Coating modified sodium ion battery layered oxide positive electrode material, preparation method thereof and battery

By covering the surface of the positive electrode material of the sodium ion battery, the problems of prone collapse of the sodium ion battery structure and low circulation stability are solved, and the circulation performance and application value of the battery are significantly improved.

CN119092687APending Publication Date: 2024-12-06ZHUJI PAWA NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411265227.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The structure of the positive electrode material of sodium ion battery is easily affected by the radius and phase transition of sodium ions, resulting in low cyclic stability and working voltage. The material is prone to structural collapse during the reaction process, affecting its application value.

Method used

The surface of the O3-type layered oxide positive electrode material is coated with Na3Ca2TaO6 material, and a cladding layer is formed through the sintering process to inhibit changes in sodium ion transfer structure and electrolyte erosion, slow down the phase transition speed, and improve the cycling performance of the material.

Benefits of technology

It significantly improves the circulation performance of sodium ion batteries, extends the service life of the material, reduces the increase in the internal impedance of the battery, and enhances the practical application value of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092687A_ABST
    Figure CN119092687A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion battery materials, and discloses a coated modified sodium ion battery layered oxide positive electrode material, a preparation method thereof and a battery. The coated modified sodium ion battery layered oxide positive electrode material comprises a positive electrode material substrate and a coating layer located on at least part of the surface of the positive electrode material substrate, the positive electrode material substrate is an O3 type layered oxide positive electrode material NaNi < x > Fe < 1-x-y > Mn < y > O < 2 >, and the material of the coating layer is Na < 3 > Ca < 2 > TaO < 6 >. And mixing the positive electrode material substrate and the coating layer material, and sintering to obtain the positive electrode material. The preparation method is simple and easy to operate. And the cycle performance of the sodium ion battery applying the coated and modified positive electrode material is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery materials, and in particular relates to the coating modification of positive electrode materials of sodium ion batteries. Background Art

[0002] Compared with lithium resources, sodium resources in the earth's crust are abundant, cheap, and widely distributed. Sodium-ion batteries are considered to be a new generation of energy storage technology. From the perspective of existing sodium-ion battery positive electrode materials, layered oxides are the earliest studied sodium storage positive electrode materials, with relatively good cycle performance, high theoretical specific capacity, and low price. However, the radius and relative molecular weight of sodium ions are large, which greatly limits their ability to charge and discharge rapidly. At the same time, during the sodium storage process, sodium ions with a larger radius can easily cause the structure of the material to collapse, greatly reducing the cycle stability of the battery. In addition, the standard electrode potential of sodium is lower than that of lithium and Na + Specific gravity ratio + The large capacity also makes the working voltage and energy density of sodium-ion batteries relatively low. The layered oxide materials of sodium-ion batteries are prone to phase change during the reaction process. As sodium ions are deintercalated, the structure is prone to local collapse, and the rapid capacity decay seriously affects its practical application. Current studies have shown that coating and modification on the surface of the positive electrode material can effectively improve the problem of capacity decay during the cycle of layered oxide materials, greatly improving the practical application value of the material. The coating material is the key to coating and modifying the surface of the positive electrode material. Summary of the invention

[0003] The main purpose of the present invention is to provide a coated modified sodium ion battery layered oxide positive electrode material and a preparation method thereof.

[0004] To achieve the above objectives, the present invention provides the following specific technical solutions.

[0005] In the first aspect, the present invention provides a coated modified sodium ion battery layered oxide positive electrode material, comprising a positive electrode material matrix and a coating layer located on at least a portion of the surface of the positive electrode material matrix; the positive electrode material matrix is ​​an O3 type layered oxide positive electrode material NaNi x Fe 1-x-y Mn y O2, 0<x<0.5, 0.5<y<1; the coating layer material is Na3Ca2TaO6.

[0006] In a second aspect, the present invention provides a method for preparing the above-mentioned coated modified sodium ion battery layered oxide positive electrode material, comprising: mixing the positive electrode material matrix and the coating layer material and then sintering to obtain.

[0007] Based on the same inventive concept, the present invention provides a sodium ion battery, comprising the aforementioned coated and modified sodium ion battery layered oxide positive electrode material.

[0008] The above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: Coating Na3Ca2TaO6 on the surface of the O3-type layered oxide positive electrode material can inhibit the structural changes in the sodium ion transfer process during the cycle, while inhibiting the erosion of the electrolyte, slowing down the phase transformation rate of the core material, and inhibiting the increase in the surface impedance of the material. Macroscopically, the cycle performance of the sodium ion battery using the coated and modified positive electrode material of the present invention is significantly improved.

[0009] The method for preparing the coated modified sodium ion battery positive electrode material of the present invention is simple, easy to operate, and has great industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is the XRD pattern of the layered oxide positive electrode material obtained in step (1) of Example 1.

[0011] Figure 2 This is a SEM image of the layered oxide positive electrode material obtained in step (1) of Example 1.

[0012] Figure 3 This is the XRD diagram of the sintered material obtained in step (2) of Example 1.

[0013] Figure 4 This is the SEM image of the coated and modified positive electrode material obtained in Example 1.

[0014] Figure 5 This is the cycle performance diagram of the battery. DETAILED DESCRIPTION

[0015] In the first aspect, some embodiments of the present invention provide a coated modified sodium ion battery layered oxide positive electrode material, comprising a positive electrode material matrix and a coating layer located on at least a portion of the surface of the positive electrode material matrix; the positive electrode material matrix is ​​an O3 type layered oxide positive electrode material NaNi x Fe 1-x-y Mn y O2, 0<x<0.5, 0.5<y<1; the coating layer material is Na3Ca2TaO6.

[0016] The applicant believes that the sodium-rich rock salt oxide Na3Ca2TaO6 is used as the coating material for sodium-ion batteries. The material structure contains three Na ions and is an octahedral configuration. Na, Ca and Ta atoms occupy octahedral sites in an orderly manner to form a superstructure with ordered cations. There are non-bonding oxygen states close to the Fermi level in the sodium-rich rock salt oxide. The redox reversibility of the oxygen radical can be enhanced by moving from 3d cations to 4d and 5d cations, thereby avoiding the formation of gaseous O2 when anions are oxidized. The coating material can inhibit the structural changes caused by the transfer of sodium ions during the cycle, while inhibiting the erosion of the electrolyte, slowing down the phase transition rate of the core material, and inhibiting the increase in the surface impedance of the material. The research results show that the coated modified positive electrode material can significantly improve the cycle performance of the battery.

[0017] In a further preferred embodiment, the mass percentage of the coating material and the positive electrode material matrix is ​​0.5% to 5%: 1. The coating layer itself does not provide capacity, and too much coating layer will lead to a decrease in the overall capacity of the material, affecting practical applications; too little coating layer material cannot form a uniform and effective coating layer.

[0018] In a second aspect, some embodiments of the present invention provide a method for preparing the above-mentioned coated modified sodium ion battery layered oxide positive electrode material, comprising: mixing the positive electrode material matrix and the coating layer material and sintering them to obtain.

[0019] In a further preferred embodiment, the sintering temperature is 750-1000° C. and the sintering time is 8-12 hours.

[0020] Cathode material matrix O3-type layered oxide cathode material NaNi x Fe 1-x-y Mn y O2 can be purchased from commercial sources or prepared by the following method: a sodium source, a nickel source, a manganese source, and an iron source are uniformly mixed according to a set molar ratio, and sintered to obtain the obtained product. In a specific embodiment, the sintering temperature is 750-1000° C., and the sintering time is 8-16 hours.

[0021] The coating material Na3Ca2TaO6 can be purchased through commercial channels, or prepared by the following method: adding sodium source, calcium source, tantalum source, and H3BO3 as flux to ethanol according to the molar ratio of Na, Ca, and Ta being 3:2:1, grinding evenly, drying, and sintering. In a specific embodiment, the amount of flux added is 2-8wt% of the mass of ethanol; the sintering temperature is 900-1200°C; and the sintering time is 3-6h.

[0022] The sodium source, nickel source, manganese source, iron source, calcium source and tantalum source are selected from oxides, carbonates, sulfates, oxalates and nitrates respectively.

[0023] In a third aspect, the present invention applies the aforementioned coated and modified sodium ion battery layered oxide positive electrode material in a sodium ion battery to test the electrical performance of the battery.

[0024] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0025] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0027] Example 1 Step (1): Na2CO3, NiO, MnO2, and Fe2O3 are uniformly mixed in a molar ratio of Na:Ni:Mn:Fe=3:1:1:1, and sintered in a muffle furnace at 900°C for 12 hours to obtain a layered oxide positive electrode material.

[0028] Figure 1 This is the XRD diagram of the layered oxide positive electrode material, which shows that it is an O3-type layered oxide positive electrode material NaNi 1 / 3Fe 1 / 3 Mn 1 / 3 O2.

[0029] Figure 2 This is the SEM image of the layered oxide positive electrode material.

[0030] Step (2): Na2CO3, CaCO3 and Ta2O5 are dispersed in ethanol at a molar ratio of Na:Ca:Ta=3:2:1, and 5% H3BO3 by mass of ethanol is added as a flux. The mixture is finely ground in an agate mortar and then dried in an oven. The dried sample is ground and then sintered at a temperature of 1100°C for 4 hours.

[0031] Figure 3 is the XRD diagram of the sintered material. It can be seen that the sintered material is Na3Ca2TaO6 and has an octahedral structure.

[0032] Step (3): The sintered material obtained in step (2) and the layered oxide positive electrode material obtained in step (1) are mixed in a mixer at a mass ratio of 2%:1. The speed of the mixer is 900 rpm and the mixing time is 30 minutes. The mixed materials are sintered at 900° C. for 12 hours to obtain a coated modified positive electrode material.

[0033] Figure 4 This is the SEM image of the coated and modified positive electrode material. It can be seen from the figure that the material is spherical particles with obvious layered characteristics, a relatively smooth outer layer, and a prominent surface coating layer morphology.

[0034] Example 2 Step (1): Na2CO3, NiO, MnO2, and Fe2O3 are uniformly mixed according to a molar ratio of Na:Ni:Mn:Fe=1:0.4:0.4:0.2, and sintered in a muffle furnace at 750°C for 8 hours to obtain a layered oxide positive electrode material.

[0035] Step (2): Na2CO3, CaCO3 and Ta2O5 are dispersed in ethanol at a molar ratio of Na:Ca:Ta=3:2:1, and 2% H3BO3 by mass of ethanol is added as a flux. The mixture is finely ground in an agate mortar and then dried in an oven. The dried sample is ground and then sintered at a temperature of 900°C for 3 h.

[0036] Step (3): The sintered material obtained in step (2) and the layered oxide positive electrode material obtained in step (1) are mixed in a mixer at a mass ratio of 0.5%:1, the mixer speed is 500 rpm, and the mixing time is 15 minutes. The mixed materials are sintered at 750° C. for 8 hours to obtain a coated modified positive electrode material.

[0037] Example 3 Step (1): Na2CO3, NiO, MnO2, and Fe2O3 are uniformly mixed according to a molar ratio of Na:Ni:Mn:Fe=1:0.3:0.4:0.3, and sintered in a muffle furnace at 1000°C for 16 hours to obtain a layered oxide positive electrode material.

[0038] Step (2): Na2CO3, CaCO3 and Ta2O5 are dispersed in ethanol at a molar ratio of Na:Ca:Ta=3:2:1, and 8% H3BO3 by mass of ethanol is added as a flux. The mixture is finely ground in an agate mortar and then dried in an oven. The dried sample is ground and then sintered at a temperature of 1200°C for 6 hours.

[0039] Step (3): The sintered material obtained in step (2) and the layered oxide positive electrode material obtained in step (1) are mixed in a mixer at a mass ratio of 5%:1, the mixer speed is 900 rpm, and the mixing time is 45 minutes. The mixed materials are sintered at 1000° C. for 12 hours to obtain a coated modified positive electrode material.

[0040] The coated modified positive electrode materials obtained in Examples 1-3, NaNi 1 / 3 Fe1 / 3 Mn 1 / 3 O2、NaNi 0.4 Fe 0.4 Mn 0.2 O2、NaNi 0.3 Fe 0.4 Mn 0.3 O2 was assembled into a battery in the following way: positive electrode material: conductive graphite: PVDF was weighed and ground in a ratio of 8:1:1, dissolved in an appropriate amount of N-methylpyrrolidone (NMP) and stirred evenly to form a slurry, the slurry was coated on the current collector aluminum foil, dried at 90°C in a blast dryer for 12 hours, and then punched into a disc electrode with a diameter of 12 mm. The disc electrode was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1 mol / L NaPF6 / EC+DEC+DMC (EC:DEC:DMC=1:1:1 volume ratio) was used as the electrolyte, and GF / D sodium electrolyte was used as the separator. The button cell was assembled in the glove box according to the assembly order of the button cell.

[0041] The electrical performance of the battery was tested in the following manner: operating voltage range 2.0-4.0V, current density 1C, and 50 cycles.

[0042] The battery cycle performance test results are as follows: Figure 5 As shown in the figure, it can be seen that the Na3Ca2TaO6-coated modified layered oxide positive electrode material makes the battery have better cycle stability.

[0043] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A coated modified sodium ion battery layered oxide positive electrode material, characterized in that: It includes a positive electrode material matrix and a coating layer located on at least part of the surface of the positive electrode material matrix; the positive electrode material matrix is ​​an O3 type layered oxide positive electrode material NaNi x Fe 1-x-y Mn y O2, 0<x<0.5, 0.5<y<1; the material of the coating layer is Na3Ca2TaO6.

2. The coated modified sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The mass percentage of the coating layer material and the positive electrode material matrix is ​​0.5%~5%:

1.

3. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 1 or 2, characterized in that: include: The positive electrode material matrix and the coating layer material are mixed and sintered; the positive electrode material matrix is ​​an O3 type layered oxide positive electrode material NaNi x Fe 1-x-y Mn y O2, 0<x<0.5, 0.5<y<1; the coating layer material is Na3Ca2TaO6.

4. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 3, characterized in that: The sintering temperature is 750-1000° C. and the sintering time is 8-12 hours.

5. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 3 or 4, characterized in that: Cathode material matrix O3-type layered oxide cathode material NaNi x Fe 1-x-y Mn y O2 is prepared by the following method: a sodium source, a nickel source, a manganese source, and an iron source are uniformly mixed according to a set molar ratio and sintered.

6. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 5, characterized in that: After the sodium source, nickel source, manganese source and iron source are evenly mixed, the sintering temperature is 750~1000℃, and the sintering time is 8~16h.

7. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 3 or 4, characterized in that: The coating material Na3Ca2TaO6 is prepared by the following method: sodium source, calcium source and tantalum source are added to ethanol according to the molar ratio of Na, Ca and Ta being 3:2:1, and H3BO3 is added as a flux, and after being evenly ground, it is dried and sintered.

8. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 7, characterized in that: The amount of flux added is 2~8wt% of the mass of ethanol.

9. The method for preparing the coated modified sodium ion battery layered oxide positive electrode material according to claim 7 or 8, characterized in that: The sintering temperature is 900~1200℃; the sintering time is 3~6h.

10. A battery, characterized in that: It comprises the coated and modified sodium ion battery layered oxide positive electrode material as described in claim 1 or 2.