were pre-cured at 90°C for 2 hours and then cured at 102°C for at least 6 hours.
[0149] Fig. 7A Shows the diameter is a 3.5-inch mesh backing, and Figure 7B Shows the diameter It is a 3.5-inch mesh backing with a patterned primer and a mineral-coated backing. Figure 7C Shows the diameter 3.5 inch mesh abrasive with patterned base, mineral and size coat.
[0150] Fig.7D Shows the diameter It is a 3.5 inch mesh backing with a uniform primer coating and a uniform mineral coating. Fig. 7E Shows the diameter A 3.5 inch web abrasive with a uniform base coat, a uniform mineral coat, and a patterned size coat. Figure 7F Shows the diameter A 3.5 inch mesh abrasive with a patterned base coat, a patterned mineral coat, and a uniform size coat.
[0151] Figure 7G Shows the diameter 3.5 inch backing with BCA and FRPL 220 uniform primer and patterned mineral coating. Figure 7H Shows Figure 7G A close up view of the product.
[0152] Fig.7I Shows the diameter A 6-inch webbed abrasive article having a uniform make coat, a uniform mineral coat, and a patterned antiloading coat.
Claims
1. A coated abrasive product comprising: a backing having opposing first and second major surfaces; a primer layer, the primer layer being bonded to the first major surface; abrasive particles, the abrasive particles directly bonded to the make coat, wherein the abrasive particles are at least partially embedded in the make coat; a size coat directly bonded to the base coat and the abrasive particles; and Only one of the primer layer or the size coat layer comprises a patterned coating.
2. The article of claim 1, wherein the patterned coating comprises any of lines, swirls, polygons, letters, or numbers.
3. The article of claim 1, wherein the make coat comprises the patterned coating, and wherein the size coat comprises a uniform coating such that for a portion of the backing, the size coat directly contacts the backing.
4. The article of claim 1, wherein the size coat comprises the patterned coating, and wherein the coated abrasive article comprises a first color and a second color, and wherein the first color is the color of the size coat.
5. The article of any one of claims 1 to 3, further comprising a supersize coating. The article of claim 5 , wherein the supersize coating comprises a supersize pattern.
7. The article of any one of claims 1 to 3, wherein the primer layer comprises a cured resin.
8. The article of any one of claims 1 to 3, wherein the size coat comprises a cured resin.
9. The abrasive article of any one of claims 1 to 3, wherein the backing comprises a polymer film, a metal foil, a woven fabric, a knitted fabric, a paper, a vulcanized fiber, a nonwoven, a foam, a screen, a mesh, or a combination thereof.
10. The abrasive article of any one of claims 1 to 3, and further comprising a laminate coated directly to the first major surface of the backing, and wherein the make layer is bonded to the laminate.
11. The abrasive article according to any one of claims 1 to 3, wherein the backing is pretreated with a backsize, a presize or an impregnant.
12. The abrasive article of any one of claims 1 to 3, wherein the abrasive particles are shaped abrasive particles.
13. The abrasive article of claim 12, wherein at least some of the shaped abrasive particles are aligned relative to each other.
14. An abrasive article according to claim 13, wherein at least some of the shaped abrasive particles are aligned so that the cutting surface of each of the shaped abrasive particles is aligned and the base of each of the shaped abrasive particles is embedded in the base layer.
15. The abrasive article of claim 14, wherein the abrasive particles are magnetically coated.
16. The abrasive article of any one of claims 1 to 3, wherein the patterned coating comprises repeating units.
17. The abrasive article of any one of claims 1 to 3, wherein the patterned coating extends from a center of the abrasive article to an edge of the abrasive article.
18. The abrasive article according to any one of claims 1 to 3, wherein the abrasive article is an abrasive disc or an abrasive belt.
19. A method of preparing a coated abrasive article, the method comprising, in order: depositing a curable make layer precursor on a major surface of the backing; depositing a plurality of abrasive particles onto the curable make layer precursor; at least partially curing the curable make layer precursor; depositing a curable size layer precursor on the plurality of abrasive particles; as well as at least partially curing the curable size layer precursor; and Only one of the curable make layer precursor and the curable size layer is deposited in a pattern on the major surface of the backing.
20. The method of claim 19, wherein the pattern comprises repeating units.
21. The method of claim 19, wherein the pattern comprises lines, swirls, polygons, letters, or numbers.
22. The method of claim 19, wherein the pattern comprises a first color and a second color.
23. The method of claim 22, wherein the first color is the color of the cured size coat.
24. The method of claim 22, further comprising depositing a supersize layer.
25. The method of claim 24, wherein the superfill layer is deposited in a superfill pattern, and wherein the second color comprises a superfill color.
26. The method of claim 19, wherein the plurality of abrasive grains are deposited such that only a first portion of each abrasive grain is embedded within the curable make layer precursor and a second portion of each abrasive grain is free of make layer precursor.
27. The method of any one of claims 19 to 26, wherein the backing comprises a polymer film, a metal foil, a woven fabric, a knitted fabric, paper, vulcanized fibers, a nonwoven, a foam, a screen, a mesh, or a combination thereof.
28. The method of any one of claims 19 to 26, and further comprising depositing a laminate directly onto the major surface of the backing, and wherein the primer layer is bonded to the laminate.
29. A method according to any one of claims 19 to 26 and further comprising pre-treating the backing with a backsize, presize or impregnant.
30. The method of any one of claims 19 to 26, wherein the abrasive particles are deposited in a particle pattern.
31. The method of claim 30, wherein the particle pattern is different from the pattern.
32. The method of any one of claims 19 to 26, wherein the abrasive particles comprise crushed abrasive particles, plate-like abrasive particles, shaped abrasive particles, or formed abrasive particles.
33. The method of claim 32, wherein the abrasive particles are shaped abrasive particles, and wherein each of the shaped abrasive particles includes at least one polygonal face.
34. The method of claim 33, wherein each of the shaped abrasive particles comprises at least one asymmetric face.
35. The method of claim 33, wherein the abrasive particles are magnetically coated.
36. The method of claim 33, wherein the abrasive particles are aligned on the backing such that the at least one polygonal face of some of the shaped abrasive particles are aligned relative to each other.
37. The method of claim 36, wherein the at least one polygonal face of some of the shaped abrasive particles are aligned relative to the backing.
38. The method of claim 37, wherein the abrasive particles are angled relative to the backing.