Method for preparing lithium-rich manganese-based positive electrode material through presintering
Through the combination of presintering process and fast ion conductors, the problems of structural stability and cycle life of lithium-rich manganese-based positive electrode materials in electrochemical cycles are solved, forming a stable redox center and cladding layer, improving the circulation of the material Stability and ion transport performance extend the life of the battery.
Patent Information
- Application Number
- CN202411064566.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
Lithium-rich manganese-based positive electrode materials show poor structural stability, lower cycle stability and short cycle life in electrochemical cycles, and are prone to metal ion migration, electrolyte decomposition and lattice oxygen detachment, which affects Overall performance and life of the battery.
Using the presintering process, metal elements such as Sr, Sb, W, Al, Mo, La are introduced to combine with oxygen to form a stable redox center, and a stable coating layer is constructed by the addition of fast ion conductors, and the calcination conditions are controlled to form a uniform The microstructure and protective film reduce internal defects and structural changes of the material.
It effectively reduces metal ion migration and structural degradation, improves the cyclic stability and ion transmission performance of materials, extends the cycle life and storage performance of the battery, and enhances the overall performance and safety of the battery.
Smart Images

Figure BDA0004978984900000091 
Figure HDA0004978984910000011 
Figure HDA0004978984910000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of C01G 53 / 00, and in particular to a method for preparing a lithium-rich manganese-based positive electrode material by pre-sintering. Background Art
[0002] Lithium-rich manganese-based cathode materials have attracted much attention due to their high energy density and cost-effectiveness, and are regarded as strong candidates for the next generation of lithium-ion battery cathode materials. Lithium-rich manganese-based cathode materials have a high theoretical specific capacity of more than 250mAh / g, which gives them a clear advantage in improving battery energy density. The abundant manganese resources make lithium-rich manganese-based cathode materials lower in cost than ternary materials containing cobalt or nickel. At present, lithium-rich manganese-based cathode materials have been used in lithium batteries in small power, energy storage, digital and other fields, and are penetrating into the power field. Despite the advantages of high energy density, lithium-rich manganese-based cathode materials still face some technical challenges in practical applications. Lithium-rich manganese-based cathode materials will undergo some irreversible side reactions during the first charging process, such as electrolyte decomposition, oxygen release, etc., resulting in the loss of active lithium, thereby reducing the first coulombic efficiency. In addition, the ion diffusion kinetics of lithium-rich manganese-based cathode materials are slow. When charging and discharging at high rates, lithium ions cannot be quickly embedded and extracted in the cathode material, resulting in poor rate performance. During the cycle, under the high voltage working environment, the lithium-rich manganese-based positive electrode material undergoes the migration of transition metal ions, phase change and irreversible release of oxygen, resulting in poor cycle stability and storage performance of the lithium-rich manganese-based positive electrode material. For example, a Chinese patent (publication number CN 116332246A) discloses a lithium-rich manganese-based positive electrode material and its preparation method and application, which improves the reversible capacity, discharge capacity and cycle stability of the battery without pre-sintering pretreatment by preparing a magnesium-doped precursor by carbonate coprecipitation, but still cannot reduce metal ion migration, inhibit material structure changes, alleviate electrolyte decomposition and reduce lattice oxygen release. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a method for preparing lithium-rich manganese-based positive electrode materials by pre-sintering, which overcomes the problems of poor structural stability, low cycle stability and short cycle life of lithium-rich manganese-based positive electrode materials prepared by existing processes in electrochemical cycles, effectively reduces metal ion migration, inhibits material structure changes, alleviates electrolyte decomposition and reduces lattice oxygen release, thereby ensuring the overall performance and life of subsequent batteries.
[0004] The present invention provides a method for preparing a lithium-rich manganese-based positive electrode material by pre-sintering, which at least comprises the following steps:
[0005] (1) preparing a lithium-rich manganese-based cathode material precursor;
[0006] (2) mixing a lithium-rich manganese-based positive electrode material precursor with a metal element and placing the mixture in a pot for pre-sintering to obtain a pre-sintered precursor;
[0007] (3) mixing the pre-sintered precursor with the lithium salt and then calcining once to obtain a single-calcined material;
[0008] (4) The primary calcined material is mixed with the fast ion conductor and then calcined for a second time, and then crushed and sieved to obtain a finished positive electrode material.
[0009] As a preferred technical solution, the structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni x Co y Mn z (OH)2, where x+y+z=1, 0.2≤x≤0.5, 0.5≤z≤1.0, y=1-xz.
[0010] Preferably, 0.2≤x≤0.3, 0.5≤z≤0.6, y=1-xz.
[0011] As a preferred technical solution, the preparation method of the lithium-rich manganese-based positive electrode material precursor is: prepare a mixed salt solution of nickel salt, cobalt salt, manganese salt and pure water, and simultaneously prepare a mixed aqueous solution of sodium hydroxide and ammonia water; mix the two solutions, obtain a precipitate after reaction, filter, wash and dry the precipitate to obtain a lithium-rich manganese-based positive electrode material precursor.
[0012] As a preferred technical solution, the nickel salt is NiSO4·6H2O, the cobalt salt is CoSO4·7H2O, and the manganese salt is MnSO4·H2O.
[0013] As a preferred technical solution, the concentration of the mixed salt solution is 0.5-3.5 mol / L, the concentration of NaOH in the mixed aqueous solution is 3-12 mol / L, and the concentration of ammonia water is 0-7 mol / L. Preferably, the concentration of the mixed salt solution is 1-2 mol / L, the concentration of NaOH in the mixed aqueous solution is 5-8 mol / L, and the concentration of ammonia water is 2-5 mol / L.
[0014] As a preferred technical solution, the reaction conditions are: reaction time is 30-45h, reaction pH is 11-12, and reaction temperature is 30-70°C. Preferably, the reaction conditions are: reaction time is 40-45h, reaction pH is 11-12, and reaction temperature is 40-60°C.
[0015] As a preferred technical solution, the metal element is at least one of Sr, Sb, W, Al, Mo, and La, preferably La or Sb.
[0016] As a preferred technical solution, the added amount of the metal element accounts for 0.05-0.5wt% of the weight of the lithium-rich manganese-based positive electrode material precursor, preferably 0.15-0.30wt%.
[0017] As a preferred technical solution, the amount of the filling is less than 90% of the volume of the sagger, preferably 50-80%.
[0018] As a preferred technical solution, the pre-sintering treatment conditions are: temperature of 600-900°C, time of 4-8 hours. Preferably, the pre-sintering treatment conditions are: temperature of 700-800°C, time of 5-7 hours.
[0019] As a preferred technical solution, the lithium salt is lithium carbonate.
[0020] As a preferred technical solution, the pre-sintered precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of (1-1.5):1, preferably (1.1-1.3):1.
[0021] Since the lithium-rich manganese-based positive electrode material prepared by conventional processes exhibits poor structural stability, low cycle stability and short cycle life in electrochemical cycles, and is more likely to undergo oxygen precipitation at high voltages, increasing safety hazards, and is more likely to undergo side reactions with the electrolyte, resulting in electrolyte decomposition, affecting the overall performance and life of the battery, the present invention has carried out targeted process optimization for lithium-rich manganese-based positive electrode materials. Specifically, the present invention designs a pre-sintering process, especially introduces at least one metal element among Sr, Sb, W, Al, Mo, and La in the pre-sintering process, which can form a more stable redox center after combining with oxygen, thereby enhancing the stability of the material structure, so that when it is operated at high voltage, it can maintain the crystal structure of the material and reduce structural degradation. Furthermore, the present invention controls the amount of metal elements added and the conditions of the pre-sintering treatment, and forms a stable oxide layer on the surface of the material through pre-sintering oxidation, which acts as a protective film to reduce the side reactions between the electrolyte and the active substance, reduce the risk of thermal runaway, and alleviate electrolyte decomposition. In addition, pre-sintering treatment can form a more uniform microstructure, reduce internal defects in the material, reduce the migration and loss of active metal ions during the charge and discharge process, and prevent structural changes that may occur during subsequent high-temperature sintering, thereby improving the material's recycling and storage performance in many aspects.
[0022] As a preferred technical solution, the conditions for the primary calcination are: temperature of 850-1000° C. and time of 6-15 hours.
[0023] As a preferred technical solution, the fast ion conductor is selected from LATP, LLZO, Li4Ti5O12 , Li3PO4, preferably LATP.
[0024] As a preferred technical solution, the addition amount of the fast ion conductor is 0.05-0.5wt% of the weight of the sintered material, preferably 0.1-0.3wt%.
[0025] Furthermore, the present invention adds fast ion conductors LATP (lithium aluminum titanium phosphate), LLZO (lithium zirconium oxide / lithium lanthanum zirconate), Li4Ti5O 12 At least one of Li3PO4 and Li2PO4, combined with the control of secondary calcination conditions, constructs a stable coating layer, reduces the structural changes of the positive electrode material during the charge and discharge process, improves the cycle stability of the material, improves the ion transport performance of the positive electrode material, accelerates the diffusion rate of lithium ions in the positive electrode material, inhibits the release of irreversible oxygen in the material, and improves the battery cycle life and storage performance.
[0026] As a preferred technical solution, the conditions for the secondary calcination are: temperature of 400-600° C. and time of 3-6 hours.
[0027] As a preferred technical solution, the mixing equipment is a high-speed mixer or an oblique mixer.
[0028] Beneficial Effects
[0029] 1. The present invention provides a method for preparing lithium-rich manganese-based positive electrode materials by pre-sintering, which overcomes the problem that the lithium-rich manganese-based positive electrode materials prepared by the existing process show poor structural stability, low cycle stability and short cycle life in the electrochemical cycle, effectively reduces metal ion migration, inhibits material structure changes, alleviates electrolyte decomposition and reduces lattice oxygen release, thereby ensuring the overall performance and life of subsequent batteries.
[0030] 2. The present invention optimizes the process of lithium-rich manganese-based positive electrode materials. Specifically, the present invention designs a pre-sintering process, especially introduces at least one metal element among Sr, Sb, W, Al, Mo, and La in the pre-sintering process, which can form a more stable redox center after combining with oxygen, thereby enhancing the stability of the material structure, so that when it runs at high voltage, it can maintain the crystal structure of the material and reduce structural degradation.
[0031] 3. The present invention controls the amount of metal elements added and the conditions of the pre-sintering treatment to form a stable oxide layer on the surface of the material through pre-sintering oxidation, which acts as a protective film to reduce the side reactions between the electrolyte and the active substance, reduce the risk of thermal runaway, and alleviate the decomposition of the electrolyte.
[0032] 4. The present invention can form a more uniform microstructure through pre-sintering treatment, reduce internal defects of the material, reduce the migration and loss of active metal ions during the charge and discharge process, and prevent structural changes that may occur during subsequent high-temperature sintering, thereby improving the material's circulation and storage performance in many aspects.
[0033] 5. The present invention adds fast ion conductors LATP (lithium aluminum titanium phosphate), LLZO (lithium zirconium oxide / lithium lanthanum zirconate), Li4Ti5O 12 At least one of Li3PO4 and Li2PO4, combined with the control of secondary calcination conditions, constructs a stable coating layer, reduces the structural changes of the positive electrode material during the charge and discharge process, improves the cycle stability of the material, improves the ion transport performance of the positive electrode material, accelerates the diffusion rate of lithium ions in the positive electrode material, inhibits the release of irreversible oxygen in the material, and improves the battery cycle life and storage performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is an electron microscope image of the positive electrode material provided in Examples 1, 2, and 3 of the present invention, where a, b, and c correspond to Examples 1, 2, and 3, respectively.
[0035] Figure 2 This is an electron microscope image of the positive electrode material provided for comparative examples 1 and 2 of the present invention, where a and b correspond to comparative examples 1 and 2, respectively.
[0036] Figure 3 XRD patterns of positive electrode materials provided for the embodiments and comparative examples. The curves in the figure correspond to embodiments 1, 2, 3, and comparative examples 1 and 2 from top to bottom, respectively.
[0037] Figure 4 The cycle test results of the positive electrode materials provided in the embodiments and comparative examples are shown in the figure. The curves in the figure correspond to embodiments 3, 2, 1, comparative examples 2, 1 from top to bottom, respectively. DETAILED DESCRIPTION
[0038] Example 1
[0039] Embodiment 1 of the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material by pre-sintering, comprising the following steps:
[0040] (1) preparing a lithium-rich manganese-based cathode material precursor;
[0041] (2) placing the lithium-rich manganese-based positive electrode material precursor in a pot and performing a pre-sintering treatment to obtain a pre-sintered precursor;
[0042] (3) crushing the pre-sintered precursor, passing it through a 300-mesh sieve, mixing it with a lithium salt, and then calcining it once to obtain a first-calcined material;
[0043] (4) The first-fired material is crushed, passed through a 300-mesh sieve, mixed with a fast ion conductor, and then calcined for a second time. After crushing and passing through a 300-mesh sieve, a finished positive electrode material is obtained.
[0044] The structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni 0.28 Co 0.15 Mn 0.57 (OH)2.
[0045] The preparation method of the lithium-rich manganese-based positive electrode material precursor is as follows: nickel salt, cobalt salt, manganese salt and pure water are prepared into a mixed salt solution, and a mixed aqueous solution of sodium hydroxide and ammonia water is prepared at the same time; the two solutions are mixed, and a precipitate is obtained after reaction, and the precipitate is filtered, washed and dried to obtain the lithium-rich manganese-based positive electrode material precursor.
[0046] The nickel salt is NiSO4·6H2O, the cobalt salt is CoSO4·7H2O, and the manganese salt is MnSO4·H2O.
[0047] The concentration of the mixed salt solution is 1.5 mol / L, the concentration of NaOH in the mixed aqueous solution is 6 mol / L, and the concentration of ammonia water is 3 mol / L.
[0048] The reaction conditions are as follows: reaction time is 42 h, reaction pH is 11, and reaction temperature is 50°C.
[0049] The amount of the filling is 70% of the volume of the sagger, and the size of the sagger is: length*width*height=330*330*100mm.
[0050] The pre-sintering treatment conditions are: temperature of 750° C. and time of 6 hours.
[0051] The lithium salt is lithium carbonate.
[0052] The pre-sintered precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of 1.2:1.
[0053] The conditions of the primary calcination are: temperature of 965° C. and time of 12 h.
[0054] The fast ion conductor is LATP.
[0055] The addition amount of the fast ion conductor is 0.2 wt % of the weight of the sintered material.
[0056] The conditions of the secondary calcination are: temperature of 450° C. and time of 4 hours.
[0057] The mixing equipment is an inclined mixer.
[0058] Example 2
[0059] Embodiment 2 of the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material by pre-sintering, comprising the following steps:
[0060] (1) preparing a lithium-rich manganese-based cathode material precursor;
[0061] (2) mixing a lithium-rich manganese-based positive electrode material precursor with a metal element and placing the mixture in a pot for pre-sintering to obtain a pre-sintered precursor;
[0062] (3) crushing the pre-sintered precursor, passing it through a 300-mesh sieve, mixing it with a lithium salt, and then calcining it once to obtain a first-calcined material;
[0063] (4) The first-fired material is crushed, passed through a 300-mesh sieve, mixed with a fast ion conductor, and then calcined for a second time. After crushing and passing through a 300-mesh sieve, a finished positive electrode material is obtained.
[0064] The structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni 0.28 Co 0.15 Mn 0.57 (OH)2.
[0065] The preparation method of the lithium-rich manganese-based positive electrode material precursor is as follows: nickel salt, cobalt salt, manganese salt and pure water are prepared into a mixed salt solution, and a mixed aqueous solution of sodium hydroxide and ammonia water is prepared at the same time; the two solutions are mixed, and a precipitate is obtained after reaction, and the precipitate is filtered, washed and dried to obtain the lithium-rich manganese-based positive electrode material precursor.
[0066] The nickel salt is NiSO4·6H2O, the cobalt salt is CoSO4·7H2O, and the manganese salt is MnSO4·H2O.
[0067] The concentration of the mixed salt solution is 1.5 mol / L, the concentration of NaOH in the mixed aqueous solution is 6 mol / L, and the concentration of ammonia water is 3 mol / L.
[0068] The reaction conditions are as follows: reaction time is 42 h, reaction pH is 11, and reaction temperature is 50°C.
[0069] The metal element is La.
[0070] The added amount of the metal element accounts for 0.15wt% of the weight of the lithium-rich manganese-based positive electrode material precursor.
[0071] The amount of the filling is 70% of the volume of the sagger, and the size of the sagger is: length*width*height=330*330*100mm.
[0072] The pre-sintering treatment conditions are: temperature of 750° C. and time of 6 hours.
[0073] The lithium salt is lithium carbonate.
[0074] The pre-sintered precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of 1.2:1.
[0075] The conditions of the primary calcination are: temperature of 965° C. and time of 12 h.
[0076] The fast ion conductor is LATP.
[0077] The addition amount of the fast ion conductor is 0.2 wt % of the weight of the sintered material.
[0078] The conditions of the secondary calcination are: temperature of 450° C. and time of 4 hours.
[0079] The mixing equipment is an inclined mixer.
[0080] Example 3
[0081] Example 3 of the present invention provides a method for preparing lithium-rich manganese-based positive electrode materials by pre-sintering. Its specific implementation method is the same as that of Example 2, except that the metal element is Sb, and the added amount of the metal element accounts for 0.30wt% of the weight of the lithium-rich manganese-based positive electrode material precursor.
[0082] Comparative Example 1
[0083] Comparative Example 1 of the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material, comprising the following steps:
[0084] (1) preparing a lithium-rich manganese-based cathode material precursor;
[0085] (2) mixing the lithium-rich manganese-based positive electrode material precursor with the lithium salt and placing them in a pot for calcining to obtain a calcined material;
[0086] (3) The primary calcined material is crushed, passed through a 300-mesh sieve, mixed with a fast ion conductor, and then calcined for a second time. After crushing and passing through a 300-mesh sieve, a finished positive electrode material is obtained.
[0087] The structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni 0.28 Co 0.15 Mn 0.57 (OH)2.
[0088] The preparation method of the lithium-rich manganese-based positive electrode material precursor is as follows: nickel salt, cobalt salt, manganese salt and pure water are prepared into a mixed salt solution, and a mixed aqueous solution of sodium hydroxide and ammonia water is prepared at the same time; the two solutions are mixed, and a precipitate is obtained after reaction, and the precipitate is filtered, washed and dried to obtain the lithium-rich manganese-based positive electrode material precursor.
[0089] The nickel salt is NiSO4·6H2O, the cobalt salt is CoSO4·7H2O, and the manganese salt is MnSO4·H2O.
[0090] The concentration of the mixed salt solution is 1.5 mol / L, the concentration of NaOH in the mixed aqueous solution is 6 mol / L, and the concentration of ammonia water is 3 mol / L.
[0091] The reaction conditions are as follows: reaction time is 42 h, reaction pH is 11, and reaction temperature is 50°C.
[0092] The amount of the filling is 70% of the volume of the sagger, and the size of the sagger is: length*width*height=330*330*100mm.
[0093] The lithium salt is lithium carbonate.
[0094] The lithium-rich manganese-based positive electrode material precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of 1.2:1 after mixing.
[0095] The conditions of the primary calcination are: temperature of 965° C. and time of 12 h.
[0096] The fast ion conductor is LATP.
[0097] The addition amount of the fast ion conductor is 0.2 wt % of the weight of the sintered material.
[0098] The conditions of the secondary calcination are: temperature of 450° C. and time of 4 hours.
[0099] The mixing equipment is an inclined mixer.
[0100] Comparative Example 2
[0101] Comparative Example 2 of the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material, comprising the following steps:
[0102] (1) preparing a lithium-rich manganese-based cathode material precursor;
[0103] (2) placing a mixture of a lithium-rich manganese-based positive electrode material precursor, a lithium salt and a metal element in a pot and calcining the mixture once to obtain a calcined material;
[0104] (3) The primary calcined material is crushed, passed through a 300-mesh sieve, mixed with a fast ion conductor, and then calcined for a second time. After crushing and passing through a 300-mesh sieve, a finished positive electrode material is obtained.
[0105] The structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni 0.28 Co 0.15 Mn 0.57 (OH)2.
[0106] The preparation method of the lithium-rich manganese-based positive electrode material precursor is as follows: nickel salt, cobalt salt, manganese salt and pure water are prepared into a mixed salt solution, and a mixed aqueous solution of sodium hydroxide and ammonia water is prepared at the same time; the two solutions are mixed, and a precipitate is obtained after reaction, and the precipitate is filtered, washed and dried to obtain the lithium-rich manganese-based positive electrode material precursor.
[0107] The nickel salt is NiSO4·6H2O, the cobalt salt is CoSO4·7H2O, and the manganese salt is MnSO4·H2O.
[0108] The concentration of the mixed salt solution is 1.5 mol / L, the concentration of NaOH in the mixed aqueous solution is 6 mol / L, and the concentration of ammonia water is 3 mol / L.
[0109] The reaction conditions are as follows: reaction time is 42 h, reaction pH is 11, and reaction temperature is 50°C.
[0110] The amount of the filling is 70% of the volume of the sagger, and the size of the sagger is: length*width*height=330*330*100mm.
[0111] The lithium-rich manganese-based positive electrode material precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of 1.2:1 after mixing.
[0112] The lithium salt is lithium carbonate.
[0113] The metal element is La, and the added amount of the metal element accounts for 0.30wt% of the weight of the mixed material.
[0114] The conditions of the primary calcination are: temperature of 965° C. and time of 12 h.
[0115] The fast ion conductor is LATP.
[0116] The addition amount of the fast ion conductor is 0.2 wt % of the weight of the sintered material.
[0117] The conditions of the secondary calcination are: temperature of 450° C. and time of 4 hours.
[0118] The mixing equipment is an inclined mixer.
[0119] Performance Testing
[0120] 1. The positive electrode materials provided in the examples and comparative examples were assembled into button cells and soft-pack batteries, wherein: the button cells were tested for charge specific capacity, discharge specific capacity, initial efficiency and 50-cycle cycle retention rate (see Figure 4), the test conditions are: 2.3-4.55V, 1C=230mAh / g; the soft-pack battery was subjected to 7-day capacity recovery rate and 7-day expansion rate tests, the test conditions are: 2.3-4.5 formation, 4.46 capacity division, the test results are shown in Table 1.
[0121] 2. SEM characterization of the positive electrode materials provided in the examples and comparative examples (see Figure 1 , 2 ) and XRD characterization (see Figure 3 ), SEM characterization results show that: the particle morphology in the embodiment is fuller, indicating that the material structure is more stable, which is beneficial to the cycle and storage performance; XRD characterization results show that: there is no obvious difference between the embodiment process and the comparative example process, and both form a lithium-rich manganese-based structure, which is consistent with the lithium-rich manganese-based XRD structural characteristics.
[0122] Table 1
[0123]
Claims
1. A method for preparing a lithium-rich manganese-based positive electrode material by pre-sintering, characterized in that: At least the following steps are included: (1) preparing a lithium-rich manganese-based cathode material precursor; (2) mixing a lithium-rich manganese-based positive electrode material precursor with a metal element and placing the mixture in a pot for pre-sintering to obtain a pre-sintered precursor; (3) mixing the pre-sintered precursor with the lithium salt and then calcining once to obtain a single-calcined material; (4) The primary calcined material is mixed with the fast ion conductor and then calcined for a second time, and then crushed and sieved to obtain a finished positive electrode material.
2. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 1, characterized in that: The structural formula of the lithium-rich manganese-based positive electrode material precursor is Ni x Co y Mn z (OH)2, where x+y+z=1, 0.2≤x≤0.5, 0.5≤z≤1.0, y=1-xz.
3. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 1 or 2, characterized in that: The metal element is at least one of Sr, Sb, W, Al, Mo and La, and the added amount of the metal element accounts for 0.05-0.5wt% of the weight of the lithium-rich manganese-based positive electrode material precursor.
4. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 3, characterized in that: The pre-sintering treatment conditions are: temperature of 600-900° C. and time of 4-8 hours.
5. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 4, characterized in that: The pre-sintered precursor and the lithium salt are mixed in a molar ratio of Li to (Ni+Co+Mn) of (1-1.5):
1.
6. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 5, characterized in that: The conditions of the primary calcination are: temperature of 850-1000° C. and time of 6-15 hours.
7. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 5, characterized in that: The fast ion conductor is selected from LATP, LLZO, Li4Ti5O 12 , Li3PO4, and the addition amount of the fast ion conductor is 0.05-0.5wt% of the weight of the calcined material.
8. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 7, characterized in that: The conditions for the secondary calcination are: temperature of 400-600° C. and time of 3-6 hours.
9. The method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to claim 8, characterized in that: The mixing equipment is a high-speed mixer or an oblique mixer.
10. A positive electrode material prepared by the method for preparing lithium-rich manganese-based positive electrode material by pre-sintering according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium-rich manganese-based positive electrode material and preparation method and application thereof
CN116332246A
Modified lithium-rich manganese-based positive electrode material and preparation method thereof
CN106654251A
Modification method of single-crystal ternary positive electrode material
CN112080800A
Electrolyte-modified lithium-rich manganese-based positive electrode material and preparation method thereof
CN116387501A
Nasicon-type solid electrolyte, positive electrode material coated with same, and preparation methods therefor
WO2023056748A1
Cited By
Modified lithium-rich manganese-based spherical aggregate and preparation method thereof, lithium-rich manganese-based electrode and preparation method and application thereof
CN120033228A
Lithium-rich manganese-based positive electrode material with core-shell structure and preparation method of lithium-rich manganese-based positive electrode material
CN121726383A