A high-toughness and anti-swelling supramolecular conductive hydrogel and its preparation method and application
Through the copolymerization reaction of cationic surfactant with acrylic acid and long-chain alkyl methacrylate, a high-strength anti-swelling supramolecular conductive hydrogel is formed, which solves the problem of swelling of conductive hydrogel in an aqueous environment and realizes the humid environment The efficient monitoring capability under the simplified preparation process, reduced costs, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202210466437.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-04-29
AI Technical Summary
The existing conductive hydrogels lose their mechanical strength and conductivity stability due to swelling in aqueous environments, which limits the application of flexible sensing materials in humid environments. The existing anti-swelling conductive hydrogel preparation methods are complex and costly. Not conducive to large-scale production.
The cationic surfactant is used to copolymerize with acrylic acid and long-chain alkyl methacrylate in deionized water, and form a high-strength anti-swelling supramolecular conductive hydrogel through hydrophobic association and electrostatic action, simplifying the preparation process and reducing raw material costs .
It achieves high strength, swelling resistance and conductivity in humid environments, is suitable for flexible strain sensors, and is simple and easy to prepare, suitable for large-scale production.
Smart Images

Figure CN114920954B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of hydrogels, and more specifically, relates to a high-toughness and swelling-resistant supramolecular conductive hydrogel and a preparation method and application thereof. Background Art
[0002] With the rapid development of wearable electronic devices, people are in urgent need of a stretchable, recoverable and conductive material to meet the needs of monitoring human movement. Conductive hydrogels have become very promising matrix materials in the field of flexible electronic devices such as flexible strain sensors, artificial skin and soft robots because of their conductive and mechanical properties similar to those of biological tissues. Among them, flexible strain sensors can accurately convert their own deformation into recordable electronic signals and have broad application prospects. However, traditional conductive hydrogels will inevitably "swell" in aqueous environments and lose their mechanical properties, which will also cause signal distortion, severely limiting their practical applications. In addition, the percolation phenomenon of the conductive network caused by swelling and dilution will also reduce the conductivity of the hydrogel. Therefore, it is a challenging task to develop a high-strength and anti-swelling conductive hydrogel material to overcome the degradation of mechanical properties and distortion of sensing signals caused by swelling and deformation.
[0003] In the past two years, some scientific researchers have conducted research on anti-swelling conductive hydrogels. Chinese patent CN202010530723.8 discloses a high-strength anti-swelling chitosan-based physical hydrogel and its preparation method. It adopts a semi-interpenetrating network strategy and utilizes the electrostatic interaction and crystallization of N-carboxyethyl chitosan (CEC). It is prepared by introducing CEC with a low degree of carboxylation into the polyacrylamide hydrophobic cross-linking system (HPAM). However, it is necessary to first use chitosan as a raw material to prepare N-carboxyethyl chitosan, and then interpenetrate with the polyacrylamide hydrophobic cross-linking system to prepare an anti-swelling hydrogel. The preparation process is relatively complicated, and N-carboxyethyl chitosan requires dialysis and freeze-drying, which also requires relatively high experimental conditions. Gao Guanghui's research group at Changchun University of Technology reported a two-step method for preparing anti-swelling hydrogels that can be used as strain sensors. First, chitosan (CS) was dissolved with acrylic acid (AA) to synthesize HP(AAm / AA)-CS hydrogel, and then the HP(AAm / AA)-CS hydrogel was immersed in ferric chloride (FeCl 3 ) solution, so that Fe 3+ Diffusion into the hydrogel network to cross-link chitosan and acrylic acid, ultimately obtaining HP(AAm / AA)-CS-Fe 3+ Anti-swelling hydrogel. Since the hydrogel is a block solid, Fe 3+The uniformity of diffusion into the hydrogel matrix is difficult to control. (Jiajun Xu etc. Cartilage-inspired hydrogel strain sensors with ultrahigh toughness, good self-recovery and stable anti-swelling [J]. J. Mater. Chem. A, 2019, 7, 25441-25448) Professor Chen Fei of Xi'an Jiaotong University and others encapsulated the conductive hydrogel / MXene with the lipid gel (Lipogel) layer through in situ polymerization, and proposed a structural gel composite (SGC) method. The hydrophobic Lipogel coating gives the hydrogel a unique anti-swelling property in the water environment, thereby realizing underwater mechanical sensing applications. The hydrogel structure is exquisitely designed, but the preparation method is relatively cumbersome, which is not conducive to large-scale production. (Zibi Wang etc. A Structural Gel Composite Enabled Robust Underwater Mechanosensing Strategy with High Sensitivity [J]. Advanced Functional Materials, 2022.). Professor Zheng Yinfei of Zhejiang University and Researcher Chen Tao of Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, prepared an ionic liquid gel with excellent waterproof ability and long-term underwater stability by polymerizing hydrophobic monomers (tert-butyl acrylate, t-BuA) in hydrophobic ionic liquids (1-butyl-3-methylimidazole bistrifluoromethanesulfonyl imide salt, [BMIm]TFSI). However, ionic liquids are very expensive, which is not conducive to large-scale production. (Junjie Wei etc. A fully hydrophobic ionogelenables highly efficient wearable underwater sensors and communicators [J]. Materials Horizonsz. 2021, 8, 2761-2770). The currently reported general preparation methods of anti-swelling conductive hydrogels are relatively cumbersome and costly, which is not conducive to large-scale production. Summary of the invention
[0004] In order to solve the above-mentioned deficiencies and shortcomings in the prior art, the primary purpose of the present invention is to provide a high-toughness and anti-swelling supramolecular conductive hydrogel. The hydrogel has unique anti-swelling properties, high strength, underwater adhesion, conductive sensitivity and stability. It solves the problem that the existing conductive hydrogel loses mechanical strength and conductive stability due to swelling in an aqueous environment, so as to truly meet the actual needs of flexible sensing materials for accurately monitoring human body movements in a humid environment.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned high-strength anti-swelling supramolecular conductive hydrogel. The method is simple and easy to implement, the raw materials are cheap and widely available, and it is easy to achieve large-scale production.
[0006] Another object of the present invention is to provide an application of the above-mentioned high-strength anti-swelling supramolecular conductive hydrogel. The prepared hydrogel material has important application prospects in the field of flexible strain sensors used in humid environments (such as sweaty skin, rain, swimming, surfing, underwater operations, etc.).
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A high-toughness and swelling-resistant supramolecular conductive hydrogel is prepared by adding a cationic surfactant to deionized water and magnetically stirring at 10-40°C to obtain a solution A; adding a long-chain alkyl methacrylate to the solution A and magnetically stirring at 10-40°C, then adding acrylic acid and magnetically stirring until it is completely dissolved, then adding an initiator and stirring and mixing uniformly to obtain a solution B; and ultrasonically defoaming the solution B, pouring it into a glass mold, and reacting at 40-70°C to obtain the supramolecular conductive hydrogel.
[0009] Preferably, the mass ratio of the cationic surfactant to the volume of deionized water is (1-6) g:20 mL.
[0010] More preferably, the mass ratio of the cationic surfactant to the volume of deionized water is (2-5) g:20 mL.
[0011] Preferably, the cationic surfactant is a quaternary ammonium salt cationic surfactant, and its molecular formula is: [R 1 R 2 R 3 N + -CH 3 ]X - , where R 1 is a C10-C18 long-chain alkyl group, R 2 , R 3 is methyl, ethyl, or benzyl or a C10-C18 long-chain alkyl group, X - It is chloride, bromide or iodide or other anionic groups, preferably chloride or bromide.
[0012] More preferably, the cationic surfactant is any one of dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, didodecyldimethylammonium bromide, ditetradecyldimethylammonium bromide, dihexadecyldimethylammonium bromide, dioctadecyldimethylammonium bromide, dodecyldimethylethylammonium bromide, tetradecyldimethylethylammonium bromide, hexadecyldimethylethylammonium bromide, dodecyldimethylbenzylammonium bromide, and hexadecyldimethylbenzylammonium bromide.
[0013] Preferably, the volume ratio of the mass of acrylic acid, the mass of cationic surfactant, the mass of initiator and the volume ratio of long-chain alkyl of methacrylic acid is 10g:3g:(50-150)mg:(0.5-2.5)mL.
[0014] Preferably, the molecular formula of the long-chain alkyl methacrylate is: CH 2 =C(CH 3 )COO(CH 2 ) n CH 3 , wherein n=11-17; the initiator is ammonium persulfate or potassium persulfate; the long-chain alkyl methacrylate is one or more of dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate or octadecyl methacrylate.
[0015] The method for preparing the high-toughness and anti-swelling supramolecular conductive hydrogel comprises the following specific steps:
[0016] S1. Add a cationic surfactant to deionized water and stir magnetically at 10 to 40° C. to obtain a solution A;
[0017] S2. Add long-chain alkyl methacrylate to solution A and stir magnetically at 10-40°C Ⅰ, then add acrylic acid and stir magnetically until it is completely dissolved, then add initiator and stir Ⅱ, mix well, and obtain solution B;
[0018] S3. Solution B is ultrasonically defoamed, then poured into a glass mold and reacted at 40-70° C. to obtain a supramolecular conductive hydrogel with high toughness and anti-swelling properties.
[0019] Preferably, the stirring time in step S1 is 2 to 6 hours, and the stirring speed is 200 to 800 rpm; the stirring rate in step S2 is 200 to 800 rpm; the stirring time I is 0.5 to 3 hours, and the stirring time II is 10 to 30 minutes; the ultrasonic defoaming time in step S3 is 5 to 10 minutes; and the reaction time is 12 to 24 hours.
[0020] The supramolecular conductive hydrogel with high toughness and swelling resistance is used in the field of flexible strain sensors in humid environments (such as sweaty skin, rain, swimming, surfing, underwater operations, etc.).
[0021] The preparation method of the high-strength and anti-swelling supramolecular conductive hydrogel of the present invention adopts a one-step method, in which acrylic acid and a hydrophobic monomer long-chain alkyl methacrylate undergo copolymerization under the action of an initiator in the presence of a cationic surfactant to form a high-strength anti-swelling supramolecular hydrogel with acrylic acid and a long-chain alkyl methacrylate copolymer as the main body. On the one hand, the cationic surfactant can form micelles, promote the aggregation of long-chain alkyl methacrylate segments to form a stable hydrophobic region, and serve as a physical crosslinking point of the hydrogel network; on the other hand, the quaternary ammonium salt head of the cationic surfactant can be adsorbed on the hydrogel network chain through a strong electrostatic interaction with the carboxyl group of acrylic acid on the hydrogel network chain. The hydrophobic long-chain tail of the cationic surfactant and the shielding effect of the hydrophilic carboxyl group on the hydrogel network main chain give the hydrogel excellent anti-swelling property. The interaction between the cationic surfactant and the acrylic acid segment in the hydrogel network is very important, which gives the hydrogel high strength and toughness, excellent anti-swelling property and conductivity. However, the anionic surfactant and polyacrylic acid have no such effect and cannot resist swelling at all. At the same time, when adhering to human skin underwater, this strong hydrophobic effect and the flexibility of the hydrogel enable the hydrogel sample to adhere firmly to the human skin, forming a seamless bond, and it is difficult for water to penetrate between the hydrogel sample and the skin. Whether the finger joints are bent and stretched, or the wrist joints are bent up and down, the hydrogel can maintain close contact with the joint skin and will not detach. In addition, the electrostatic adsorption of cationic surfactants and acrylic acid carboxyl groups on the hydrogel network chain can greatly promote the dissociation of hydrogen ions, giving the hydrogel good conductivity.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The supramolecular conductive hydrogel of the present invention is formed by hydrophobic association and electrostatic action. There is no chemical crosslinking in the system. It is a supramolecular hydrogel and is easy to recycle. The conductive hydrogel has excellent anti-swelling property, high strength, large deformation capacity and good conductivity. It overcomes the technical defects that most of the existing conductive hydrogels easily absorb water and swell in an aqueous environment, resulting in serious performance degradation and inability to achieve signal monitoring in an aqueous environment. It can achieve long-term underwater anti-swelling stability, reliability and durability. After being immersed in deionized water for 7 days, it still maintains good mechanical properties, such as high tensile strength (800-1600KPa) and excellent large deformation capacity (>900%). It can be used as a strain sensor and shows good sensitivity, reliability, durability and stability in deionized water, physiological saline and seawater environments.
[0024] 2. The supramolecular conductive hydrogel of the present invention can maintain shaped adhesion to the surface of human skin underwater without the help of additional tape. When the fingers, wrists and other joints move, it can extend and retract along with the joint movement without debonding from the skin surface, thereby greatly improving the monitoring accuracy of human underwater movement signals.
[0025] 3. The preparation method of the present invention is simple and easy to implement, and water is used as solvent in the preparation process, and the reaction conditions are simple, mild and pollution-free. The raw materials are cheap and widely available, and it is easy to realize large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the total reflection infrared spectrum of the high-toughness and swelling-resistant supramolecular conductive hydrogel prepared in Example 1.
[0027] Figure 2 The swelling curves of the high-toughness and swelling-resistant supramolecular conductive hydrogel prepared in Example 1 after being immersed in different aqueous environments for 15 days.
[0028] Figure 3 This is a diagram showing the high-toughness and swelling-resistant supramolecular conductive hydrogel prepared in Example 1 adhering to human fingers and wrists in water.
[0029] Figure 4 This is a photo of the high-strength, tough and swelling-resistant supramolecular conductive hydrogel prepared in Example 1 turning on an LED light in water.
[0030] Figure 5 This is a test signal diagram of the high-strength and anti-swelling supramolecular conductive hydrogel prepared in Example 1 used as a strain sensor to monitor the bending and extension movement of finger joints. DETAILED DESCRIPTION
[0031] The content of the present invention is further described below in conjunction with specific examples, but it should not be construed as limiting the present invention. If not specifically indicated, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0032] The chemicals used in the embodiments of the present invention are as follows: hexadecyl trimethyl ammonium bromide (CTAB): also known as N,N,N-trimethyl-1-hexadecyl ammonium bromide; whale trimethyl ammonium bromide; positive soap; cetyl trimethyl ammonium bromide; trimethyl ammonium bromide; hexadecyl trimethyl ammonium bromide; hexadecyl trimethyl quaternary ammonium bromide; hexadecyl trimethyl ammonium bromide; CTMAB; trimethyl hexadecyl ammonium bromide; trimethyl ammonium bromide; trimethyl amino hexadecyl ester; trimethyl amino hexadecyl ester bromide; trimethyl ammonium bromide; (1-hexadecyl) trimethyl ammonium bromide. Analytically pure, Shanghai MacLean Company; acrylic acid: molecular formula C 3 H 4 O 2 , analytically pure, Tianjin Damao Chemical Reagent Factory; dodecyl methacrylate: also known as lauryl methacrylate, molecular formula is C 39 H 72 O 6 , analytically pure, Shanghai McLean Company; ammonium persulfate: molecular formula is H 8 N 2 O 8 S 2 , analytical grade, Tianjin Zhiyuan Chemical Reagent Co., Ltd.; physiological saline and artificial seawater are commercially available. Deionized water was homemade in the laboratory.
[0033] The glass mold used in the present invention has the following specifications: glass plates with a thickness of 10 mm at the top and bottom, a square silicone mold frame of 100 mm*100 mm in the middle, a mold frame edge width of 10 mm, and a thickness of 2 mm. The mold frame size can be adjusted according to actual conditions.
[0034] Example 1
[0035] 1. Add 3.0 g of hexadecyltrimethylammonium bromide (CTAB) to 20 mL of deionized water and stir magnetically at 800 rpm for 3 h at 25 °C to obtain solution A.
[0036] 2. Add 1.25 mL of dodecyl methacrylate (LMA) to solution A, and stir magnetically at 500 rpm for 1 h at 25°C; then add 10 g of acrylic acid (AAc), and stir magnetically at 500 rpm for 20 min at 25°C until all dissolved, then add 100 mg of initiator ammonium persulfate, stir for 30 min, and mix thoroughly to obtain solution B;
[0037] 3. Solution B was ultrasonically defoamed for 5 minutes, then poured into a glass mold (100mm*100mm*2mm), and reacted at 60°C for 15 hours to obtain a high-strength anti-swelling supramolecular conductive hydrogel. The supramolecular conductive hydrogel was taken out and soaked in a large amount of deionized water for 7 days for standby use, during which the water was changed every 24 hours.
[0038] After soaking in deionized water for 7 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel of this embodiment at 25°C was about 1613KPa, and the tensile deformation was about 940%, showing good flexibility and elasticity. After soaking in deionized water at 25°C for 15 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel at 25°C was about 1597KPa, and the tensile deformation was about 940%, and the mechanical properties remained basically unchanged.
[0039] Figure 1 This is the total reflection infrared spectrum of the high-toughness and anti-swelling supramolecular conductive hydrogel sample prepared in Example 1. The total reflection infrared spectrum can provide information of the sample surface at a depth of 2 μm, so the infrared spectrum test results reflect the structural composition of the hydrogel surface layer. Figure 1 It can be seen that 1710cm -1 The peak at 2923cm belongs to the stretching vibration of the carboxyl group (C=O) of the polyacrylic acid chain segment. -1 and 2855cm -1 The typical crab-leg-shaped peak at 100° is attributed to the -CH 3 and -CH 2 The vibration peaks prove that the quaternary ammonium salt head of the cationic surfactant CTAB can be adsorbed on the hydrogel polymer network through the strong electrostatic interaction between it and the carboxyl group of acrylic acid. Figure 2 The swelling curves of the high-toughness and anti-swelling supramolecular conductive hydrogel samples prepared in Example 1 after being immersed in different aqueous environments for 15 days are shown. When the hydrogel sample is immersed in an aqueous environment, the methyl and long-chain alkyl hydrophobic tails on CTAB can shield the hydrophilic groups in the hydrogel network, namely the carboxyl groups, and form a dense hydrophobic layer on the surface of the hydrogel, which effectively prevents water molecules from diffusing into the gel matrix, thereby enabling the hydrogel sample to maintain long-term anti-swelling stability in an aqueous environment. Figure 3 The following are the effects of the high-toughness and anti-swelling supramolecular conductive hydrogel prepared in Example 1 adhering to human fingers and wrists in water. (a) shows the hydrogel seamlessly adhering to the straightened finger, (b) shows the hydrogel seamlessly adhering to the bent finger, (c) shows the hydrogel seamlessly adhering to the downward-bent wrist (convex surface), and (d) shows the hydrogel seamlessly adhering to the upward-bent wrist (concave surface). Figure 3It can be seen that the high-toughness and anti-swelling supramolecular conductive hydrogel exhibits good excipient adhesion to the human b joint. Figure 3 (a)) or bending ( Figure 3 (b)), the hydrogel samples adhered to the finger skin without interface detachment; regardless of whether the wrist was bent downward (convex) ( Figure 3 (c)) or is it curved upward (concave) ( Figure 3 (d)), the hydrogel sample also adheres tightly to the wrist skin without interfacial detachment. Figure 4 The following are photos of the high-toughness and anti-swelling supramolecular conductive hydrogel prepared in Example 1 conducting an LED light in water. (a) shows that the LED light bulb becomes darker when the hydrogel strip is stretched, and (b) shows that the LED light bulb becomes brighter when the hydrogel strip is retracted. The high-toughness and anti-swelling supramolecular conductive hydrogel exhibits excellent conductivity and strain sensitivity in water. As the hydrogel strip connected to the circuit is stretched, the brightness of the LED light bulb becomes darker ( Figure 4 (a)), the LED light brightness increases when the hydrogel strip retracts ( Figure 4 (b)). Figure 5 The following are sensor signal diagrams of the high-toughness and swelling-resistant supramolecular conductive hydrogel prepared in Example 1 as a strain sensor in different aqueous environments. Among them, (a) is the sensor signal measured in deionized water, (b) is the sensor signal measured in physiological saline, and (c) is the sensor signal measured in seawater. Specifically, the supramolecular conductive hydrogel of Example 1 was immersed in deionized water, physiological saline and seawater, respectively, and the two ends of the gel were connected to the positive and negative electrodes of the electrochemical workstation through wires, and the resistance change of the sensor was recorded and calculated in real time. The discharge voltage of the electrochemical workstation was 1V, the spline deformation was between 0 and 100%, and the stretching speed was 100mm / min. From Figure 5 It can be seen that the signals collected by the supramolecular conductive hydrogel of Example 1 in three aqueous environments, namely, deionized water, physiological saline and seawater, are very stable with almost no fluctuations, indicating that the supramolecular conductive hydrogel can be used as a strain sensor to achieve stable and accurate signal collection in an aqueous environment.
[0040] Example 2
[0041] 1. Add 3.0 g of hexadecyltrimethylammonium bromide to 30 mL of deionized water and stir magnetically at 35 °C at 500 rpm for 6 h to obtain a clear solution A.
[0042] 2. Add 1.25 mL of dodecyl methacrylate to solution A, stir magnetically at 35°C and 500 rpm for 3 h, then add 10 g of acrylic acid, stir magnetically at 30°C and 500 rpm for 1 h until all dissolved, then add 90 mg of initiator ammonium persulfate and stir for 20 min, mix thoroughly and evenly to obtain solution B;
[0043] 3. Solution B was ultrasonically defoamed for 5 minutes, then poured into a glass mold (100 mm*100 mm*2 mm), and reacted at 60°C for 24 hours to obtain a high-strength anti-swelling supramolecular conductive hydrogel. The supramolecular conductive hydrogel was taken out and immersed in a large amount of deionized water for 7 days for use, during which the water was changed every 24 hours.
[0044] After soaking in deionized water for 7 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel of this embodiment at 25°C was about 1178KPa, and the tensile deformation was about 972%, showing good flexibility and elasticity. After soaking in deionized water at 25°C for 15 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel at 25°C was about 1173KPa, and the tensile deformation was about 955%, and the mechanical properties remained basically unchanged.
[0045] Example 3
[0046] 1. Add 3.0 g of hexadecyltrimethylammonium bromide to 40 mL of deionized water and stir magnetically at 500 rpm for 15 min at 30°C to obtain a clear solution A.
[0047] 2. Add 1.25 mL of dodecyl methacrylate to solution A, stir magnetically at 600 rpm for 4 h at 30°C, then add 10 g of acrylic acid, stir magnetically at 600 rpm for 1.5 h at 30°C until all dissolved, then add 100 mg of initiator potassium persulfate, stir for 15 min, mix thoroughly, and obtain solution B;
[0048] 3. Solution B was ultrasonically defoamed for 5 min, then poured into a glass mold (100 mm*100 mm*2 mm), and reacted at 60°C for 12 h to obtain a high-strength anti-swelling supramolecular conductive hydrogel. The supramolecular conductive hydrogel was taken out and soaked in a large amount of deionized water for 7 days for use, during which the water was changed every 24 hours.
[0049] After soaking in deionized water for 7 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel of this embodiment at 25°C was about 805KPa, and the tensile deformation was about 970%, showing good flexibility and elasticity. After soaking in deionized water at 25°C for 15 days, the tensile strength of the high-toughness and anti-swelling supramolecular conductive hydrogel at 25°C was about 779KPa, and the tensile deformation was about 934%. Although the tensile strength and tensile deformation of the sample decreased slightly, it still maintained a high ductility.
[0050] Comparative Example 1
[0051] Add 10 g of acrylic acid (AAc) to 20 mL of deionized water, stir magnetically at 500 rpm at 25°C for 20 min until completely dissolved, then add 100 mg of initiator ammonium persulfate and stir for 30 min. Mix thoroughly, then pour into a glass mold (100 mm*100 mm*2 mm), react at 60°C for 15 h to obtain a hydrogel, marked as comparative sample 1, and take out and place in a polyethylene sealed bag, seal and store for later use.
[0052] In the preparation process of this comparative example, no surfactant and long-chain alkyl methacrylate were added, and the obtained hydrogel had very poor anti-swelling property. It was severely deformed after being immersed in water for 30 minutes, and the mechanical strength could not be tested, and the hydrogel completely lost its usability.
[0053] Comparative Example 2
[0054] 1. Add 3.0 g of anionic surfactant sodium dodecyl sulfate (SDS) into 20 mL of deionized water and stir magnetically at 500 rpm for 3 h at 25 °C to obtain a clear solution A.
[0055] 2. Add 1.25 mL of dodecyl methacrylate to solution A, stir magnetically at 500 rpm for 1 h, then add 10 g of acrylic acid, stir magnetically at 500 rpm for 20 min until all dissolved, then add 100 mg of initiator ammonium persulfate, stir for 30 min, mix thoroughly, and obtain solution B;
[0056] 3. Solution B was ultrasonically defoamed for 5 min, then poured into a glass mold (100 mm*100 mm*2 mm), and reacted at 60°C for 15 h to obtain a hydrogel, which was marked as comparative sample 2. The hydrogel was taken out and placed in a polyethylene sealed bag for sealed storage.
[0057] In the preparation process of this comparative example, anionic surfactants were used instead of cationic surfactants, and the resulting hydrogel had relatively poor anti-swelling properties. After being immersed in water for 24 hours, the swelling ratio was as high as 25 times, and the hydrogel became very brittle and broke into pieces when squeezed. The mechanical strength could not be tested and the hydrogel lost its usability.
[0058] Table 1 shows the tensile properties of the supramolecular conductive hydrogels prepared in Examples 1-3 after being immersed in deionized water for 7 days. Among them, the tensile properties test of the obtained high-strength anti-swelling supramolecular conductive hydrogel was carried out on a universal material testing machine, and the test specimens were long strips with a length of 400mm, a width of 10mm, and a thickness of 2.0mm. The clamp spacing was 10mm, and the tensile rate was 100mm / min. Five specimens were tested for each sample and the average value was taken. It can be seen from Table 1 that the supramolecular conductive hydrogels of Examples 1-3 exhibited high tensile strength (>800kPa) and large deformation capacity (>900%) in water, and the mechanical properties remained almost unchanged after being immersed in deionized water for 7 days and 15 days, and had excellent anti-swelling properties and long-term stability. However, Comparative Examples 1 and Comparative Examples 2 will soon swell and deform in water, resulting in serious performance degradation, and mechanical properties cannot be tested.
[0059] Table 1 Comparison of tensile properties of supramolecular conductive hydrogels prepared in Examples 1-3 after immersion in deionized water for 7 days and 15 days
[0060]
[0061]
[0062] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high-toughness and anti-swelling supramolecular conductive hydrogel, characterized in that: The supramolecular conductive hydrogel is prepared by adding a cationic surfactant into deionized water and magnetically stirring at 10 to 40° C. to obtain a solution A; Add long-chain alkyl methacrylate to solution A and stir magnetically at 10-40°C, then add acrylic acid and stir magnetically until it is completely dissolved, then add initiator and stir to mix evenly to obtain solution B; after ultrasonic defoaming, pour solution B into a glass mold and react at 40-70°C to obtain a solution; the mass ratio of the cationic surfactant to deionized water is (1-6) g:20 mL; the mass ratio of the acrylic acid, the mass of the cationic surfactant, the mass of the initiator and the volume ratio of the long-chain alkyl methacrylate is 10 g:3 g:(50-150) mg:(0.5-2.5) mL; the initiator is ammonium persulfate or potassium persulfate; the cationic surfactant is a quaternary ammonium salt cationic surfactant, and the molecular formulas thereof are: [R1R2R3N + -CH3]X - , wherein R1 is a C10-C18 long-chain alkyl group, R2 and R3 are methyl, ethyl, or benzyl or a C10-C18 long-chain alkyl group, and X - is chloride ion, bromide ion or iodide ion; the molecular formula of the long-chain alkyl methacrylate is: CH2=C(CH3)COO(CH2) n CH3, where n = 11~17.
2. The high-toughness and anti-swelling supramolecular conductive hydrogel according to claim 1, characterized in that: The cationic surfactant is any one of dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, didodecyldimethylammonium bromide, ditetradecyldimethylammonium bromide, dihexadecyldimethylammonium bromide, dioctadecyldimethylammonium bromide, dodecyldimethylethylammonium bromide, tetradecyldimethylethylammonium bromide, hexadecyldimethylethylammonium bromide, dodecyldimethylbenzylammonium bromide and hexadecyldimethylbenzylammonium bromide.
3. The high-toughness and anti-swelling supramolecular conductive hydrogel according to claim 1, characterized in that: The long-chain alkyl methacrylate is one or more of dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate or octadecyl methacrylate.
4. A method for preparing a high-toughness and anti-swelling supramolecular conductive hydrogel according to any one of claims 1 to 3, characterized in that: The specific steps include: S1. Add a cationic surfactant to deionized water and stir magnetically at 10 to 40°C to obtain solution A; S2. Add long-chain alkyl methacrylate to solution A and stir magnetically at 10 to 40°C I, then add acrylic acid and stir magnetically until it is completely dissolved, then add initiator and stir II, mix well, and obtain solution B; S3. Solution B is ultrasonically defoamed, then poured into a glass mold and reacted at 40 to 70°C to obtain a supramolecular conductive hydrogel with high strength and anti-swelling properties.
5. The method for preparing the high-toughness and anti-swelling supramolecular conductive hydrogel according to claim 4, characterized in that: The stirring time in step S1 is 2 to 6 hours, and the stirring speed is 200 to 800 rpm; The stirring rate in step S2 is 200 to 800 rpm; The stirring time of I is 0.5 to 3 h, and the stirring time of II is 10 to 30 min.
6. The method for preparing the high-toughness and anti-swelling supramolecular conductive hydrogel according to claim 4, characterized in that: The ultrasonic defoaming time in step S3 is 5 to 10 min; the reaction time is 12 to 24 h.
7. Application of the high-toughness and swelling-resistant supramolecular conductive hydrogel according to any one of claims 1 to 3 in the field of flexible strain sensors in a humid environment.
Citation Information
Patent Citations
High-strength anti-swelling chitosan-based physical hydrogel and preparation method thereof