A kind of thermal conductive silicone gel and preparation method thereof

By using modifiers such as vinyl silicone oil, hydrogen-containing silicone oil and alkoxy silicone oil in thermal conductivity, combined with thermal fillers and catalysts, the problems of low thermal conductivity and rising thermal resistance are solved, and efficient and stable thermal conductivity are achieved. Performance, suitable for the high temperature and high power heat dissipation needs of 5G base stations.

CN114958002BActive Publication Date: 2024-11-15XIAMEN WELDTONE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210744200.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-27
Publication Date
2024-11-15
Estimated Expiration
2042-06-27

AI Technical Summary

Technical Problem

The existing thermal conductivity silicon gel has low thermal conductivity and untimely heat dissipation. The thermal resistance increases significantly after long-term aging, resulting in performance attenuation and affecting the heat dissipation effect and reliability of 5G base stations.

Method used

Using vinyl silicone oil, hydrogen-containing silicone oil and alkoxy silicone oil as modifiers, combined with thermal fillers and catalysts, the thermal conductivity and high temperature stability of thermal conductivity of thermally conductive silicone gels can be improved through specific structures and composite methods to ensure that they are Maintain efficient heat dissipation during long-term use.

Benefits of technology

It significantly improves the thermal conductivity and long-term stability of thermally conductive silicon gel, ensures continuous and efficient heat dissipation in high-temperature environments, extends service life, and improves the heat dissipation effect and reliability of 5G base stations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114958002B_ABST
    Figure CN114958002B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of thermal conductive interface materials, and relates to a single-component highly reliable thermal conductive silicone gel and a preparation method thereof. The thermal conductive silicone gel contains 40-70 parts by weight of vinyl silicone oil, 0.5-3 parts by weight of hydrogenated silicone oil, 0.5-25 parts by weight of alkoxy silicone oil, 400-2200 parts by weight of thermal conductive filler, 1-5 parts by weight of catalyst, and 0-7 parts by weight of optional pigment, and the alkoxy silicone oil has a structure shown in formula (I). The thermal conductive silicone gel provided by the present invention has the advantages of higher thermal conductivity and more stable performance after long-term aging compared to existing products on the market, thereby ensuring that it can always maintain high heat dissipation efficiency during long-term use and has strong reliability. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal conductive interface materials, and particularly relates to a single-component highly reliable thermal conductive silicone gel and a preparation method thereof. Background Art

[0002] The fifth generation of mobile communication technology (5G) has the characteristics of large bandwidth, high speed, and wide connection compared with the previous 3G / 4G, and has accelerated the development of industries such as AI and the Internet of Things. The dependence of digital industries on communication infrastructure will make 5G new infrastructure an important driver for boosting the economy. 5G has three main application scenarios, namely: eMBB (Enhanced Mobile Broadband), uRLLC (Ultra Reliable Low Latency Communications), and mMTC (Massive Machine Type Communications). With the continuous development of mobile communication services, massive amounts of data need to be processed, and the transmission rate needs to be doubled. The power consumption of BBU and AAU of 5G base stations will gradually increase. The power consumption of 5G base stations has reached 2.5-3.5 times that of 4G base stations, which is mainly generated by AAU and BBU in the process of performing signal conversion, processing and transmission. At present, the full load power of a single station is nearly 3700W. The increase in base station power consumption means an increase in heat generation. If the heat dissipation is not timely, the internal ambient temperature of the base station will rise. Once it exceeds the rated temperature, it will seriously affect the stability of the network and the service life of the equipment. In order to better solve the heat dissipation problem of 5G base stations and reduce the temperature difference between the chip and the shell, it is necessary to use ultra-high thermal conductivity thermal interface materials to allow the heat on the chip to be transferred to the heat dissipation shell more quickly.

[0003] At present, most of the thermal conductive filler modifiers used in the preparation of thermal conductive pads and thermal conductive silicone greases on the market are C5-C 16 Long-chain silanes or phthalates, etc., result in low thermal conductivity of the corresponding products, poor heat dissipation effect, and serious performance degradation after long-term aging, resulting in low product reliability. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of low thermal conductivity, untimely heat dissipation, significant increase in thermal resistance and performance degradation of traditional thermally conductive silicone gels, and to provide a single-component, highly reliable ultra-high thermal conductive silicone gel with high thermal conductivity and stable performance after long-term aging and a preparation method thereof.

[0005] The first aspect of the present invention provides a thermally conductive silicone gel, wherein the thermally conductive silicone gel contains 40-70 parts by weight of vinyl silicone oil, 0.5-3 parts by weight of hydrogenated silicone oil, 0.5-25 parts by weight of alkoxy silicone oil, 400-2200 parts by weight of thermally conductive filler, 1-5 parts by weight of catalyst and 0-7 parts by weight of optional pigment, wherein the alkoxy silicone oil has a structure shown in formula (I):

[0006]

[0007] In formula (I), R 11 , R 12 and R 13 Each independently for OC a H 2a+1 an alkoxy group, a is an integer of 0-16; R 14 and R 15 Each independently is C b H 2b+1 alkyl, b is an integer of 0-16; R 16 , R 17 and R 18 Each independently selected from OC a' H 2a'+1 or all selected from C b' H 2b'+1 an alkyl group, a' is an integer from 0 to 16, b' is an integer from 0 to 16; or R 16 , R 17 and R 18 Any two of them are independently OC a" H 2a"+1 Alkoxy or C b" H 2b"+1 alkyl and the remaining one is vinyl, a" is an integer of 0-16, b" is an integer of 0-16; and n in formula (I) is an integer of 4-50.

[0008] The key to the present invention is to use an alkoxy silicone oil having the formula (I) as a modifier, wherein the three groups bonded to the Si atom at at least one end of the alkoxy silicone oil are all alkoxy groups. On the one hand, the thermal conductive filler modified by the alkoxy silicone oil has a lower oil absorption value than the thermal conductive filler modified by the common long-chain alkyl silane coupling agent, small molecule silane or terminal hydroxyl silane, and can make the thermal conductive filler easier to fill and disperse. This is because the thermal conductive silicone gel is mostly silicone oil except for the thermal conductive filler, and the molecules wrapped or grafted on the surface of the thermal conductive filler modified by the alkoxy silicone oil are similar to the molecular structure of the silicone oil, so that it can be better soluble in the silicone oil, which is similar to the principle of like dissolves like, thereby The thermal conductive gel using alkoxy silicone oil can maintain high efficiency and high stability during long-term heat dissipation, while most of the thermal conductive silicone gels on the market that have been treated with long-chain alkyl silane coupling agents, small molecule silanes or terminal hydroxyl silanes are prone to cracking during long-term high-temperature use due to insufficient dissolution of the thermal conductive filler and silicone oil. In addition, the thermal conductive filler treated with alkoxy silicone oil will not dry out during long-term high-temperature use after making the gel, compared with the thermal conductive filler treated with small molecule silane. This is because the silicone oil macromolecule is more resistant to high temperature than the silane small molecule; on the other hand, the long-chain alkyl grafted with silicone oil makes the modified powder more resistant to high temperature. In summary, the thermal conductive silicone gel provided by the present invention has a higher thermal conductivity coefficient than existing products on the market and has the advantages of more stable performance after long-term aging, thereby ensuring that it can always maintain high heat dissipation efficiency during long-term use and has strong reliability.

[0009] In a preferred embodiment, in formula (I), R 11 , R 12 and R 13 Each independently for OC a H 2a+1 an alkoxy group, a is an integer of 1 to 16; R 14 and R 15 Each independently is C b H 2b+1 alkyl, b is an integer of 1-16; R 16 , R 17 and R 18 Any two of them are independently C b" H 2b"+1 The alkyl group is an alkyl group and the remaining one is a vinyl group, b" is an integer of 1-16; and n is an integer of 4-50.

[0010] In a preferred embodiment, the vinyl silicone oil has a structure shown in formula (II):

[0011]

[0012] In formula (II), R 21For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 Each independently is C1-C 16 alkyl, m is an integer from 0 to 1000; or, m R 24 At least one of them is vinyl and the remaining R 24 C1-C 16 The alkyl group, R 21 , R 22 , R 23 , R 25 , R 26 , R 27 and R 28 Each is independently a C1-C5 alkyl group, and m is an integer of 0-1000.

[0013] In a preferred embodiment, the hydrogen-containing silicone oil is composed of a terminal hydrogen-containing silicone oil represented by formula (III) and a side hydrogen-containing silicone oil represented by formula (IV);

[0014]

[0015] In formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 Each independently is C1-C 16 alkyl, p is an integer from 0 to 1000; in formula (IV), R 41 and R 45 are each independently H or a C1-C5 alkyl group, R 42 , R 43 , R 44 , R 46 and R 47 Each is independently a C1-C5 alkyl group, and q is an integer of 0-1000. The terminal hydrogen-containing silicone oil is used for chain extension, and the side hydrogen-containing silicone oil is used for cross-linking, and such a compound can significantly improve the bulk strength and toughness of the thermal conductive silicone gel.

[0016] In a preferred embodiment, the mass ratio of the terminal hydrogen-containing silicone oil to the side hydrogen-containing silicone oil is (1-10):1.

[0017] In a preferred embodiment, the content of Si—H in the terminal hydrogen-containing silicone oil is 0.2-0.6 mmoles / g; the content of Si—H in the side hydrogen-containing silicone oil is 0.5-0.8 mmoles / g.

[0018] In a preferred embodiment, the vinyl content in the vinyl silicone oil is 0.2-0.8 mmoles / g.

[0019] In a preferred embodiment, the viscosity of the vinyl silicone oil is 30-500 cSt; the viscosity of the hydrogen-containing silicone oil is 40-200 cSt; and the viscosity of the alkoxy silicone oil is 20-500 cSt.

[0020] In a preferred embodiment, the thermally conductive filler is selected from at least one of diamond, graphite, carbon nanotubes, graphene, aluminum oxide, aluminum nitride, silicon nitride, boron nitride, silicon carbide and zinc oxide.

[0021] In a preferred embodiment, based on the total weight of the thermally conductive filler, the thermally conductive filler with a particle size of 0.1-3 microns accounts for 1-30%, the thermally conductive filler with a particle size of 5-15 microns accounts for 10-40%, and the thermally conductive filler with a particle size of 50-150 microns accounts for 30-70%. Such compounding of the thermally conductive fillers can achieve dense stacking between the powders, greatly optimize the heat transfer path, and further improve the thermal conductivity of the thermally conductive silicone gel.

[0022] In a preferred embodiment, the catalyst is selected from at least one of chloroplatinic acid, platinum-vinylsiloxane complex and platinum-alkyne chelate.

[0023] In a preferred embodiment, the pigment is selected from at least one of carbon black, iron red, cobalt blue and cadmium yellow.

[0024] A second aspect of the present invention provides a method for preparing the thermally conductive silicone gel, the method comprising:

[0025] S1, mixing vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil uniformly to obtain a first mixture;

[0026] S2, uniformly mixing the first mixture obtained in step S1, the thermally conductive filler and the optional pigment to obtain a second mixture;

[0027] S3, stirring and mixing the second mixture obtained in step S2 and the catalyst at 100-120° C. under vacuum conditions to obtain thermally conductive silicone gel. DETAILED DESCRIPTION

[0028] The thermally conductive silicone gel provided by the invention contains vinyl silicone oil, hydrogen-containing silicone oil, alkoxy silicone oil, thermally conductive filler, catalyst and optional pigment. wherein the content of the vinyl silicone oil is 40-70 parts by weight, such as 40, 45, 50, 55, 60, 65, 70 parts by weight; the content of the hydrogen-containing silicone oil is 0.5-3 parts by weight, such as 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3 parts by weight; the content of the alkoxy silicone oil is 0.5-25 parts by weight, such as 0.5, 1, 5, 8, 10, 12, 15, 18, 20, 22, 25 parts by weight, etc.; the content of the thermal conductive filler is 400-2200 parts by weight, such as 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, the content of the catalyst is 1-5 parts by weight, such as 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.5, 4, 4.5, 5 parts by weight; the content of the pigment is 0-7 parts by weight, such as 0, 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.5, 4, 4.5, 5 parts by weight.

[0029] The alkoxy silicone oil has a structure shown in formula (I):

[0030]

[0031] In formula (I), R 11 , R 12 and R 13 Each independently for OC a H 2a+1 alkoxy, a is an integer from 0 to 16, that is, R 11 , R 12 and R 13 Each independently is H or C1-C 16 Alkoxy; R 14 and R 15 Each independently is C b H 2b+1 alkyl, b is an integer from 0 to 16, that is, R 14 and R 15 Each independently is H or C1-C 16 Alkyl; R 16 , R 17 and R 18 Each independently selected from OC a' H 2a'+1or all selected from C b' H 2b'+1 alkyl, a' is an integer from 0 to 16, b' is an integer from 0 to 16, that is, R 16 , R 17 and R 18 Each independently is C1-C 16 An alkyl group (in this case, one end of the alkoxy silicone oil is a trialkoxy group and the other end is an alkyl group), or a C1-C 16 Alkoxy groups (in this case, both ends of the alkoxy silicone oil are trialkoxy groups), or R 16 , R 17 and R 18 Any two of them are independently OC a" H 2a"+1 Alkoxy or C b" H 2b"+1 The remaining one is vinyl, a" is an integer from 0 to 16, b" is an integer from 0 to 16, that is, R 16 , R 17 and R 18 Any two of them are independently H, C1-C 16 Alkyl or C1-C 16 The remaining one is a vinyl group (in this case, one end of the alkoxy silicone oil is a trialkoxy group and the other end is a vinyl group); n is an integer of 4-50. 16 Specific examples of the alkoxy group of include, but are not limited to, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentoxy, isopentoxy, neopentoxy, hexoxy, heptoxy, octoxy, nonyloxy, heptoxy, undecyloxy, dodecyloxy, tridecyloxy, tetradecyloxy, pentadecyloxy or hexadecyloxy, preferably methoxy, ethoxy, isopropoxy or n-butoxy. 16 Specific examples of the alkyl group include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decanyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl or hexadecyl, preferably methyl, ethyl, isopropyl or n-butyl. It should be noted that n R on the same molecular chain 14 And n R 15 It can be the same or different.

[0032] In a preferred embodiment, in formula (I), R 11 , R 12 and R 13 Each independently for OC a H 2a+1alkoxy, a is an integer from 1 to 16, that is, R 11 , R 12 and R 13 Each independently is C1-C 16 Alkoxy; R 14 and R 15 Each independently is C b H 2b+1 alkyl, b is an integer from 1 to 16, that is, R 14 and R 15 Each independently is C1-C 16 Alkyl; R 16 , R 17 and R 18 Any two of them are independently C b" H 2b"+1 The remaining one is vinyl, b" is an integer from 1 to 16, that is, R 16 , R 17 and R 18 Any two of them are independently C1-C 16 An alkyl group is present and the remaining one is a vinyl group, and n is an integer of 4-50, so that one end of the corresponding alkoxy silicone oil is a trialkoxy group and the other end is a vinyl group. At this time, the thermal conductive silicone gel has a higher thermal conductivity and better high temperature aging resistance.

[0033] In addition, the viscosity of the alkoxy silicone oil is preferably 20-500 cSt. In the present invention, the viscosity is the viscosity corresponding to 25°C.

[0034] The present invention has no particular limitation on the type of vinyl silicone oil, and the vinyl silicone oil may be at least one of vinyl terminated polydimethylsiloxane, vinyl terminated polydimethylsiloxane in which the methyl groups of the main chain are partially substituted by long-chain alkyl groups, methyl terminated polysiloxane containing vinyl groups in the side chains, and methyl terminated polysiloxane containing vinyl groups in the side chains and methyl groups in the main chain are partially substituted by long-chain alkyl groups. In a preferred embodiment, the vinyl silicone oil has a structure shown in formula (II):

[0035]

[0036] In formula (II), R 21 For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 Each independently is C1-C 16wherein m is an integer of 0-1000 (in this case, the terminal group of the vinyl silicone oil contains a vinyl group), preferably, m is an integer of 1-500; or, m R 24 At least one of them is vinyl and the remaining R 24 C1-C 16 The alkyl group, R 21 , R 22 , R 23 , R 25 , R 26 , R 27 and R 28 Each independently is C1-C 16 wherein m is an integer of 0-1000 (in this case, the side chain of the vinyl silicone oil contains a vinyl group), and preferably, m is an integer of 1-500. The vinyl content in the vinyl silicone oil is preferably 0.2-0.8 mmoles / g. In addition, the viscosity of the vinyl silicone oil is preferably 30-500 cSt.

[0037] The hydrogen-containing silicone oil is used as a cross-linking agent, which can be a terminal hydrogen-containing silicone oil, a side hydrogen-containing silicone oil, or a both terminal and side hydrogen-containing silicone oil. In a preferred embodiment, the hydrogen-containing silicone oil is composed of a terminal hydrogen-containing silicone oil represented by formula (III) and a side hydrogen-containing silicone oil represented by formula (IV);

[0038]

[0039] In formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 Each independently is C1-C 16 alkyl, p is an integer of 0-1000, preferably, p is an integer of 1-300; in formula (IV), R 41 and R 45 Each independently represents H or a C1-C5 alkyl group, R 42 , R 43 , R 44 , R 46 and R 47Each independently is an alkyl group of C1-C5, q is an integer of 0-1000, preferably, q is an integer of 1-300. More preferably, the mass ratio of the end hydrogen-containing silicone oil and the side hydrogen-containing silicone oil is (1-10):1, such as 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 and any value therebetween. Wherein, the end hydrogen-containing silicone oil is used for chain extension, and the side hydrogen-containing silicone oil is used for cross-linking. Compounding according to the above preferred embodiments can significantly improve the bulk strength and toughness of the thermally conductive silicone gel. The content of Si-H in the end hydrogen-containing silicone oil is preferably 0.2-0.6 mmoles / g. The content of Si-H in the side hydrogen-containing silicone oil is preferably 0.5-0.8 mmoles / g. In addition, the viscosity of the hydrogen-containing silicone oil is preferably 40-200 cSt.

[0040] The present invention does not particularly limit the type of thermally conductive filler, which can be a conventional choice in the art, for example, it can be selected from at least one of diamond, graphite, carbon nanotubes, graphene, aluminum oxide, aluminum nitride, silicon nitride, boron nitride, silicon carbide and zinc oxide. The particle size of the thermally conductive filler is preferably 0.1-150 microns, and can be spherical or quasi-spherical. In a preferred embodiment, based on the total weight of the thermally conductive filler, the proportion of thermally conductive fillers with a particle size of 0.1-3 microns is 1-30%, the proportion of thermally conductive fillers with a particle size of 5-15 microns is 10-40%, and the proportion of thermally conductive fillers with a particle size of 50-150 microns is 30-70%. The use of such a compound of thermally conductive fillers can achieve dense stacking between the powders, greatly optimize the heat transfer path, and thus be more conducive to the improvement of the thermal conductivity of the thermally conductive silicone gel.

[0041] The catalyst can be any common catalyst for addition-type liquid silicone rubber, such as chloroplatinic acid, platinum-vinylsiloxane complex, platinum-alkyne chelate, etc. The specific types of the platinum-vinylsiloxane complex and platinum-alkyne chelate are well known to those skilled in the art and will not be described in detail herein.

[0042] The present invention has no particular limitation on the type of pigment, which can be reasonably selected according to the actual color required. Specific examples include, but are not limited to, at least one of carbon black, iron red, cobalt blue and cadmium yellow.

[0043] The second aspect of the present invention provides a method for preparing the thermally conductive silicone gel, which comprises: S1, mixing vinyl silicone oil, hydrogenated silicone oil and alkoxy silicone oil evenly to obtain a first mixture; S2, mixing the first mixture obtained in step S1, a thermally conductive filler and an optional pigment evenly to obtain a second mixture; S3, stirring and mixing the second mixture obtained in step S2 and a catalyst evenly under vacuum conditions at 100-120°C to obtain a thermally conductive silicone gel. The mixing of the three steps can be carried out in various existing mixing equipment, preferably in a planetary mixer. The mixing conditions of the three steps are based on uniform dispersion of the components. In addition, the mixing in step S1 is generally carried out at room temperature, and the mixing in step S2 is generally carried out at 40-80°C.

[0044] The present invention will be described in detail below through examples.

[0045] Example 1 This example is used to illustrate the thermal conductive silicone gel and its preparation method

[0046] (1) Raw materials: The components of the thermally conductive silicone gel are measured by weight and contain 50 parts of vinyl silicone oil, 2 parts of hydrogenated silicone oil, 15 parts of alkoxy silicone oil, 2200 parts of thermally conductive filler, 4 parts of catalyst, and 5 parts of pigment.

[0047] The vinyl silicone oil is a vinyl-terminated polydimethylsiloxane having a structure shown in formula (II), wherein R 21 For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 All are methyl, the vinyl content is 0.37mmoles / g, and the viscosity is 100cSt.

[0048] The hydrogen-containing silicone oil is 1.5 parts of terminal hydrogen-containing polydimethylsiloxane and 0.5 parts of side hydrogen-containing polydimethylsiloxane. The terminal hydrogen-containing polydimethylsiloxane has a structure shown in formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 The side hydrogen-containing polydimethylsiloxane has the structure shown in formula (IV), R 41 , R 42 , R 43 , R 44 , R 45 , R 46 and R 47All of them are methyl, with a Si-H content of 0.75 mmoles / g and a viscosity of 45 cSt.

[0049] The alkoxy silicone oil is a long-chain silicone oil with trimethoxy groups at both ends, purchased from Ambiya Company, with the brand name Andisil SF 191-109, and has the structure shown in formula (I), R 11 , R 12 , R 13 , R 16 , R 17 and R 18 All are methoxy, R 14 and R 15 All are methyl, n is an integer of 4-50, and the viscosity is 100 cSt.

[0050] The high thermal conductivity filler is aluminum nitride, which is spherical thermal conductive particles with a particle size of 0.1-120 microns, of which particles with a particle size of 70-120 microns account for 60% of the total, particles with a particle size of 5-15 microns account for 20% of the total, and particles with a particle size of 0.1-3 microns account for 20% of the total.

[0051] The catalyst is chloroplatinic acid.

[0052] The pigment is iron red.

[0053] (2) Preparation process:

[0054] S1: Weigh vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil according to the proportion and add them into a planetary mixer, stir at room temperature for 1.5 hours, and mix them evenly for use;

[0055] S2: Weigh the corresponding thermal conductive fillers and pigments and add them into the planetary mixer with uniform stirring. Evacuate at 60°C and -0.1MPa, and stir at 100rpm for 2h.

[0056] S3: Weigh the corresponding catalyst and add it to the above-mentioned planetary mixer with uniform stirring, evacuate the temperature to 100°C and stir for 2 hours, then cool to room temperature, and put the mixed single-component gel into a 30CC single-component tube to obtain a thermally conductive silicone gel.

[0057] Example 2 This example is used to illustrate the thermal conductive silicone gel and its preparation method

[0058] (1) Raw materials: The components of the thermally conductive silicone gel are measured by weight and contain 40 parts of vinyl silicone oil, 0.5 parts of hydrogenated silicone oil, 5 parts of alkoxy silicone oil, 400 parts of thermally conductive filler, 1 part of catalyst, and 1 part of pigment.

[0059] The vinyl silicone oil is a vinyl-terminated polydimethylsiloxane having a structure shown in formula (II), wherein R 21For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 All are methyl, the vinyl content is 0.37mmoles / g, and the viscosity is 100cSt.

[0060] The hydrogen-containing silicone oil is 1 part of terminal hydrogen-containing polydimethylsiloxane and 1 part of side hydrogen-containing polydimethylsiloxane. The terminal hydrogen-containing polydimethylsiloxane has a structure shown in formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 The side hydrogen-containing polydimethylsiloxane has the structure shown in formula (IV), R 41 , R 42 , R 43 , R 44 , R 45 , R 46 and R 47 All of them are methyl, with a Si-H content of 0.75 mmoles / g and a viscosity of 45 cSt.

[0061] The alkoxy silicone oil is a long-chain silicone oil with trimethoxy groups at both ends, purchased from Ambiya Company, with the brand name Andisil SF 191-109, and has the structure shown in formula (I), R 11 , R 12 , R 13 , R 16 , R 17 and R 18 All are methoxy, R 14 and R 15 All are methyl, n is an integer of 4-50, and the viscosity is 100 cSt.

[0062] The high thermal conductive filler is aluminum oxide, which is a spherical thermal conductive particle with a particle size of 0.1-120 microns, of which particles with a particle size of 70-120 microns account for 60% of the total, particles with a particle size of 5-15 microns account for 20% of the total, and particles with a particle size of 0.1-3 microns account for 20% of the total.

[0063] The catalyst is chloroplatinic acid.

[0064] The pigment is cadmium yellow.

[0065] (2) Preparation process:

[0066] S1: Weigh vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil according to the proportion and add them into a planetary mixer, stir at room temperature for 1.5 hours, and mix them evenly for use;

[0067] S2: Weigh the corresponding thermal conductive fillers and pigments and add them into the planetary mixer with uniform stirring. Evacuate at 60°C and -0.1MPa, and stir at 100rpm for 2h.

[0068] S3: Weigh the corresponding catalyst and add it into the above-mentioned planetary mixer with uniform stirring, evacuate and heat to 120°C and stir for 1 hour, then cool to room temperature, and put the mixed single-component gel into a 30CC single-component tube to obtain thermal conductive silicone gel.

[0069] Example 3 This example is used to illustrate the thermal conductive silicone gel and its preparation method

[0070] (1) Raw materials: The components of the thermally conductive silicone gel are measured by weight and contain 70 parts of vinyl silicone oil, 3 parts of hydrogenated silicone oil, 25 parts of alkoxy silicone oil, 1500 parts of thermally conductive filler, 5 parts of catalyst, and 7 parts of pigment.

[0071] The vinyl silicone oil is a vinyl-terminated polydimethylsiloxane having a structure shown in formula (II), wherein R 21 For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 All are methyl, the vinyl content is 0.76mmoles / g, and the viscosity is 50cSt.

[0072] The hydrogen-containing silicone oil is 1 part of terminal hydrogen-containing polydimethylsiloxane and 1 part of side hydrogen-containing polydimethylsiloxane. The terminal hydrogen-containing polydimethylsiloxane has a structure shown in formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 The side hydrogen-containing polydimethylsiloxane has the structure shown in formula (IV), R 41 , R 42 , R 43 , R 44 , R 45 , R 46 and R 47 All of them are methyl, with a Si-H content of 0.75 mmoles / g and a viscosity of 45 cSt.

[0073] The alkoxy silicone oil is a long-chain silicone oil with trimethoxy groups at both ends, purchased from Ambiya Company, with the brand name Andisil SF 191-109, and has the structure shown in formula (I), R 11 , R 12 , R 13 , R 16 , R 17 and R 18 All are methoxy, R 14 and R 15 All are methyl, n is an integer of 4-50, and the viscosity is 100 cSt.

[0074] The high thermal conductive filler is a composite of aluminum nitride and aluminum oxide in a mass ratio of 1:1, and is a spherical thermal conductive particle with a particle size of 0.1-120 microns, of which particles with a particle size of 70-120 microns account for 60% of the total, particles with a particle size of 5-15 microns account for 20% of the total, and particles with a particle size of 0.1-3 microns account for 20% of the total.

[0075] The catalyst is platinum-vinylsiloxane.

[0076] The pigment is cobalt blue.

[0077] (2) Preparation process:

[0078] S1: Weigh vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil according to the proportion and add them into a planetary mixer, stir at room temperature for 1.5 hours, and mix them evenly for use;

[0079] S2: Weigh the corresponding thermal conductive fillers and pigments and add them into the planetary mixer with uniform stirring. Evacuate at 60°C and -0.1MPa, and stir at 100rpm for 2h.

[0080] S3: Weigh the corresponding catalyst and add it to the above-mentioned planetary mixer with uniform stirring, evacuate the temperature to 100°C and stir for 2 hours, then cool to room temperature, and put the mixed single-component gel into a 30CC single-component tube to obtain a thermally conductive silicone gel.

[0081] Example 4 This example is used to illustrate the thermal conductive silicone gel and its preparation method

[0082] (1) Raw materials: The components of the thermally conductive silicone gel are measured by weight and contain 50 parts of vinyl silicone oil, 2 parts of hydrogenated silicone oil, 15 parts of alkoxy silicone oil, 2200 parts of thermally conductive filler, 4 parts of catalyst, and 5 parts of pigment.

[0083] The vinyl silicone oil is a vinyl-terminated polydimethylsiloxane having a structure shown in formula (II), wherein R 21 For vinyl, R 22, R 23 , R 24 , R 25 , R 26 , R 27 and R 28 All are methyl, the vinyl content is 0.76mmoles / g, and the viscosity is 50cSt.

[0084] The hydrogen-containing silicone oil is 0.5 parts of terminal hydrogen-containing polydimethylsiloxane and 1.5 parts of side hydrogen-containing polydimethylsiloxane. The terminal hydrogen-containing polydimethylsiloxane has a structure shown in formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 The side hydrogen-containing polydimethylsiloxane has the structure shown in formula (IV), R 41 , R 42 , R 43 , R 44 , R 45 , R 46 and R 47 All of them are methyl, with a Si-H content of 0.75 mmoles / g and a viscosity of 45 cSt.

[0085] The alkoxy silicone oil is a long-chain silicone oil with trimethoxy groups at both ends, purchased from Ambiya Company, with the brand name Andisil SF 191-109, and has the structure shown in formula (I), R 11 , R 12 , R 13 , R 16 , R 17 and R 18 All are methoxy, R 14 and R 15 All are methyl, n is an integer of 4-50, and the viscosity is 100 cSt.

[0086] The high thermal conductive filler is silicon carbide, which is a spherical thermal conductive particle with a particle size of 0.1-120 microns, of which particles with a particle size of 70-120 microns account for 70% of the total, particles with a particle size of 5-15 microns account for 20% of the total, and particles with a particle size of 0.1-3 microns account for 10% of the total.

[0087] The catalyst is platinum-vinylsiloxane.

[0088] The pigment is carbon black.

[0089] (2) Preparation process:

[0090] S1: Weigh vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil according to the proportion and add them into a planetary mixer, stir at room temperature for 1.5 hours, and mix them evenly for use;

[0091] S2: Weigh the corresponding thermal conductive fillers and pigments and add them into the planetary mixer with uniform stirring. Evacuate at 60°C and -0.1MPa, and stir at 100rpm for 2h.

[0092] S3: Weigh the corresponding catalyst and add it to the above-mentioned planetary mixer with uniform stirring, evacuate the temperature to 100°C and stir for 2 hours, then cool to room temperature, and put the mixed single-component gel into a 30CC single-component tube to obtain a thermally conductive silicone gel.

[0093] Example 5

[0094] Thermally conductive silicone gel was prepared according to the method of Example 1, except that the alkoxy silicone oil was replaced by a long-chain silicone oil having a triethoxy end-capped at one end and a vinyl end-capped at the other end, purchased from Gelest Company, with the brand name GEL-MCR-XT11, having the structure shown in formula (I), R 11 , R 12 and R 13 All are ethoxy, R 17 and R 18 All are methyl, R 16 is vinyl, n is an integer of 4-50, the viscosity is 24 cSt, and the other conditions are the same as those in Example 1 to obtain a thermally conductive silicone gel.

[0095] Example 6

[0096] Thermally conductive silicone gel was prepared according to the method of Example 1, except that in the hydrogen-containing silicone oil, the side hydrogen-containing polydimethylsiloxane was replaced by the same weight portion of terminal hydrogen-containing polydimethylsiloxane, and the other conditions were the same as those of Example 1 to obtain thermally conductive silicone gel.

[0097] Example 7

[0098] Thermally conductive silicone gel was prepared according to the method of Example 1, except that the particle sizes of the thermally conductive fillers were all controlled to be 70-120 μm. The other conditions were the same as those of Example 1, to obtain thermally conductive silicone gel.

[0099] Comparative Example 1

[0100] The thermal conductive silicone gel was prepared according to the method of Example 6, except that the alkoxy silicone oil was replaced by the same weight portion of hydrogen-containing silicone oil (terminated hydrogen-containing polydimethylsiloxane having the structure shown in formula (III), R 31 , R 32 , R 33 , R 34 , R35 and R 36 All of them are methyl, wherein the Si-H content is 0.4 mmoles / g, and the viscosity is 100 cSt), and the other conditions are the same as those in Example 1 to obtain a reference thermal conductive silicone gel.

[0101] Comparative Example 2

[0102] The thermal conductive silicone gel was prepared according to the method of Example 6, except that the alkoxy silicone oil was replaced by the same weight portion of the terminal hydroxyl silicone oil (purchased from Ambiya Company, brand DA30, having the structure shown in formula (I), R 11 and R 16 All are hydroxyl groups, R 12 , R 13 , R 14 , R 15 , R 17 and R 18 The remaining conditions were the same as those in Example 1 to obtain a reference thermally conductive silicone gel.

[0103] Comparative Example 3

[0104] A thermally conductive silicone gel was prepared according to the method of Example 6, except that the alkoxy silicone oil was replaced by the same weight portion of hexadecyltrimethoxysilane, and the other conditions were the same as those of Example 1, to obtain a reference thermally conductive silicone gel.

[0105] Test Case

[0106] (1) Thermal conductivity: The thermal conductivity of the thermally conductive silicone gel obtained in each embodiment and comparative example was tested according to the method of ASTM-D547. The results are shown in Table 1.

[0107] (2) 150℃ aging cracking: The test was conducted using a high temperature oven observation method. The results are shown in Table 1.

[0108] (3) The first initial thermal resistance at room temperature (25°C) and the thermal resistance after 1000 hours of cycling at 125°C: The test was conducted using the ASTM-D5470 method. The results are shown in Table 1.

[0109] (4) The second initial thermal resistance at room temperature (25°C) and the thermal resistance after repeated hot and cold cycles from -40°C to 125°C for 1000 hours: The test was conducted using the ASTM-D5470 method. The results are shown in Table 1.

[0110] (5) The third initial thermal resistance at room temperature (25° C.) and the thermal resistance after 1000 hours of cycling at 85° C. and 85% humidity: The test was conducted using the ASTM-D5470 method. The results are shown in Table 1.

[0111]

[0112] It can be seen from the results in Table 1 that, compared with similar products currently available on the market, the thermally conductive silicone gel provided by the present invention has the advantages of higher thermal conductivity, better extrusion performance, higher temperature resistance, and almost unchanged thermal resistance under various aging conditions for 1000 hours, thereby ensuring that it always maintains a high working efficiency during long-term high-power heat dissipation and has good reliability.

[0113] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. A thermally conductive silicone gel, characterized in that the thermally conductive silicone gel contains 40-70 parts by weight of vinyl silicone oil, 0.5-3 parts by weight of hydrogenated silicone oil, 0.5-25 parts by weight of alkoxy silicone oil, 400-2200 parts by weight of thermally conductive filler, 1-5 parts by weight of catalyst and 0-7 parts by weight of optional pigment, wherein the alkoxy silicone oil has a structure shown in formula (I): Formula (I) In formula (I), R 11 , R 12 and R 13 Each independently for OC a H 2a+1 an alkoxy group, a is an integer of 1 to 16; R 14 and R 15 Each independently is C b H 2b+1 alkyl, b is an integer of 1-16; R 16 , R 17 and R 18 Any two of them are independently C b" H 2b"+1 The remaining one is vinyl, b" is an integer from 1 to 16; n is an integer from 4 to 50; The hydrogen-containing silicone oil is composed of terminal hydrogen-containing silicone oil represented by formula (III) and side hydrogen-containing silicone oil represented by formula (IV); Formula (III), Formula (IV), In formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 Each independently is C1-C 16 An alkyl group, p is an integer from 1 to 1000; In formula (IV), R 41 and R 45 Each independently represents H or a C1-C5 alkyl group, R 42 , R 43 , R 44 , R 46 and R 47 Each is independently a C1-C5 alkyl group, and q is an integer from 1 to 1000; The viscosity of the hydrogen-containing silicone oil is 40-200 cSt; The mass ratio of the end hydrogen-containing silicone oil to the side hydrogen-containing silicone oil is (2-10):1; The content of Si-H in the terminal hydrogen-containing silicone oil is 0.2-0.6 mmoles / g; the content of Si-H in the side hydrogen-containing silicone oil is 0.5-0.8 mmoles / g; The vinyl silicone oil has a structure shown in formula (II): Formula (II) In formula (II), R 21 For vinyl, R 22 , R 23 , R 24 , R 25 , R 26 , R 27 and R 28 Each independently is C1-C 16 An alkyl group, m is an integer from 1 to 1000; The vinyl content of the vinyl silicone oil is 0.2-0.8 mmoles / g; The viscosity of the vinyl silicone oil is 30-500 cSt.

2. The thermally conductive silicone gel according to claim 1, wherein the viscosity of the alkoxy silicone oil is 20-500 cSt.

3. The thermally conductive silicone gel according to claim 1 or 2, wherein the thermally conductive filler is selected from at least one of diamond, graphite, carbon nanotubes, graphene, aluminum oxide, aluminum nitride, silicon nitride, boron nitride, silicon carbide and zinc oxide.

4. The thermally conductive silicone gel according to claim 3 is characterized in that, based on the total weight of the thermally conductive filler, the thermally conductive filler with a particle size of 0.1-3 microns accounts for 1-30%, the thermally conductive filler with a particle size of 5-15 microns accounts for 10-40%, and the thermally conductive filler with a particle size of 50-150 microns accounts for 30-70%.

5. The thermally conductive silicone gel according to claim 1 or 2, wherein the catalyst is selected from at least one of chloroplatinic acid, platinum-vinylsiloxane complex and platinum-alkyne chelate.

6. The thermally conductive silicone gel according to claim 1 or 2, wherein the pigment is selected from at least one of carbon black, iron red, cobalt blue and cadmium yellow.

7. The method for preparing the thermally conductive silicone gel according to any one of claims 1 to 6, wherein the method comprises the following steps: S1, mixing vinyl silicone oil, hydrogen silicone oil and alkoxy silicone oil uniformly to obtain a first mixture; S2, uniformly mixing the first mixture obtained in step S1, the thermally conductive filler and the optional pigment to obtain a second mixture; S3, stirring and mixing the second mixture obtained in step S2 and the catalyst at 100-120° C. under vacuum conditions to obtain thermally conductive silicone gel.