Porous silica, deodorant, and method for producing deodorant
By using porous silica doped with Mn, Cu or Fe in the deodorant, the existing deodorant has solved the problem of low sulfur-containing odor removal and metal ion separation, and achieved efficient and stable odor removal and reduce drainage treatment burden.
Patent Information
- Application Number
- CN202080093281.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-01-17
AI Technical Summary
Existing deodorants are less efficient in removing sulfur-containing odors, and there are difficulties in drainage treatment that may detach and cause in use.
Porous silica doped with Mn, Cu or Fe is used as a deodorant, and a liquid deodorant is formed by mixing it with the solvent. The adsorption function of metal X is used to efficiently remove sulfur-containing odor, and doping metals Y and Z To improve hydrothermal durability and porous structure stability.
It significantly improves the removal efficiency of sulfur-containing odors, reduces the burden of metal ions detachment and drainage treatment, and enhances the deodorization ability of various odors.
Smart Images

Figure GDA0003748583670000171 
Figure GDA0003748583670000181
Abstract
Description
Technical Field
[0001] The present invention relates to porous silica, a deodorant and a method for producing the deodorant. Background Art
[0002] There are various products known as deodorants. Among deodorants, there is a certain demand for liquid deodorants according to their uses. In addition, there are various types of deodorants according to the odors to be deodorized. For example, there is a certain demand for deodorants that are to be deodorized for odors caused by sulfur-containing compounds (hereinafter also referred to as sulfur-containing odors).
[0003] Regarding the above-mentioned deodorant, for example, Patent Document 1 (Japanese Patent Application Laid-Open No. 2003-261425) discloses a deodorant for hair treated with cysteamine, which is characterized by containing one or more divalent metal ions. Cysteamine is a sulfur-containing compound. Summary of the invention
[0004] The present inventors have conducted research on improving the deodorizing efficiency of a liquid deodorant for removing sulfur-containing odors.
[0005] That is, an object of the present invention is to provide a liquid deodorant capable of efficiently deodorizing sulfur-containing odors, and a method for producing the same.
[0006] In order to solve the above-mentioned problems, the present invention includes the following matters.
[0007] [1] A porous silicon dioxide doped with a metal X, wherein the metal X is Mn or Cu.
[0008] [2] A porous silica for use in a liquid deodorant, the porous silica comprising at least one metal X selected from the group consisting of Mn, Cu and Fe.
[0009] [3] The porous silica according to [2], wherein the metal X is doped into the porous silica.
[0010] [4] The porous silica according to any one of [1] to [3], further comprising a metal different from the metal X.
[0011] [5] The porous silica according to [4], wherein the metal different from the metal X is a metal Y selected from the group consisting of Al and Zr.
[0012] [6] The porous silica according to [4] or [5], wherein the metal different from the metal X is a metal Z selected from the group consisting of Co, Zn, Ag and Ca.
[0013] [7] The porous silica according to [4] has a structure having a chemical composition represented by the following formula 1.
[0014] (Formula 1)SiO 2 aXO b / 2 ·cYO d / 2 ·eZO f / 2
[0015] (In Formula 1, X represents the metal X,
[0016] Y represents a metal Y selected from Al and Zr,
[0017] Z represents a metal Z selected from Co, Zn, Ag and Ca,
[0018] a represents a number greater than 0 and less than 0.1,
[0019] c and e represent numbers from 0 to 0.1, respectively.
[0020] b, d and f represent the valence of the metal X, the metal Y and the metal Z respectively. )
[0021] [8] The porous silica according to any one of [1] to [7], wherein the specific surface area is 500 m 2 / g or above.
[0022] [9] A powder deodorant for hair perms, comprising the porous silica described in [1] to [8].
[0023]
[10] A liquid deodorant comprising the porous silica according to any one of [1] to [8] and a solvent.
[0024]
[11] The liquid deodorant according to
[10] , wherein the pH is 6 to 11.
[0025]
[12] The liquid deodorant according to
[10] or
[11] , which is a deodorant for hair perming.
[0026]
[13] The liquid deodorant according to any one of
[10] to
[12] , which is a deodorant for sulfur-containing odors.
[0027]
[14] The liquid deodorant according to any one of
[10] to
[13] , further comprising a fragrance or a hair protecting component.
[0028]
[15] The liquid deodorant according to any one of
[10] to
[14] , wherein the solvent contains water.
[0029]
[16] The liquid deodorant according to any one of
[10] to
[15] , wherein the content of the porous silica is 0.001 to 50% by mass.
[0030]
[17] A method for producing a deodorant, comprising: a step of preparing porous silica having at least one metal X selected from the group consisting of Mn, Cu and Fe; and a step of mixing the porous silica with a solvent.
[0031] According to the present invention, a liquid deodorant and a method for producing the same are provided, which are capable of efficiently deodorizing sulfur-containing odors. DETAILED DESCRIPTION
[0032] The following describes an embodiment of the present invention. The deodorant according to the present embodiment includes a solvent and porous silica. The porous silica is dispersed in the solvent and contains at least one metal X selected from Mn, Cu and Fe. By adopting such a structure, sulfur-containing odor can be efficiently deodorized.
[0033] 1: Solvent
[0034] The solvent is not particularly limited as long as it does not dissolve the porous silica but disperses it. A liquid containing water as a main component (for example, 50% by mass or more) is preferably used as the solvent.
[0035] The pH of the solvent is preferably 6 to 11, more preferably 6 to 9. If the pH is 6 or higher, the metal will not be eluted from the porous silica. If the pH is 11 or lower, the porous silica will dissolve.
[0036] In addition, the solvent preferably has a low viscosity. If the solvent has a low viscosity, the sulfur-containing compound to be deodorized can be easily diffused into the pores of the porous silica, and the time required for deodorization can be shortened. The viscosity of the solvent is, for example, 0.5 to 100 mPa / sec at 25°C.
[0037] 2: Porous silica
[0038] The porous silica is dispersed in the solvent as described above. The content of the porous silica in the deodorant is, for example, 0.001 to 50% by mass, preferably 0.1 to 10% by mass. If the content of the porous silica is 0.001% by mass or more, a sufficient deodorizing effect can be obtained. If the content of the porous silica is 50% by mass or less, an effect of maintaining fluidity can be obtained.
[0039] The specific surface area of porous silica is, for example, 500 m 2 / g or more, preferably 800 to 2000 m 2 / g, more preferably 800 to 1600 m 2 / g. If the specific surface area of porous silica is 500m 2 / g or more, the contact area between the metal X contained in the porous silica and the odor to be deodorized can be sufficiently ensured, and a high deodorization efficiency can be obtained. 2 / g or less, the strength for maintaining the pore structure can also be ensured.
[0040] The size of the holes formed in the porous silica may be any size that allows the solvent molecules and the sulfur-containing compound molecules to enter and exit. For example, a hole diameter of 2 nm or more is sufficient.
[0041] The metal X contained in the porous silica has the function of adsorbing sulfur-containing compounds. The metal X is preferably doped in the porous silica. "Doping" means that the metal X enters the SiO 4 The state of the position of the Si element within the framework.
[0042] By doping the porous silica with metal X, the deodorization efficiency becomes higher than when the porous silica is not doped with metal X and exists in a granular form. When the metal X is doped, the metal X is spread over the entire surface of the porous silica. As a result, compared with the case where the metal X exists in a granular form, the contact area between the odor and the metal X becomes larger, and a high deodorization efficiency is obtained.
[0043] In addition, for example, when metal X is supported on porous silica in the form of a metal salt soluble in a solvent, when a deodorant is used, metal X will be dissolved into the solvent as metal ions. Therefore, it is sometimes necessary to implement a high-cost treatment such as ion exchange so that the metal ions do not flow out as drainage, and there is a situation where the burden required for drainage treatment is generated. In this regard, when metal X is doped with porous silica, metal X is prevented from detaching from the porous silica, so it can be easily separated and recovered in the form of powder by a precipitation device, which can reduce the burden on drainage treatment.
[0044] In addition, when the metal X is contained in the porous silica in a doped form, the odor of the metal X alone can be reduced.
[0045] The content of metal X in the porous silica is, for example, 0.01 to 10% by mass, preferably 0.1 to 5% by mass. If the content of metal X is 0.01% by mass or more, a sufficient deodorizing effect can be obtained. If it is 10% by mass or less, porous silica containing metal X can be easily synthesized.
[0046] As the metal X, Mn or Cu is preferably used from the viewpoint of deodorizing properties.
[0047] The porous silica preferably contains a metal different from the metal X.
[0048] Examples of the metal different from the metal X include metal Y for suppressing hydrolysis of porous silica. Examples of the metal Y include metals selected from Al and Zr. The metal Y is preferably doped in the porous silica.
[0049] The hydrothermal durability of porous silica can be improved by doping the porous silica with metal Y. The reason for this is believed to be that the doping with metal Y inhibits the hydrolysis of the siloxane skeleton of silica and makes the pore structure less likely to be destroyed.
[0050] The content of metal Y in the porous silica is, for example, 0.01 to 10% by mass, preferably 0.1 to 5% by mass. If the content of metal Y is 0.1% by mass or more, the effect of maintaining the specific surface area over time due to the inhibition of hydrolysis of the siloxane skeleton can be obtained. If it is 10% by mass or less, a specific surface area of 500 m 2 / g or more high specific surface area.
[0051] In addition, as a metal different from the metal X, a metal Z having a function of removing odors other than sulfur-containing odors may be contained in the porous silica. As the metal Z, for example, at least one metal selected from Co, Zn, Ag and Ca may be cited, and Co or the like may be preferably cited. When Co or the like is contained in the porous silica, not only sulfur-containing odors but also the decomposition of acetaldehyde and the deodorization of fatty acid odors can be expected, and porous silica that can eliminate multiple odors at once can be obtained.
[0052] The metal Z may be “doped” into the porous silica, or may be “supported on the porous silica as particles.” It is preferred that the metal Z be doped into the porous silica.
[0053] It should be noted that the phrase “supported on porous silica as particles” means a state in which the metal is supported by porous silica without being doped.
[0054] The content of the metal Z in the porous silica is, for example, 0.01 to 10 mass %, or preferably 0.1 to 5 mass %.
[0055] Specifically, it is preferred that at least a part of the porous silica has a chemical structure represented by Formula 1 below.
[0056] (Formula 1): SiO 2 aXO b / 2 ·cYO d / 2 ·eZO f / 2
[0057] In addition, in Formula 1, X represents a metal X.
[0058] Y represents metal Y.
[0059] Z represents metal Z.
[0060] a represents a number greater than 0 and less than 0.1.
[0061] c and e represent numbers ranging from 0 to 0.1, respectively.
[0062] b, d and f represent the valences of metal X, metal Y and metal Z, respectively.
[0063] It should be noted that since the porous silica is doped with metal X, metal Y or metal Z, a water-soluble metal salt containing metal X, metal Y or metal Z in an aqueous solution may be mixed with the porous silica or its precursor when the porous silica is manufactured. Whether the metal is doped can be confirmed by measuring the chemical bonding state by X-ray photoelectron spectroscopy or Raman spectroscopy.
[0064] The deodorant of this embodiment realizes the function of removing sulfur-containing odor in water by the doped metal X.
[0065] The sulfur-containing compound to be deodorized is not particularly limited as long as it is deodorized by the doped metal X, and examples thereof include cysteamine, thioglycolic acid, cysteine, thiazolidine, methyl mercaptan, tert-butyl mercaptan, and hydrogen sulfide.
[0066] Cysteamine, thioglycolic acid, cysteine, and the like are components contained in, for example, perm agents. Therefore, the deodorant according to the present embodiment is preferably used to remove the odor of cysteamine and the like attached to hair after a perm treatment.
[0067] Generally, in a perm treatment, hair is first rolled up in a curler. Then, a chemical called a perm preparation is applied to the hair. The perm preparation contains a reducing agent that cuts the cystine bonds of the hair. Specific examples of such a reducing agent include cysteamine, thioglycolic acid, and cysteine.
[0068] If the cystine bonds are cut, the hair will adapt to the shape of the curler.
[0069] Then, the second perm agent is applied to the hair. The second perm agent contains an oxidant. The cystine bonds that were cut are rebonded by the action of the oxidant. As a result, the shape of the hair is fixed in the shape of the curler.
[0070] The deodorant according to the present embodiment can be used as a component of the above-mentioned two perm agents, for example. Or it can be used as a drug applied to the hair separately from the two perm agents. For example, the deodorant according to the present embodiment can also be used in combination with a conditioner, hair gel, hair wax, etc. applied to the hair after the perm treatment.
[0071] The deodorant applied to the hair may or may not be rinsed off after the deodorizing function is exerted.
[0072] The deodorant may contain a fragrance or a hair protecting component. The fragrance or the hair protecting component is preferably present in a state of being contained in porous silica. In the case of containing the fragrance or the hair protecting component, if the hair is left standing after the deodorant is applied, the fragrance or the hair protecting component is slowly released. Thus, not only the deodorizing function of sulfur-containing odors can be achieved, but also other functions such as deodorizing body odor and scalp odor, and protecting hair can be achieved through the fragrance.
[0073] In order to contain a fragrance or a hair protection component in porous silica, there is a method of adding porous silica to a solution in which these components are dispersed, stirring the solution, and then removing the solvent by vacuum drying.
[0074] The deodorant according to the present embodiment is not necessarily used only for deodorizing hair after a perm treatment, but can also be used for other purposes. For example, water waste contains sulfur-containing odors. Therefore, the deodorant according to the present embodiment is also preferably used for deodorizing sprays for water waste.
[0075] As described above, according to the deodorant according to the present embodiment, since the porous silica doped with the metal X is dispersed in the solvent, it is possible to efficiently deodorize the sulfur-containing odor.
[0076] In particular, since porous silica is used, the metal X that exhibits a deodorizing function can be uniformly dispersed in the solvent, and as a result, the chemical reaction rate between the metal X and the sulfur-containing compound can be increased.
[0077] Furthermore, porous silica itself also has deodorizing performance against odors other than sulfur-containing odors (acidic and alkaline odors). Therefore, the deodorant according to the present embodiment can eliminate odors other than sulfur-containing odors.
[0078] In addition, porous silica easily adheres to hair. Therefore, when the deodorant according to the present embodiment is applied to hair, porous silica adheres to the hair. Thus, the deodorizing effect of metal X can be more reliably exerted.
[0079] 3: Manufacturing method
[0080] The deodorant according to the present embodiment can be obtained by producing porous silica and then dispersing the porous silica in a solvent.
[0081] In addition, porous silica can be produced by a method including the following steps, for example.
[0082] (A) a step of mixing a metal X doping compound containing a solvent, a surfactant, and a metal X to prepare a surfactant solution;
[0083] (B) adding a silica source to a surfactant solution to integrate micelles of the silica source on the surface;
[0084] (C) a step of condensing the integrated silica source;
[0085] (D) After the condensation step, the micelles are recovered and fired.
[0086] Each step is described below in detail.
[0087] (A): Preparation of surfactant solution
[0088] First, a surfactant and a compound for doping with metal X are added to a solvent to prepare a surfactant solution. The surfactant solution is preferably stirred at room temperature to 200° C. for 30 minutes to 10 hours. Thus, the surfactant forms micelles.
[0089] As the solvent, for example, water can be used. Alternatively, a mixture of water and an organic solvent such as ethanol or toluene can be used as the solvent.
[0090] The amount of the surfactant added is preferably 50 to 400 mmol / L, more preferably 50 to 150 mmol / L.
[0091] Alternatively, the amount of the surfactant added is 0.01 to 5.0 mol, preferably 0.05 to 1.0 mol, based on 1 mol of the silica source added later.
[0092] The surfactant is not particularly limited, and any of cationic, anionic, and nonionic surfactants may be used.
[0093] Preferably, the surfactant is neutral or cationic, and more preferably an alkylammonium salt. The alkylammonium salt preferably has 8 or more carbon atoms, and in view of the ease of industrial acquisition, more preferably has 12 to 18 carbon atoms. As the alkylammonium salt, hexadecyl trimethylammonium chloride, cetyl trimethylammonium bromide, stearyl trimethylammonium bromide, cetyl trimethylammonium chloride, stearyl trimethylammonium chloride, dodecyl trimethylammonium bromide, octadecyl trimethylammonium bromide, dodecyl trimethylammonium chloride, octadecyl trimethylammonium chloride, behenyl dimethylammonium bromide, tetradecyl dimethylammonium bromide, behenyl dimethylammonium chloride, tetradecyl dimethylammonium chloride, etc. can be cited. These surfactants can be used alone, and can also be used in combination of two or more.
[0094] The metal X doping compound is a substance that serves as a supply source of the metal X doped into the porous silica. As the metal X doping compound, a water-soluble compound containing the metal X is preferably used. More preferably, a chloride, nitrate, sulfate, or the like of the metal X is used.
[0095] For example, when the metal X is iron, iron (III) chloride or the like is added as a compound for doping the metal X.
[0096] For example, when the metal X is copper, copper (II) nitrate or the like is added as a compound for doping the metal X.
[0097] For example, when the metal X is manganese, manganese (II) chloride or the like is added as a compound for doping the metal X.
[0098] The metal X doping compound may be used alone or in combination of two or more.
[0099] The amount of the metal X doping compound added is, for example, 0.001 to 0.5 mol, preferably 0.01 to 0.1 mol, relative to 1 mol of the silica source.
[0100] (B): Addition of silica source
[0101] Next, a silica source is added to the surfactant solution.
[0102] The silicon dioxide source is not particularly limited if it is a raw material for silicon dioxide, and examples thereof include silicon oxynitride film, tetramethoxysilane, tetra-n-butoxysilane, and sodium silicate. These silicon dioxide sources can be used alone or in combination of two or more. The silicon dioxide source is preferably an alkoxysilane. The silicon dioxide source is more preferably a silicon oxynitride film. The organic functional groups on the silicon atoms are lost due to hydrolysis, and therefore do not affect the structure of the synthesized product. Among them, if the organic functional groups are large, the hydrolysis rate slows down and the synthesis time becomes longer.
[0103] When sodium silicate is used alone or in combination as a silica source, the surfactant solution is heated under reflux at 200° C. or lower for 20 to 2 hours.
[0104] The amount of the silica source added is not particularly limited, and is, for example, 0.2 to 1.8 mol / L. Alternatively, when the solvent contains water, the concentration of the silica source is, for example, 0.001 to 0.05 mol per mol of water.
[0105] (C): Condensation of silica source
[0106] Next, the silica source is condensed. Specifically, the pH of the solution is increased or decreased until the silica source condenses. For example, the silica source can be condensed by adding an alkaline aqueous solution and stirring. The stirring is performed for, for example, more than 1 hour. By adding an alkaline aqueous solution, the silica source integrated on the surface of the micelle undergoes dehydration condensation to form a silica wall.
[0107] As the alkaline aqueous solution, aqueous solutions of sodium hydroxide, sodium carbonate, ammonia, etc. can be cited. The alkaline aqueous solution is preferably an aqueous sodium hydroxide solution. These alkaline aqueous solutions can be used alone or in combination of two or more. The alkaline aqueous solution preferably has a pH of 8 to 14 after addition, and more preferably 9 to 11. The addition of the alkaline aqueous solution accelerates the dehydration condensation reaction of the silica source.
[0108] As a result, the surface tension of the condensed part increases, the wall of the silica becomes spherical, and the spheres become multi-layered, leading to spinodal decomposition (phase separation). These structures are frozen by chemical crosslinking.
[0109] It should be noted that the silica source has a property of condensing even in a low pH state. Therefore, the silica source can be condensed by adding not only an alkaline aqueous solution but also an acidic aqueous solution.
[0110] (D): Recovery and sintering of micelles
[0111] Next, micelles are recovered from the aqueous solution as a precursor. Specifically, if the silica source is condensed, micelles are precipitated. Therefore, by filtering out the precipitate, micelles are recovered as a precursor. The recovered precursor is dried. After drying, the precursor is fired to remove the organic components contained in the precursor. That is, the surfactant constituting the micelles is removed. Thus, porous silica having pores is formed. It should be noted that firing is performed above the decomposition temperature of the surfactant. The firing temperature is, for example, 400 to 600°C.
[0112] The porous silica obtained by the above method is doped with the metal X derived from the compound for doping with the metal X. That is, porous silica doped with the metal X is obtained.
[0113] It should be noted that in the above method, an example in which the metal X doping compound is added in step (A) is described. The metal X doping compound does not have to be added in step (A), and can be added to the solution at any stage before the firing in step (D). In the solution, if the integrated silica source is mixed with the metal X doping compound, the metal X from the metal X doping compound is taken up by the silica source, and porous silica doped with metal X can be obtained.
[0114] When producing porous silica containing metal Y and / or metal Z in addition to metal X, a metal Y doping compound or a metal Z supplying compound may be added at any stage before step (D).
[0115] The metal Y doping compound and the metal Z supplying compound are substances that serve as supply sources of metal Y and metal Z, respectively. As the metal Y doping compound and the metal Z supplying compound, water-soluble compounds containing metal Y or Z are preferably used. More preferably, chlorides, nitrates, sulfates, and the like of metal Y or metal Z are used.
[0116] For example, when the metal Y is aluminum, aluminum chloride or the like is added as a compound for doping the metal Y.
[0117] For example, when the metal Y is Zr, zirconium oxide chloride or the like is added as a compound for doping the metal Y.
[0118] For example, when the metal Z is cobalt, cobalt nitrate or the like is added as a compound for supplying the metal Z.
[0119] For example, when the metal Z is Zn, zinc nitrate or the like is added as a compound for supplying the metal Z.
[0120] For example, when the metal Z is Ag, silver nitrate or the like is added as a compound for supplying the metal Z.
[0121] For example, when the metal Z is Ca, calcium carbonate or the like is added as a compound for supplying the metal Z.
[0122] The metal Y doping compound and the metal Z supplying compound may be used alone or in combination of two or more.
[0123] The addition amount of the metal Y doping compound and the metal Z supplying compound is, for example, 0.001 to 0.5 mol, preferably 0.01 to 0.1 mol, respectively, relative to 1 mol of the silica source.
[0124] (Example)
[0125] Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.
[0126] Deodorants according to Examples 1 to 8 and Comparative Examples 1 to 6 were prepared. The specific surface area, metal content, and cysteamine adsorption amount of the obtained deodorants were measured. The preparation method and measurement method of each example and comparative example are as follows.
[0127] Example 1
[0128] Hexadecyltrimethylammonium chloride as a surfactant, magnesium chloride as a metal X doping compound, and aluminum chloride as a metal Y doping compound were added to water as a solvent, and stirred at 100°C for 1 hour. After the aqueous solution was cooled to room temperature, a silicon oxynitride film as a silicon dioxide source was added and stirred. Next, sodium hydroxide was added as a condensation catalyst and stirred. The amount of each compound added was the following amount relative to 1 mol of the silicon oxynitride film.
[0129] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0130] Metal X doping compound (manganese chloride): 0.0118 mol
[0131] Metal Y doping compound (aluminum chloride): 0.0482 mol
[0132] Water: 125 mol
[0133] Sodium hydroxide: 0.195 mol
[0134] The solid product was filtered from the obtained suspension, dried, and then calcined to remove the organic components, thereby obtaining porous silica.
[0135] Example 2
[0136] Before adding the silicon dioxide source, cobalt nitrate was further added as a compound for supplying metal Z. The addition amount of each compound was set to the following amount per 1 mol of the silicon oxynitride film.
[0137] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0138] Metal X doping compound (manganese chloride): 0.0118 mol
[0139] Metal Y doping compound (aluminum chloride): 0.0241 mol
[0140] Metal Z supplying compound (cobalt nitrate): 0.011 mol
[0141] Water: 125 mol
[0142] Sodium hydroxide: 0.195 mol
[0143] The deodorant according to Example 2 was prepared in the same manner as in Example 1 with respect to other points.
[0144] Example 3
[0145] Copper nitrate was used as the compound for doping with the metal X. The addition amount of each compound was set to the following amount per 1 mol of the silicon oxynitride film.
[0146] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0147] Metal X doping compound (copper nitrate): 0.0204 mol
[0148] Metal Y doping compound (aluminum chloride): 0.0482 mol
[0149] Water: 125 mol
[0150] Sodium hydroxide: 0.195 mol
[0151] The deodorant according to Example 3 was prepared in the same manner as in Example 1 with respect to other points.
[0152] Example 4
[0153] Copper nitrate was used as the compound for doping metal X. Aluminum chloride and zirconium oxychloride were used as the compound for doping metal Y. Cobalt nitrate was added as the compound for supplying metal Z. The addition amount of each compound was set to the following amount per 1 mol of the silicon oxynitride film.
[0154] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0155] Metal X doping compound (copper nitrate): 0.0102 mol
[0156] Metal Y doping compound (aluminum chloride): 0.0478 mol
[0157] Metal Y doping compound (zirconium oxide chloride): 0.021 mol
[0158] Metal Z supplying compound (cobalt nitrate): 0.0116 mol
[0159] Water: 125 mol
[0160] Sodium hydroxide: 0.282 mol
[0161] A deodorant according to Example 4 was prepared in the same manner as in Example 1 with respect to other points.
[0162] Example 5
[0163] Copper nitrate was used as a compound for doping with metal X. Aluminum chloride and zirconium chloride oxide were added as compounds for doping with metal Y. The addition amount of each compound was set to the following amount per mol of the silicon oxynitride film.
[0164] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0165] Metal X doping compound (copper nitrate): 0.0102 mol
[0166] Metal Y doping compound (aluminum chloride): 0.0498 mol
[0167] Metal Y doping compound (zirconium oxide chloride): 0.022 mol
[0168] Water: 125 mol
[0169] Sodium hydroxide: 0.282 mol
[0170] A deodorant according to Example 5 was prepared in the same manner as in Example 1 with respect to other points.
[0171] Example 6
[0172] Ferric chloride was added as a compound for doping with metal X. The addition amount of each compound was set to the following amount per 1 mol of the silicon oxynitride film.
[0173] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0174] Metal X doping compound (ferric chloride): 0.0537 mol
[0175] Metal Y doping compound (aluminum chloride): 0.0241 mol
[0176] Water: 125 mol
[0177] Sodium hydroxide: 0.195 mol
[0178] A deodorant according to Example 6 was prepared in the same manner as in Example 1 with respect to other points.
[0179] Example 7
[0180] Manganese oxide was added as a compound for doping with metal X. No compound for doping with metal Y was added. The amount of each compound added was set to the following amount per mol of the silicon oxynitride film.
[0181] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0182] Metal X doping compound (manganese oxide): 0.0118 mol
[0183] Water: 125 mol
[0184] Sodium hydroxide: 0.195 mol
[0185] A deodorant according to Example 7 was prepared in the same manner as in Example 1 with respect to other points.
[0186] Example 8
[0187] No surfactant and metal Y doping compound were added. Copper nitrate was used as the metal X doping compound. Nitric acid was used as the condensation catalyst. The addition amount of each compound was set to the following amount per mol of the silicon oxynitride film.
[0188] Metal X doping compound (copper nitrate): 0.0102 mol
[0189] Water: 10 mol
[0190] Nitric acid: 0.1 mol
[0191] A deodorant according to Example 8 was prepared in the same manner as in Example 1 with respect to other points.
[0192] Comparative Example 1
[0193] For Comparative Example 1, manganese (IV) oxide powder manufactured by Wako Pure Chemical Industries, Ltd. (Wako Grade 1, Catalog code 138-09675) was prepared.
[0194] Comparative Example 2
[0195] Cobalt chloride and manganese nitrate were dissolved in water at a molar ratio of 1:1, heated at 100° C. to volatilize water, and then calcined at 570° C. for 5 hours to obtain a powder, which was used in Comparative Example 2.
[0196] Comparative Example 3
[0197] A copper nanoparticle reagent (Catalog code 794317) manufactured by Sigma-Aldrich was prepared and used in Comparative Example 3.
[0198] Comparative Example 4
[0199] Ferric chloride was fired at 500° C. for 5 hours to obtain a powder, which was used in Comparative Example 4.
[0200] Comparative Example 5
[0201] Mesoporous silica MCM-41 (Catalog code 643645) manufactured by Sigma-Aldrich was prepared and used in Comparative Example 5.
[0202] Comparative Example 6
[0203] No metal X doping compound was added. Aluminum chloride and zirconium oxychloride were added as metal Y doping compounds. Cobalt nitrate was added as a metal Z supplying compound. The addition amount of each compound was set to the following amount per 1 mol of the silicon oxynitride film.
[0204] Surfactant (hexadecyltrimethylammonium chloride): 0.225 mol
[0205] Metal Y doping compound (aluminum chloride): 0.0478 mol
[0206] Metal Y doping compound (zirconium oxide chloride): 0.035 mol
[0207] Metal Z supplying compound (cobalt nitrate): 0.0231 mol
[0208] Water: 125 mol
[0209] Sodium hydroxide: 0.282 mol
[0210] The deodorant according to Comparative Example 6 was prepared in the same manner as in Example 1 with respect to other points.
[0211] Determination method of specific surface area
[0212] The measurement was performed at the liquid nitrogen temperature by a single-point method using FlowSorb II 2300 manufactured by Micromeritics.
[0213] Determination of the content of metal X and metal Y
[0214] About 50 mg of the deodorant involved in the embodiment or comparative example was accurately weighed, dissolved in 4 ml of hydrochloric acid, and the concentration of each metal (Mn, Cu, Fe, Al, Co, and Zr) in the aqueous solution was measured under ICP-OES manufactured by Thermo Scientific. By treating with hydrochloric acid, all the metal components contained in the deodorant were dissolved in hydrochloric acid. Therefore, based on the measurement results, the content of each metal present in the deodorant was calculated as the metal content.
[0215] Cysteamine adsorption test
[0216] 0.5896 g of cysteamine was weighed and weighed with ultrapure water using a 10 ml volumetric flask to obtain a solution 1-1. The cysteamine concentration in the solution 1-1 was 5.85 wt %, which was a concentration equivalent to that of a perm solution.
[0217] Measure 10 mg of the deodorant to be measured in a centrifuge test tube. Add 0.9 ml of water to the tube and shake it evenly to obtain a uniform dispersion. Add 0.1 ml of solution 1-1 to the dispersion and shake it for 30 seconds to react. The cysteamine concentration before the reaction is 7.64×10 -2 mol / L, the initial cysteamine amount was 5.89 mg. The centrifugal separation was performed for 90 seconds. The supernatant was weighed promptly and the absorbance of the reaction solution at 235 nm was measured.
[0218] According to the determination of the standard curve, when the cysteamine concentration was 7.5×10 -4 mol / L~1.2×10 -4 In the range of mol / L, it is confirmed that the absorbance at 235nm is proportional to the cysteamine concentration. Therefore, in a manner located in this concentration range, the reaction solution is appropriately diluted using an automatic pipette and the absorbance at 235nm is measured. As a result, the residual concentration of cysteamine is calculated by the following formula 1. In addition, the value of the adsorption rate is calculated using the following formula 2.
[0219] (Formula 1) Residual concentration = constant × absorbance at 235 nm × dilution ratio
[0220] (Formula 2) Adsorption rate (%) = (initial concentration - residual concentration) / initial concentration × 100
[0221] Furthermore, the capacity and the like were calculated according to the following formulas 3 to 5.
[0222] (Formula 3) Adsorption amount (mg) = adsorption rate (%) × initial cysteamine amount (mg) / 100
[0223] (Formula 4) Metal X amount (mg) = deodorant dosage (mg) × metal X metal amount (wt%) / 100
[0224] (Formula 5) Capacity (mg / metal X mg) = adsorption amount (mg) / metal X amount (mg)
[0225] In addition, as an absorbance measuring device, the following device was used.
[0226] Absorbance measuring device: Corona absorption grating microplate reader SH-1000 (manufactured by Corona Electric Co., Ltd.), metal plate: UV Flat Bottom Microtite (registered trademark) Plates (manufactured by Thermo), measuring range: 200 to 600 nm, response: 3
[0227] Tables 1 and 2 show the measurement results.
[0228] As shown in Tables 1 and 2, the deodorants according to Examples 1 to 7 have a higher cysteamine adsorption rate than the deodorant according to Comparative Example 6. Thus, the cysteamine adsorption performance is improved by containing the metal X in the porous silica.
[0229] In addition, the deodorants according to Examples 1 to 8 have a higher capacity for cysteamine adsorption than the deodorants according to Comparative Examples 1 to 4 that do not use porous silica. Therefore, by including metal X in porous silica, the deodorizing ability of metal X per unit mass is improved compared to the case of directly using metal X. That is, by including metal X in porous silica, it is possible to achieve a deodorizing ability equal to or higher than that of metal X using a small amount of metal X.
[0230] Furthermore, the deodorants according to Examples 1 to 7 had a higher cysteamine adsorption rate than the deodorant according to Example 8. This shows that a higher specific surface area can provide a higher cysteamine adsorption rate.
[0231] In addition, Examples 1 and 3 have higher cysteamine adsorption capabilities (rate and capacity) than Example 6. Therefore, it is determined that Mn and Cu are particularly preferable as the metal X.
[0232]
[0233]
Claims
1. A liquid deodorant comprising the following porous silica and a solvent, wherein the porous silica is doped with a metal X, wherein the metal X comprises Cu, Furthermore, the porous silica includes a metal Y different from the metal X, and the metal Y includes Al. 2 . The liquid deodorant according to claim 1 , wherein the porous silica further comprises a metal Z selected from the group consisting of Co, Zn, Ag and Ca.
3. The liquid deodorant according to claim 1 or 2, wherein The specific surface area is 500m 2 / g or above.
4. The liquid deodorant according to claim 1 or 2, wherein The pH is 6-11.
5. The liquid deodorant according to claim 1 or 2, which is a deodorant for hair perming treatment.
6. The liquid deodorant according to claim 1 or 2, which is a deodorant for sulfur-containing odors.
7. The liquid deodorant according to claim 1 or 2, wherein It may further contain fragrance or hair protection ingredients.
8. The liquid deodorant according to claim 1 or 2, wherein Water is included as the solvent.
9. The liquid deodorant according to claim 1 or 2, wherein The content of the porous silica is 0.001 to 50 mass %.
10. A method for producing a liquid deodorant, the method for producing a liquid deodorant according to any one of claims 1 to 9, comprising: A process for preparing the porous silica; and A step of mixing the porous silica with the solvent.