A nickel niobate negative electrode material and its preparation method and application

The nickel niobate negative electrode material was prepared by molten salt method, combining carbon black and polyvinylidene fluoride, which solved the problem of poor dynamics of traditional graphite-based materials in lithium-ion batteries, and achieved rapid charging and discharge and high cycle stability of lithium-ion batteries Suitable for large-scale applications.

CN114975987BActive Publication Date: 2024-11-19WUHAN UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210808311.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-11-19
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

Traditional graphite-based anode materials have poor kinetics during charging and discharging in lithium-ion batteries, which are prone to lithium dendrites. They have safety problems under high current density, making it difficult to achieve fast charging and discharging, high energy density and high cycle stability.

Method used

The nickel niobate negative electrode material is prepared by molten salt method. By mixing the compounds of niobium and nickel with inorganic salts, adding ethanol solution for wet mixing and heating, forming nickel niobate, used for lithium-ion battery negative electrode, combining carbon black and polydefluoride Ethylene is assembled as a conductive agent and a binder.

Benefits of technology

It achieves excellent rate performance and cycle stability of nickel niobate in lithium-ion batteries, reduces reaction temperature and particle size, shortens the diffusion path of lithium ions, improves the diffusion rate, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003738198700000011
    Figure HDA0003738198700000011
  • Figure HDA0003738198700000012
    Figure HDA0003738198700000012
  • Figure HDA0003738198700000021
    Figure HDA0003738198700000021
Patent Text Reader

Abstract

The present invention provides a nickel niobate negative electrode material and a preparation method and application thereof. The preparation method comprises the following steps: mixing a niobium compound and a nickel compound, and adding an inorganic salt to obtain a mixture; adding an appropriate amount of ethanol solution to the mixture to completely infiltrate it and wet mix it, and drying it; grinding the dried product into a powder, putting it into a muffle furnace, heating it to 600-1200°C, keeping it warm for 0.5 to 20 hours, and then cooling it; washing and filtering the cooled product, and drying it to obtain the nickel niobate negative electrode material. The present invention adopts a molten salt method to prepare nickel niobate, and the method can successfully prepare nickel niobate below 1000°C, and the prepared nickel niobate has a high capacity, excellent rate performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a nickel niobate negative electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion (LIBs) batteries have become one of the most attractive energy storage technologies due to their light weight, small size, high operating voltage, low self-discharge rate and long cycle life. With the increasing application of electric vehicles, portable consumer electronics and energy storage systems, the demand for LIBs has also increased. As one of the key performances of the new generation of lithium-ion batteries, fast charge / discharge capability has received increasing attention and attention worldwide. The fast charge and discharge performance of lithium-ion batteries depends on the electrochemical reaction kinetics and electron ion transport characteristics inside the battery. The electrode active materials and their properties, as the core of energy storage, determine the overall performance of lithium-ion batteries. Traditional graphite-based anode materials have poor bulk lithium insertion kinetics, are very easy to form lithium dendrites during the charge and discharge process, and have a series of safety issues at high current density. Therefore, the development of new anode materials with fast charge and discharge rates, high energy density, high cycle stability and high safety is the key to further improve the performance of lithium-ion batteries, and is of great significance to promote the development of electric vehicles, hybrid vehicles and high-power energy storage devices. Summary of the invention

[0003] The present invention provides a nickel niobate negative electrode material and a preparation method and application thereof to solve the above technical problems. The present invention adopts a molten salt method to prepare nickel niobate, which can successfully prepare nickel niobate at below 1000°C. The prepared nickel niobate has a high capacity, excellent rate performance and cycle performance.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for preparing a nickel niobate negative electrode material, the preparation method comprising the following steps:

[0006] mixing a niobium compound and a nickel compound, and adding an inorganic salt to obtain a mixture;

[0007] Adding an appropriate amount of ethanol solution to the mixture to completely soak it and wet mix it, and then drying it;

[0008] The dried product is ground into powder, placed in a muffle furnace, heated to 600-1200°C, kept warm for 0.5-20h, and then cooled;

[0009] The cooled product is washed, filtered, and dried to obtain the nickel niobate negative electrode material.

[0010] Preferably, the drying temperature is 60 to 150° C. The drying time after wet mixing is 12 to 24 hours.

[0011] Preferably, the heating rate to 600-1200° C. is 0.5-20° C. / min.

[0012] Preferably, the niobium compound is one or a mixture of two or more of niobium oxide, niobium carbonate, niobium hydroxide, niobium chloride, niobium nitrate or niobium sulfate; the nickel compound is one or a mixture of two or more of nickel oxide, nickel carbonate, nickel hydroxide, nickel chloride, nickel nitrate or nickel sulfate.

[0013] Preferably, the niobium compound and the nickel compound are mixed in a molar ratio of 0.5-18.

[0014] Preferably, the inorganic salt is a mixture of two or more of alkali metal chlorides or fluorides and nickel chloride, and the nickel chloride accounts for 3 to 15 mol% of the total amount of the inorganic salt.

[0015] Preferably, the mass ratio of the inorganic salt to the total amount of the niobium compound and the nickel compound is 5:1-1:20.

[0016] Preferably, the wet mixing time is 2 to 24 hours.

[0017] Preferably, the heating rate is 0.5-20°C / min.

[0018] The nickel niobate negative electrode material obtained by the preparation method.

[0019] Preferably, the nickel niobate is Ni2Nb 34 O 67 , single phase or mixed phase of NiNb2O6, Ni2Nb2O7, Ni4Nb2O9.

[0020] Application of the nickel niobate negative electrode material in lithium ion batteries.

[0021] The present invention also provides a method for preparing a negative electrode for a lithium electronic battery: nickel niobate, carbon black (conductive agent) and polyvinylidene fluoride (PVDF, binder) in a mass percentage of (70-85): (5-10): (10-20) are mixed and ground, NMP is added to prepare a uniform slurry, and the slurry is uniformly coated on a copper foil to obtain a negative electrode for a lithium ion battery.

[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention adopts the molten salt method to select a variety of niobium and nickel raw materials, the preparation process is simple, and it is convenient for large-scale application. Compared with the solid phase method, the reaction temperature can be effectively reduced, the reaction uniformity is improved, the product particle size is small, which is conducive to shortening the diffusion path of lithium ions and increasing the diffusion rate of lithium ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD diagram of nickel niobate, the negative electrode material for lithium-ion batteries prepared in Example 1.

[0024] Figure 2 This is a SEM image of nickel niobate, a negative electrode material for a lithium-ion battery prepared in Example 1.

[0025] Figure 3 This is the XRD diagram of nickel niobate, the negative electrode material for lithium-ion batteries prepared in Example 2.

[0026] Figure 4 This is a SEM image of nickel niobate, a negative electrode material for a lithium-ion battery prepared in Example 2.

[0027] Figure 5 This is the rate performance of nickel niobate, the negative electrode material for lithium-ion batteries prepared in Example 1.

[0028] Figure 6 The cycle performance of nickel niobate, a negative electrode material for lithium-ion batteries prepared in Example 1, at 1C.

[0029] Figure 7 This is the XRD diagram of nickel niobate, the negative electrode material for lithium-ion batteries prepared in Example 3.

[0030] Figure 8 This is the rate performance of nickel niobate, the negative electrode material for lithium-ion batteries prepared in Example 3.

[0031] Fig. 9 This is the cycling performance of nickel niobate, a negative electrode material for lithium-ion batteries prepared in Example 3, at 1C. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] Example 1

[0034] Preparation of nickel niobate (NiNb2O6) material:

[0035] Nb2O5 and Ni(OH)2 are mixed at a Nb / Ni molar ratio of 2:1, and inorganic salts KCl, NaCl and NiCl2 (molar percentages of 45%, 45% and 10%, respectively) are added as molten salt reaction media, and metal oxides and inorganic salts are mixed at a mass ratio of 1:5; an appropriate amount of ethanol solution is added to the above mixture to make it completely infiltrated and wet mixed for 4 hours, and then placed in an 80℃ oven for drying for 24 hours. The dried product is ground into powder, placed in a corundum crucible, placed in a muffle furnace, heated to 750℃ at a heating rate of 10℃ / min, kept warm for 5 hours, and then cooled to room temperature. The product in the crucible is then washed and filtered with deionized water for multiple times, and after drying at 80℃, nickel niobate (NiNb2O6 single phase) material is obtained. Figure 1 is the XRD pattern of nickel niobate, a negative electrode material for lithium-ion batteries, obtained in Example 1. Figure 1 It can be seen that according to the scheme of Example 1, pure phase NiNb2O6 can be prepared.

[0036] For comparison, a reaction without adding NiCl2 in the molten salt medium was also carried out, that is, KCl and NaCl were used as the medium (molar percentage content was 50% respectively), and other reaction raw materials, reaction conditions and treatment process remained unchanged. Figure 1 It can also be seen that under the same conditions, if NiCl2 is not added to the molten salt medium, the reaction will be incomplete, and there is an obvious diffraction peak of Nb2O5 in the figure. This shows that the addition of a small amount of NiCl2 can promote the reaction of generating nickel niobate and avoid the formation of Nb2O5 residues and other niobate impurities.

[0037] Figure 2 is a SEM image of nickel niobate, a negative electrode material for lithium-ion batteries, prepared in Example 1. Figure 2 It can be seen that according to the scheme of Example 1, the NiNb2O6 particles prepared are flaky and small in size, basically within 500nm.

[0038] Assembling batteries using the prepared nickel niobate:

[0039] The synthesized sample (active material), carbon black (conductive agent) and PVDF (binder) were mixed in a mass ratio of 7:2:1, zirconium beads were added for ball milling, NMP was used to adjust the viscosity, and then evenly coated on the copper foil and placed in a vacuum drying oven at 40°C for 12 hours. The copper foil was then cut into electrode discs with a diameter of 12 mm and used as the negative electrode. Metal lithium sheets were used as counter electrodes, and Celgard 2325 polypropylene porous membranes were used as diaphragms. CR2016 button-type lithium-ion batteries were assembled in a glove box protected by high-purity argon. The assembled battery was left to stand at room temperature for 24 hours before its electrochemical performance was tested. Battery test parameters: In the voltage window of 0.005 to 3V, its rate performance was tested: during the charge and discharge cycle, at different current densities of 0.5, 1, 2, 5, 10, 20, 50C (1C = 236mAh g -1 ) were cycled 10 times, and the battery was finally restored to 1C rate. The cycle performance test is to charge and discharge the battery at a fixed current density (1C, 10C). The charge and discharge test temperature of all batteries was carried out in a 25℃ constant temperature box.

[0040] Figure 5 is the rate performance of the lithium ion battery negative electrode material nickel niobate prepared in Example 1. Figure 5 It can be seen that the nickel niobate prepared according to the scheme of Example 1 exhibits excellent rate performance, with a capacity of 300 mAh g at 1C. -1 The specific capacity at 5C is greater than 200mAh g -1 , after being tested at different rates, it recovered to 1C, and its specific capacity remained at a level comparable to the initial capacity.

[0041] Figure 6 The cycle performance of the lithium-ion battery negative electrode material nickel niobate prepared in Example 1 at 1C. Figure 6 It can be seen that the nickel niobate prepared according to the scheme of Example 1 exhibits excellent cycle stability, and can still maintain ~330 mAh g after 250 cycles at 1C. -1 Specific capacity.

[0042] Example 2

[0043] Preparation of nickel niobate (NiNb2O6) material:

[0044] Nb2O5 and NiO are mixed at a Nb / Ni molar ratio of 2:1, and KCl, NaCl and NiCl2 (molar percentages of 46%, 46% and 8% respectively) are added as molten salt reaction media, and metal oxides and inorganic salts are mixed at a mass ratio of 1:3; an appropriate amount of ethanol solution is added to the above mixture to make it completely infiltrated and wet mixed for 4 hours, and then placed in an 80℃ oven for drying for 24 hours. The dried product is ground into powder, placed in a corundum crucible, placed in a muffle furnace, heated to 950℃ at a heating rate of 10℃ / min, kept warm for 5 hours, and then cooled to room temperature. The product in the crucible is then washed and filtered with deionized water for multiple times, and after drying at 80℃, nickel niobate (NiNb2O6 single phase) material is obtained.

[0045] Figure 3 is the XRD pattern of nickel niobate, a negative electrode material for lithium-ion batteries, prepared in Example 2. Figure 3 It can be seen that according to the scheme of Example 2, pure phase NiNb2O6 can be prepared.

[0046] Figure 4 is a SEM image of nickel niobate, a negative electrode material for lithium-ion batteries, prepared in Example 2. Figure 4 It can be seen that according to the scheme of Example 2, the NiNb2O6 particles prepared are flaky and small in size, basically within 1 μm.

[0047] The prepared nickel niobate (NiNb2O6) is used to assemble the battery:

[0048] The synthesized sample (active material), carbon black (conductive agent) and PVDF (binder) were mixed in a mass ratio of 8:1:1, zirconium beads were added for ball milling, the viscosity was adjusted with NMP, and then evenly coated on copper foil and placed in a vacuum drying oven at 40°C for 12 hours. The copper foil was then cut into electrode discs with a diameter of 12 mm and used as the negative electrode. Metal lithium sheets were used as counter electrodes, and Celgard2325 polypropylene porous membranes were used as diaphragms. CR2016 button-type lithium-ion batteries were assembled in a glove box protected by high-purity argon. The assembled battery was left standing at room temperature for 24 hours before its electrochemical performance was tested.

[0049] Battery test parameters: Test its rate performance in the voltage window of 0.005~3V: During the charge and discharge cycle, test the battery at different current densities of 0.5, 1, 2, 5, 10, 20, 50C (1C = 236mAh g -1 ) were cycled 10 times, and the battery was finally restored to 1C rate. The cycle performance test is to charge and discharge the battery at a fixed current density (1C, 10C). The charge and discharge test temperature of all batteries was carried out in a 25℃ constant temperature box.

[0050] Example 3

[0051] Preparation of nickel niobate (Ni4Nb2O9 and NiNb2O6 mixed phase) material:

[0052] Nb2O5 and Ni(OH)2 are mixed at a Nb / Ni molar ratio of 3:1, and KCl, NaCl and NiCl2 (molar percentages of 45%, 45% and 10%, respectively) are added as molten salt reaction media, and metal oxides and inorganic salts are mixed at a mass ratio of 1:5; an appropriate amount of ethanol solution is added to the above mixture to make it completely infiltrated and wet mixed for 4 hours, and then placed in an 80℃ oven for drying for 24 hours. The dried product is ground into powder, placed in a corundum crucible, placed in a muffle furnace, heated to 950℃ at a heating rate of 10℃ / min, kept warm for 8 hours, and then cooled to room temperature. The product in the crucible is then washed and filtered with deionized water for multiple times, and after drying at 80℃, nickel niobate (Ni4Nb2O9 and NiNb2O6 mixed phase) material is obtained.

[0053] Figure 7 is the XRD pattern of nickel niobate, a negative electrode material for lithium-ion batteries, prepared in Example 3. Figure 7 It can be seen that according to the scheme of Example 3, dual-phase nickel niobate of NiNb2O6 and Ni4N2O9 can be prepared.

[0054] Assembling batteries using the prepared nickel niobate:

[0055] The synthesized sample (active material), carbon black (conductive agent) and PVDF (binder) were mixed in a mass ratio of 7:2:1, zirconium beads were added for ball milling, the viscosity was adjusted with NMP, and then evenly coated on copper foil and placed in a vacuum drying oven at 40°C for 12 hours. The copper foil was then cut into electrode discs with a diameter of 12 mm and used as the negative electrode. A metal lithium sheet was used as the counter electrode, and a Celgard2325 polypropylene porous membrane was used as the diaphragm. A CR2016 button lithium-ion battery was assembled in a glove box protected by high-purity argon. The assembled battery was left standing at room temperature for 24 hours before its electrochemical performance was tested.

[0056] Battery test parameters: Test its rate performance in the voltage window of 0.005~3V: During the charge and discharge cycle, test the battery at different current densities of 0.5, 1, 2, 5, 10, 20, 50C (1C = 236mAh g -1 ) were cycled 10 times, and the battery was finally restored to 1C rate. The cycle performance test is to charge and discharge the battery at a fixed current density (1C, 10C). The charge and discharge test temperature of all batteries was carried out in a 25℃ constant temperature box.

[0057] Figure 8is the rate performance of the lithium ion battery negative electrode material nickel niobate prepared in Example 3. Figure 8 It can be seen that the nickel niobate prepared according to the scheme of Example 3 exhibits excellent rate performance, with a capacity of 300 mAh g at 1C. -1 The specific capacity at 5C is greater than 200mAh g -1 , after being tested at different rates, it recovered to 1C, and its specific capacity remained at a level comparable to the initial capacity.

[0058] Fig. 9 The cycle performance of the lithium-ion battery negative electrode material nickel niobate prepared in Example 3 at 1C. Fig. 9 It can be seen that the nickel niobate prepared according to the scheme of Example 3 exhibits excellent cycle stability, and can still maintain ~360 mAh g after 250 cycles at 1C. -1 Specific capacity.

[0059] Example 4

[0060] Preparation of nickel niobate (Ni2Nb2O7) material:

[0061] NbCl5 and NiO are mixed at a Nb / Ni molar ratio of 1:1, and KF, NaF and NiCl2 (molar percentages of 44%, 44% and 12% respectively) are added as molten salt reaction media, and metal oxides and inorganic salts are mixed at a mass ratio of 1:3; an appropriate amount of ethanol solution is added to the above mixture to make it completely infiltrated and wet mixed for 8 hours, and then placed in an 80℃ oven for drying for 24 hours. The dried product is ground into powder, placed in a corundum crucible, placed in a muffle furnace, heated to 850℃ at a heating rate of 5℃ / min, kept warm for 6 hours, and then cooled to room temperature. The product in the crucible is then washed and filtered with deionized water for multiple times, and after drying at 80℃, nickel niobate (Ni2Nb2O7) material is obtained.

[0062] The prepared nickel niobate (Ni2Nb2O7) is used to assemble the battery:

[0063] The synthesized sample (active material), carbon black (conductive agent) and PVDF (binder) were mixed in a mass ratio of 7:2:1, zirconium beads were added for ball milling, the viscosity was adjusted with NMP, and then evenly coated on copper foil and placed in a vacuum drying oven at 40°C for 12 hours. The copper foil was then cut into electrode discs with a diameter of 12 mm and used as the negative electrode. A metal lithium sheet was used as the counter electrode, and a Celgard2325 polypropylene porous membrane was used as the diaphragm. A CR2016 button lithium-ion battery was assembled in a glove box protected by high-purity argon. The assembled battery was left standing at room temperature for 24 hours before its electrochemical performance was tested.

[0064] Battery test parameters: Test its rate performance in the voltage window of 0.005~3V: During the charge and discharge cycle, test the battery at different current densities of 0.5, 1, 2, 5, 10, 20, 50C (1C = 236mAh g -1 ) were cycled 10 times, and the battery was finally restored to 1C rate. The cycle performance test is to charge and discharge the battery at a fixed current density (1C, 10C). The charge and discharge test temperature of all batteries was carried out in a 25℃ constant temperature box.

[0065] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A method for preparing a nickel niobate negative electrode material, characterized in that: The preparation method comprises the following steps: mixing a niobium compound and a nickel compound, and adding an inorganic salt to obtain a mixture; Adding an appropriate amount of ethanol solution to the mixture to completely soak it and wet mix it, and then drying it; The dried product is ground into powder, placed in a muffle furnace, heated to 600-1200°C, kept warm for 0.5-20h, and then cooled; The cooled product is washed, filtered, and dried to obtain the nickel niobate negative electrode material, which is a mixed phase of Ni4Nb2O9 and NiNb2O6.

2. The preparation method according to claim 1, characterized in that The niobium compound is one of niobium oxide, niobium carbonate, niobium hydroxide, niobium chloride, niobium nitrate or niobium sulfate, or a mixture of two or more thereof; the nickel compound is one of nickel oxide, nickel carbonate, nickel hydroxide, nickel chloride, nickel nitrate or nickel sulfate, or a mixture of two or more thereof.

3. The preparation method according to claim 1, characterized in that: The niobium compound and the nickel compound are mixed at a molar ratio of 0.5 to 18.

4. The preparation method according to claim 1, characterized in that: The inorganic salt is a mixture of two or more of alkali metal chlorides or fluorides and nickel chloride, and the nickel chloride accounts for 3-15 mol% of the total amount of the inorganic salt.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the inorganic salt to the total amount of the niobium compound and the nickel compound is 5:1-1:

20.

6. The preparation method according to claim 1, characterized in that: The wet mixing time is 2 to 24 hours.

7. The preparation method according to claim 1, characterized in that: The heating rate is 0.5~20℃ / min.

8. The nickel niobate negative electrode material obtained by the preparation method according to claim 1.

9. The nickel niobate negative electrode material according to claim 8, characterized in that: The nickel niobate is a mixed phase of Ni4Nb2O9 and NiNb2O6.

10. Use of the nickel niobate negative electrode material according to claim 8 or 9 in a lithium ion battery.