Method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion

Through the combination of simulation experiments and comprehensive evaluation indicators, the problem of difficulty in evaluating the resistance of water vapor oxidation and erosion of blast furnace refractory materials in the existing technology is solved, a scientific and reasonable evaluation system is established, and the long-lived production of blast furnace cylinders is guided.

CN114993922BActive Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210537984.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-11-15
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

The existing technology lacks a clear and scientific and reasonable method to evaluate the oxidative corrosion resistance of blast furnace refractories, and traditional methods are difficult to comprehensively and accurately reflect the oxidative corrosion of furnace refractories in actual applications.

Method used

A simulation experimental method is used to determine relevant parameters based on actual production conditions, and a comprehensive evaluation system for blast furnace refractory materials resisting water vapor oxidation corrosion performance is established by calculating the erosion rate, mass change rate, volume change rate, erosion degree and micromorphic change characteristics.

Benefits of technology

A comprehensive and accurate assessment of the anti-oxidation and erosion properties of blast furnace refractory materials has been achieved, and scientific and reasonable evaluation indicators are provided, which can guide the production practice of blast furnace furnace cylinders for longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114993922B_ABST
    Figure CN114993922B_ABST
Patent Text Reader

Abstract

The present invention provides a method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials. The method of simulation experiment is adopted to determine the experimental related parameters according to the actual production conditions, and the simulation experiment is carried out to obtain a series of data of water vapor oxidation erosion of refractory materials; the erosion rate is calculated by using a limited formula, and it is combined with indicators such as mass change rate, volume change rate, erosion degree, microscopic morphology change characteristics, etc., to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and the water vapor oxidation erosion resistance of blast furnace refractory materials is comprehensively evaluated. The method of the present invention is simple, the experimental success rate is high, and the evaluation indicators obtained are comprehensive and accurate; the definition of erosion rate is introduced when evaluating the water vapor oxidation erosion resistance of refractory materials, and an accurate calculation method is given. The indicator is scientific and reasonable, with high accuracy, and is consistent with the actual erosion situation of blast furnace hearth refractory materials, providing a guiding basis for the long-life production practice of blast furnace hearths.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace smelting, and in particular to a method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials. Background Art

[0002] Modern blast furnaces are developing towards large-scale furnace capacity and efficient production. Whether the life of blast furnaces can be extended has a huge impact on the normal production order and overall economic benefits of steel enterprises. The longevity of blast furnaces means improved economic benefits. In recent years, with the development of blast furnace smelting technology, the application of new equipment, the improvement of operating level and the change of blast furnace design concept, the limiting factor of blast furnace life has shifted to the blast furnace hearth. The blast furnace hearth is a structural area of ​​the blast furnace, generally referring to the furnace body between the center line of the first exhaust port and the furnace bottom. Regardless of the hearth structure, refractory materials are an important component. As a high-temperature and high-pressure reaction vessel, the hearth undertakes tasks such as direct reduction reaction, high-temperature melting, and frequent slag and iron operations. It is subjected to severe high-temperature reactions, scouring and erosion damage. And because it cannot be repaired and relined during the repair, the hearth safety has become a key link in limiting the life of a generation of blast furnaces.

[0003] The investigation found that a lot of accumulated water is often discharged from the inner side of the furnace shell of the blast furnace in production, such as the temperature detection holes and grouting holes. Analysis found that the main sources of water accumulation in the furnace shell are: 1) damage and leakage of the furnace cooler or the tuyere sleeve; 2) supersaturated water in the upper gas condenses on the furnace shell and leaks along the furnace shell to the furnace shell; 3) cold air humidification condenses on the tuyere sleeve and then penetrates to the cold end along the buffer layer; 4) water evaporated during the drying process before the blast furnace is started condenses and enters the furnace shell; 5) water brought in by amorphous materials during the grouting process of the furnace shell. Since the hearth is at the lowest position of the whole furnace, when the cooler in the tuyere and above area leaks, the leaked water will seep into the hearth along the gap between the furnace shell and the cooler due to gravity; the supersaturated water formed on the top of the furnace will condense under the action of the lower temperature and pressure change of the furnace shell, and will also seep into the hearth along the furnace shell; the cooling wall temperature at the hearth is the lowest in the whole furnace, and water vapor in other areas flows to the hearth with the coal gas, condenses and precipitates after encountering the low-temperature cooler, and gathers into water. The accumulation of water vapor in the blast furnace hearth will aggravate the oxidation erosion of carbon-containing refractory materials, causing damage to the hearth, posing a great threat to the longevity of the hearth. Therefore, the study of the resistance of refractory materials in the blast furnace hearth to water vapor oxidation erosion is of great significance to the life of the blast furnace.

[0004] However, there is little research on how to evaluate the resistance of blast furnace refractory materials to water vapor oxidation corrosion. There is no clear, scientific and reasonable evaluation system for blast furnace refractory materials to water vapor oxidation corrosion. The traditional evaluation method that only uses a single mass and volume change is difficult to fully and accurately reflect the oxidation corrosion of furnace hearth refractory materials in actual applications.

[0005] In view of this, it is necessary to design an improved method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion to solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials. The method of simulation experiment is adopted to determine the relevant parameters of the simulation experiment according to the actual production conditions, and a series of data of water vapor oxidation erosion refractory material samples are obtained; the erosion rate of the sample is calculated by a limited formula, and it is combined with the indicators of mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and a comprehensive evaluation is performed on the water vapor oxidation erosion resistance of blast furnace refractory materials.

[0007] To achieve the above-mentioned object of the invention, the present invention provides a method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials, which adopts a simulation experiment method to evaluate the water vapor oxidation erosion resistance of blast furnace refractory materials, comprising the following steps:

[0008] S1. Making a cylindrical refractory material sample from an actual blast furnace hearth refractory material, and pretreating the cylindrical refractory material sample to obtain a pretreated refractory material sample; the ratio of the diameter to the height of the refractory material sample is (2.0-6.5):1;

[0009] S2, placing the refractory material sample pretreated in step S1 in a crucible, placing the crucible in a heating device, and connecting it to a weighing system of the heating device to record the mass change of the refractory material sample in real time; the heating device is also provided with an image acquisition system to record the morphology change of the refractory material sample in real time;

[0010] S3, determining relevant parameters of the simulation experiment according to actual production conditions; performing a simulation experiment of the refractory material sample according to the relevant parameters, and introducing a mixed gas containing water vapor and its carrier gas into the heating device for reaction throughout the experiment;

[0011] S4. After the simulation experiment is completed, data on the refractory material sample is obtained, including the mass change data and the morphology change data of the refractory material sample, and the data are processed; and the erosion rate of the refractory material sample by water vapor is calculated using the following formula:

[0012]

[0013] Where v is the erosion rate of the refractory sample, g / (h·mm 2 );ρ is the density of refractory material, g / cm 3;w c is the carbon content of the refractory material, %; h1 is the height of the refractory material sample before the experiment, mm; d1 is the diameter of the refractory material sample before the experiment, mm; d2 is the diameter of the refractory material sample after the experiment, mm; t is the reaction time of the simulation experiment, h;

[0014] S5. Combining the erosion rate of the refractory material sample obtained in step S4 with the indicators of mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the refractory material, obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and conduct a comprehensive evaluation of the water vapor oxidation erosion resistance of blast furnace refractory materials.

[0015] As a further improvement of the present invention, in step S4, processing the data of the refractory material sample includes: calculating the mass change rate of the refractory material sample according to the mass change data, and obtaining the size change of the refractory material sample according to the morphology change data; and calculating the volume change rate and erosion degree of the refractory material sample according to the size change.

[0016] As a further improvement of the present invention, in step S3, the relevant parameters include reaction temperature, reaction time, and the content of water vapor in the mixed gas.

[0017] As a further improvement of the present invention, in step S3, the temperature of the mixed gas introduced into the heating device is above 100°C, and the flow rate of the mixed gas is 200-800 mL / min.

[0018] As a further improvement of the present invention, the refractory material is a carbon-containing refractory material; the carrier gas type of the water vapor includes an inert gas; and the carrier gas needs to be purified by a purification system before mixing with the water vapor to remove O2, moisture and CO2 impurities therein.

[0019] As a further improvement of the present invention, in step S5, the calculation formula of the erosion degree is as follows:

[0020]

[0021] Wherein, Δd is the erosion degree of the refractory sample, mm / h; t is the reaction time of the simulation experiment, h; d1 is the diameter of the refractory sample before the experiment, mm; d2 is the diameter of the refractory sample after the experiment, mm.

[0022] As a further improvement of the present invention, in step S3, the method for preparing the mixed gas is: using an injection pump to inject deionized water into a mixing tank, mixing and heating it with the carrier gas injected therein to obtain the mixed gas; the percentage of water vapor in the mixed gas is 0 to 100%.

[0023] As a further improvement of the present invention, the injection speed of the deionized water is 0.1-1500 mL / h; the heating temperature is 300-400°C.

[0024] As a further improvement of the present invention, the water vapor content in the mixed gas in step S3 is set to different gradients, and repeated simulation experiments are performed to obtain a curve of the influence of the change in water vapor content on the erosion rate of the refractory sample.

[0025] As a further improvement of the present invention, in step S1, the pretreatment includes grinding, polishing, and alcohol cleaning the surface of the refractory material sample, and drying it.

[0026] As a further improvement of the present invention, the heating device includes: a high-temperature energy-saving vertical tube furnace, a precision temperature controller, a computer acquisition system, a weighing system and an image acquisition system; the precision temperature controller adjusts the temperature of the high-temperature energy-saving vertical tube furnace, and the data collected by the weighing system and the image acquisition system are fed back to the computer acquisition system.

[0027] The beneficial effects of the present invention are:

[0028] 1. A method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials of the present invention adopts a simulation experiment method to establish an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials. Determine the relevant parameters of the simulation experiment according to the actual production conditions, and conduct a simulation experiment to obtain a series of data on the water vapor oxidation erosion of refractory samples; use a limited formula to calculate the erosion rate of the refractory samples, and combine it with the indicators of the mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the refractory materials to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and conduct a comprehensive evaluation of the water vapor oxidation erosion resistance of blast furnace refractory materials. The method is simple and easy to operate, has a high experimental success rate, and has comprehensive and accurate evaluation indicators, which can provide a guiding basis for the longevity of the blast furnace hearth.

[0029] 2. When evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials, the present invention introduces the definition of erosion rate and provides an accurate calculation method; the calculation method utilizes the important relationship between the water vapor oxidation erosion resistance of refractory materials and the loss of carbon content in the refractory materials, the reaction contact area, and the reaction time, and further deduces and verifies that the evaluation index is scientific and reasonable, has high accuracy, and is consistent with the actual erosion conditions of blast furnace hearth refractory materials. Using erosion rate to characterize the water vapor oxidation resistance of refractory materials can better simulate the changes in the thickness of refractory materials in the blast furnace hearth and bottom with temperature, time, and water vapor content in actual production, while the traditional single use of volume or mass changes cannot well characterize the changes in furnace lining thickness. The present invention can intuitively compare the advantages and disadvantages of the water vapor oxidation resistance of different refractory materials through the calculation of the water vapor oxidation erosion resistance rate of refractory materials, and has the advantages of being simple, effective, accurate, and reasonable.

[0030] 3. The present invention establishes an evaluation system for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials, combines a series of indicators such as mass change rate, volume change rate, erosion degree, erosion rate, and microscopic morphology change characteristics, and obtains a more systematic and accurate evaluation standard. The simulation experimental method adopted is close to the actual working conditions of blast furnace hearth refractory materials, and takes into account the influence of relevant parameters such as water vapor content and temperature on the erosion of blast furnace refractory materials. It can more systematically and accurately evaluate the water vapor oxidation erosion resistance of blast furnace refractory materials, reveal the influence mechanism of water vapor on blast furnace hearth refractory materials, provide a reference for the rational selection of blast furnace refractory materials and the reduction of water vapor oxidation erosion, and provide a guiding basis for the long-life production practice of blast furnace hearths. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 These are electron microscope images of carbon composite bricks before and after the experiment of Example 1 of the present invention (a is before the experiment, b is after the experiment).

[0032] Figure 2 The following is a schematic diagram of the device used in the simulation test of the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0035] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0036] A method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials, using a simulation experiment method to evaluate the water vapor oxidation erosion resistance of blast furnace refractory materials, comprising the following steps:

[0037] S1. The actual refractory material for the blast furnace hearth is made into a cylindrical refractory material sample, and the refractory material is pretreated to obtain the pretreated refractory material sample; the ratio of the diameter to the height of the refractory material sample is (2.0-6.5):1; wherein the pretreatment includes grinding, polishing, and alcohol cleaning the surface of the refractory material sample, and drying it; the cylindrical sample with a diameter to height ratio within this range is used, the shape of the cylindrical sample is uniform, the rate of water vapor oxidation erosion in all directions is more uniform, and the calculated erosion rate result is less accidental and more accurate;

[0038] S2, placing the refractory material sample pretreated in step S1 in a crucible, placing the crucible in a heating device, and connecting it to a weighing system of the heating device to record the mass change of the refractory material sample in real time; the heating device is also provided with an image acquisition system to record the morphological change of the refractory material sample in real time;

[0039] S3. Determine relevant parameters of the simulation experiment according to actual production conditions; conduct a simulation experiment of the refractory material sample according to the relevant parameters, and introduce a mixed gas containing water vapor and its carrier gas into the heating device for reaction throughout the experiment;

[0040] S4. After the simulation experiment is completed, data on the refractory sample is obtained, including the mass change data and morphology change data of the refractory sample, and the data are processed; and the erosion rate of the refractory sample by water vapor is calculated using the following formula:

[0041]

[0042] Where v is the erosion rate of the refractory sample, g / (h·mm 2 );ρ is the density of refractory material, g / cm 3 ;w c is the carbon content of the refractory material, %; h1 is the height of the refractory material sample before the experiment, mm; d1 is the diameter of the refractory material sample before the experiment, mm; d2 is the diameter of the refractory material sample after the experiment, mm; t is the reaction time of the simulation experiment, h;

[0043] Among them, the calculation method of erosion rate uses the important relationship between the resistance of refractory materials to water vapor oxidation erosion and the loss of carbon content in the refractory materials, the reaction contact area, and the reaction time. It is further deduced and verified that the evaluation index is scientific and reasonable, with high accuracy, and consistent with the actual erosion of blast furnace hearth refractory materials;

[0044] S5. Combine the erosion rate of the refractory sample obtained in step S4 with the indicators of mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the refractory to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory, and conduct a comprehensive evaluation of the water vapor oxidation erosion resistance of blast furnace refractory.

[0045] The present invention uses erosion rate to characterize the water vapor oxidation resistance of refractory materials, which can better simulate the change of refractory material thickness over time in actual production of blast furnace hearth and furnace bottom, while the traditional single use of volume or mass change cannot well characterize the change of furnace lining thickness. By calculating the water vapor oxidation resistance erosion rate of refractory materials, the advantages and disadvantages of water vapor oxidation resistance of different refractory materials can be intuitively compared, which has the advantages of being simple, effective, accurate and reasonable. The established evaluation system for the water vapor oxidation resistance erosion performance of blast furnace refractory materials combines a series of indicators such as mass change rate, volume change rate, erosion degree, erosion rate, and microscopic morphology change characteristics to obtain a more systematic and accurate evaluation standard.

[0046] Specifically, in step S4, the relevant parameters include reaction temperature, reaction time, and the content of water vapor in the mixed gas. The temperature of the mixed gas introduced into the heating device is above 100°C, and the flow rate of the mixed gas is 200-800mL / min. The refractory material is a carbon-containing refractory material, including carbon bricks, carbon composite bricks, etc. The types of carrier gas for water vapor include inert gases. When studying the effect of water vapor on the oxidative corrosion of refractory materials, the type of carrier gas needs to be inert gas; the inert gas carrier gas needs to be purified by a gas purification system before entering the mixing tank, and its flow rate is controlled by a mass flow meter.

[0047] In a specific embodiment, the gas purification system includes: soda lime, Mg(ClO4)2, H2SO4 and Mg(500℃) devices, wherein Mg(500℃) is used to remove O2 impurities in the carrier gas, Mg(ClO4)2 and H2SO4 are used to remove moisture in the carrier gas, and soda lime is used to remove CO2 in the carrier gas to prevent O2, moisture and CO2 impurities in the carrier gas from affecting the results of the simulation experiment.

[0048] In a specific embodiment, the method and the device used in the present invention can also be used to study the influence of other gases on the oxidation corrosion performance of furnace hearth refractory materials, by replacing water vapor with the gas to be studied.

[0049] In particular, in step S4, processing the data of the refractory material sample includes: calculating the mass change rate of the refractory material sample according to the mass change data, obtaining the size change of the refractory material sample according to the morphology change data; and calculating the volume change rate and erosion degree of the refractory material sample according to the size change. The calculation formula of the mass change rate is as follows:

[0050]

[0051] Where, η is the mass change rate, %;

[0052] m1—mass of refractory material before testing, g;

[0053] m2—mass of refractory material after testing, g;

[0054] The volume change rate is calculated as follows:

[0055]

[0056] Where, λ—volume change rate, %;

[0057] d1—diameter of refractory material before test, mm;

[0058] d2—diameter of refractory material after testing, mm;

[0059] h1—height of refractory material before test, mm;

[0060] h2—height of refractory material after testing, mm.

[0061] The calculation formula of erosion degree is as follows:

[0062]

[0063] Where, Δd is the erosion rate of the refractory sample, mm / h;

[0064] t is the reaction time of the simulation experiment, h;

[0065] d1 is the diameter of the refractory sample before the experiment, mm;

[0066] d2 is the diameter of the refractory sample after the test, mm.

[0067] Specifically, the preparation method of the mixed gas is: deionized water is injected into the mixing tank by using an injection pump, and mixed and heated with the carrier gas injected therein to obtain a mixed gas; the percentage of water vapor in the mixed gas is 0 to 100%. Among them, the injection speed of deionized water is 0.1 to 1500 mL / h; the heating temperature is 300 to 400°C. After the deionized water and the carrier gas are mixed, the mixing tank is placed in a small heating furnace, and the temperature of the mixing tank is controlled at above 300°C using a simple temperature control box to ensure that the liquid deionized water can be completely vaporized in the mixing tank and mixed evenly with the carrier gas. The mixed gas containing water vapor enters the heating device through a silicone tube wrapped with a heating wire (the temperature is controlled at above 100°C to ensure that the water vapor will not condense), and a subsequent simulation experiment of refractory material resistance to water vapor oxidation erosion is carried out.

[0068] In particular, the water vapor content in the mixed gas in step S3 is set to different gradients, and repeated simulation experiments are carried out to obtain the regular curve of the influence of the change in water vapor content on the erosion rate of the refractory sample; in practical applications, the erosion rate of the refractory sample can be directly obtained according to the change in water vapor content in the regular curve, providing some guidance for the long-life production practice of the blast furnace hearth. In addition, in the actual production of the blast furnace, the ambient temperature of the refractory materials in different parts is different; by adjusting the temperature of the simulation experiment of this scheme and carrying out repeated simulation tests, the regularity of the erosion rate of the refractory sample by water vapor at different temperatures is obtained, which has guiding significance for the practical application of refractory materials.

[0069] In a specific embodiment, the heating device includes: a high-temperature energy-saving vertical tube furnace, a precision temperature controller, a computer acquisition system, a weighing system and an image acquisition system; the precision temperature controller adjusts the temperature of the high-temperature energy-saving vertical tube furnace, and the data collected by the weighing system and the image acquisition system are fed back to the computer acquisition system. The heating device and the mixed gas preparation device can be connected as an integrated device, from gas injection, gas preparation, transportation to the heating device, the heating device starts the simulation experiment, obtains the data results, and forms a closed system; the method is relatively simple in equipment, simple in sample preparation, easy to operate, high in experimental success rate, and the evaluation indicators obtained are comprehensive and accurate.

[0070] Example 1

[0071] This embodiment provides a method for evaluating the steam oxidation erosion resistance of blast furnace refractory materials. The refractory materials are carbon composite bricks, and the Figure 2 The experimental device shown in the figure is used to perform a simulation experiment, which specifically includes the following steps:

[0072] S1. Randomly drill cylindrical samples with a diameter of 12.5mm and a height of 2mm from the actual carbon composite bricks used in the blast furnace hearth; grind, polish and clean (alcohol) the surface of the sample, and then dry it at 110±5℃ for 4h to prevent the moisture on the surface of the sample from affecting the experimental results. Then put the carbon composite brick sample in a drying oven for use; before the experiment, use a balance to weigh the sample mass, use a vernier caliper to measure the sample diameter and height, and take pictures of the sample to observe the macroscopic morphology of the sample before the reaction. Randomly sample again from this complete blast furnace carbon composite brick, make a scanning electron microscope sample for SEM-EDS analysis; among them, the oxidation rate of the carbon composite brick sample used in the oxidation rate test experiment is 0.90%;

[0073] S2. Determine the relevant parameters of the simulation experiment according to the actual production conditions, the reaction temperature is 800℃, the time is 2h, and the carrier gas type is argon; turn on the SRS13A precision temperature controller of the heating device, set the temperature program, and set the heating rate and cooling rate to 5℃ / min; and set the specific heating preparation. After the program setting is completed, check the set program; start the heating key;

[0074] The specific heating system is as follows: the first step is to heat from 0°C to 300°C for 60 minutes; the second step is to heat from 300°C to 800°C for 100 minutes; the third step is to keep at 800°C for 150 minutes; the fourth step is to cool from 800°C to 300°C for 100 minutes; the fifth step is to cool from 300°C to 0°C for 60 minutes.

[0075] S3, argon is passed into the mixing tank at a flow rate of 200mL / min, the Mg device in the gas purification system is heated to 500℃, the temperature controller of the mixing tank is heated to 300℃, and the temperature controller of the heating line is heated to 100℃. When all three reach the specified temperature, deionized water is injected into the mixing tank through an injection pump at a flow rate of 3.6mL / h, and after heating and gasification, it is mixed with the purified argon gas, and then enters the high-temperature energy-saving vertical tube furnace through a silicone tube wrapped with a heating line at a flow rate of 100mL / min; the mixed gas is passed into the furnace when the tube furnace reaches 800℃, and the sample is placed in the tube furnace after being kept warm in the gas environment for 30 minutes to ensure that the composition of the mixed gas in the high-temperature tube furnace is stable when the carbon composite brick anti-water vapor oxidation erosion experiment is carried out; wherein, the water vapor content in the mixed gas is 50%;

[0076] S4. When the tube furnace is heated to 800°C, turn on the weighing system (turn on preheating 30 minutes in advance), the image acquisition system and the computer acquisition system at the same time, and check whether the connection is successful; put the carbon composite brick sample into the crucible, connect the suspension rod and fix it under the balance of the weighing system, and place the crucible in the middle of the constant temperature zone of the tube furnace to prevent contact with the side wall of the furnace tube;

[0077] S5. After the simulation experiment is completed, data on the carbon composite brick sample is obtained, including the mass change data and morphology change data of the carbon composite brick sample, and the data are processed; and the erosion rate of the carbon composite brick sample by water vapor is calculated using the following formula:

[0078]

[0079] Where v is the erosion rate of the carbon composite brick sample, g / (h·mm 2 );ρ is the density of carbon composite brick, g / cm 3 ;w c is the carbon content of the carbon composite brick, %; h1 is the height of the carbon composite brick sample before the experiment, mm; d1 is the diameter of the carbon composite brick sample before the experiment, mm; d2 is the diameter of the carbon composite brick sample after the experiment, mm; t is the reaction time of the simulation experiment, h;

[0080] The mass change rate of the carbon composite brick sample is calculated based on the mass change data, and the size change of the carbon composite brick sample is obtained based on the morphology change data; the volume change rate and erosion degree of the carbon composite brick sample are calculated based on the size change. The calculation formula for the mass change rate is as follows:

[0081]

[0082] Where, η is the mass change rate, %; m1 is the mass of carbon composite brick before the experiment, g; m2 is the mass of carbon composite brick after the experiment, g;

[0083] The volume change rate is calculated as follows:

[0084]

[0085] Wherein, λ is the volume change rate, %; d1 is the average diameter of the carbon composite brick before the experiment, mm; d2 is the average diameter of the carbon composite brick after the experiment, mm; h1 is the average height of the carbon composite brick before the experiment, mm; h2 is the average height of the carbon composite brick after the experiment, mm.

[0086] The calculation formula of erosion degree is as follows:

[0087]

[0088] Wherein, Δd is the erosion degree of the carbon composite brick sample, mm / h; t is the reaction time of the simulation experiment, h; d1 is the diameter of the carbon composite brick sample before the experiment, mm; d2 is the diameter of the carbon composite brick sample after the experiment, mm;

[0089] S6. The obtained erosion rate of the carbon composite brick sample is combined with the indicators of mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the carbon composite brick to obtain an evaluation system for the blast furnace carbon composite brick's resistance to water vapor oxidation erosion.

[0090] The samples after the experiment were made into scanning electron microscope specimens for SEM-EDS analysis to observe the microscopic morphology and structural characteristics after the reaction. The physical phase characteristics after the reaction were analyzed by EDS to analyze the degree and mechanism of oxidation corrosion of water vapor on carbon composite bricks.

[0091] See also Figure 1 As shown, Figure 1 The electron microscope images of the carbon composite bricks before and after the experiment of Example 1 (a is before the experiment, b is after the experiment). It can be seen from Figure a that the sample before the reaction has fewer pores, smaller pore size, and a relatively smooth surface; while the pores on the surface of the sample after the reaction in Figure b are significantly increased, and the pore size is significantly increased, and the surface becomes rough. This is because water vapor oxidizes the carbon in the carbon composite brick, generating pores, or increases the original pore size, causing the surface to become rough, resulting in oxidation corrosion of the sample.

[0092] Example 2

[0093] Example 2 provides a method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion. Compared with Example 1, the difference is that the refractory material used is a small carbon block formed by molding and firing, and its size is the same as the sample size of Example 1. The oxidation rate of the sample is 16.31%, and the rest is roughly the same as Example 1, which will not be repeated here.

[0094] The results of the evaluation indexes of the refractory materials of Examples 1 and 2 for their resistance to water vapor oxidation corrosion are shown in the following table.

[0095] Table 1 Experimental data results of Examples 1 and 2

[0096]

[0097] As shown in Table 1, the erosion rate of the small carbon blocks pressed and fired in Example 2 is higher than that of the carbon composite brick sample in Example 1, and its mass change rate, volume change rate and erosion degree are also higher than those in Example 1; this corresponds to the test results of the oxidation rate, indicating that the accuracy of the data for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials in this scheme is good. In addition, the erosion rate introduced has a good performance for evaluating the water vapor oxidation erosion resistance of refractory materials, and the erosion rate can be used to well grasp the erosion of refractory materials during blast furnace service.

[0098] Embodiments 3 to 6

[0099] Examples 3 to 6 provide a method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion. Compared with Example 2, the difference is that the reaction temperatures of the experiments in Examples 3 to 6 are 400°C, 600°C, 1000°C, and 1200°C, respectively; the rest are roughly the same as Example 2 and will not be repeated here.

[0100] The results of the evaluation indexes of the steam oxidation corrosion resistance of the small carbon blocks obtained by compression firing in Examples 3 to 6 are shown in the following table.

[0101] Table 2 Experimental data results of Examples 3 to 6

[0102]

[0103] It can be seen from Table 2 that the mass change rate, volume change rate, erosion degree and erosion rate of the furnace hearth refractory materials at different temperatures are different; it can be seen that as the temperature increases, the erosion rate and erosion degree of the refractory materials increase.

[0104] From the data of Examples 2 to 6, we can obtain the influence of temperature changes on the erosion rate of small carbon blocks formed by molded firing of the refractory material, and the erosion rate of water vapor on refractory material samples at different temperatures; in practical applications, the erosion rate of the refractory material sample at different positions in the furnace can be directly obtained according to the corresponding law, which has guiding significance for the practical application of refractory materials.

[0105] Comparative Example 1

[0106] Comparative Example 1 provides a method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion. Compared with Example 1, the difference is that the sample used is in the shape of a regular quadrangular prism with a bottom side length of 12 mm and a height of 5 mm; the rest is roughly the same as Example 1 and will not be repeated here.

[0107] The experiment of Example 1 and Comparative Example 1 was repeated many times, and it was found that the erosion rate indicators of the multiple experiments of Comparative Example 1 had a large difference. This was because the two directions overlapped during the water vapor oxidation process of the sample with this shape, so the oxidation was uneven, resulting in a large randomness in the experimental results, errors in the data, and instability. However, in Example 1, since the shape of the sample was uniform, the water vapor oxidation erosion rate in all directions was relatively uniform, and the calculated erosion rate result was less random and more accurate.

[0108] In summary, the present invention provides a method for evaluating the water vapor oxidation erosion resistance of blast furnace refractory materials, and adopts a simulation experiment method to establish an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials; determines relevant parameters of the simulation experiment according to actual production conditions, conducts a simulation experiment, and obtains a series of data of water vapor oxidation erosion of refractory material samples; uses a limited formula to calculate the erosion rate of the refractory material samples, and combines it with indicators of mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the refractory materials to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and conducts a comprehensive evaluation of the water vapor oxidation erosion resistance of blast furnace refractory materials. The present invention introduces the definition of erosion rate and erosion degree when evaluating the anti-water vapor oxidation erosion performance of blast furnace refractory materials, and provides an accurate calculation method. The evaluation index is scientific and reasonable, has high accuracy, and is consistent with the actual erosion situation of blast furnace hearth refractory materials; by combining a series of indicators such as mass change rate, volume change rate, erosion degree, erosion rate, and microscopic morphology change characteristics, an evaluation system for evaluating the anti-water vapor oxidation erosion performance of blast furnace refractory materials is established, so that the evaluation standard is more systematic and accurate. The simulation experiment method is simple and easy to operate, the experimental success rate is high, and the obtained evaluation index is comprehensive and accurate, which provides a partial guiding basis for the long-life production practice of blast furnace hearths.

[0109] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion, characterized in that: The simulation experiment method is used to evaluate the performance of blast furnace refractory materials against water vapor oxidation corrosion, including the following steps: S1. Making a cylindrical sample of refractory material for an actual blast furnace hearth and pretreating the cylindrical sample to obtain a pretreated refractory sample; the ratio of the diameter to the height of the refractory sample is (2.0-6.5):1; S2, placing the refractory material sample in step S1 in a crucible, placing the crucible in a heating device, and connecting it to a weighing system of the heating device to record the mass change of the refractory material sample in real time; the heating device is also provided with an image acquisition system to record the morphology change of the refractory material sample in real time; S3, determining relevant parameters of the simulation experiment according to actual production conditions; conducting a simulation experiment of refractory materials according to the relevant parameters, and introducing a mixed gas containing water vapor and its carrier gas into the heating device for reaction throughout the experiment; S4. After the simulation experiment is completed, data on the refractory material sample is obtained, including the mass change data and the morphology change data of the refractory material sample, and the data are processed; and the erosion rate of the refractory material sample by water vapor is calculated using the following formula: Where v is the erosion rate of the refractory sample, g / (h·mm 2 );ρ is the density of refractory material, g / cm 3 ;w c is the carbon content of the refractory material, %; h1 is the height of the refractory material sample before the experiment, mm; d1 is the diameter of the refractory material sample before the experiment, mm; d2 is the diameter of the refractory material sample after the experiment, mm; t is the reaction time of the simulation experiment, h; S5. Combine the erosion rate of the refractory material sample obtained in step S4 with the mass change rate, volume change rate, erosion degree, and microscopic morphology change characteristics of the refractory material sample to obtain an evaluation system for the water vapor oxidation erosion resistance of blast furnace refractory materials, and conduct a comprehensive evaluation of the water vapor oxidation erosion resistance of blast furnace refractory materials.

2. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S3, the relevant parameters include reaction temperature, reaction time, and the content of water vapor in the mixed gas.

3. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S3, the temperature of the mixed gas introduced into the heating device is above 100°C, and the flow rate of the mixed gas is 200-800 mL / min.

4. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: The refractory material is a carbon-containing refractory material; the carrier gas type of the water vapor includes an inert gas, and the carrier gas needs to be purified by a purification system before mixing with the water vapor to remove O2, moisture and CO2 impurities therein.

5. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S4, processing the data of the refractory material sample includes: calculating the mass change rate of the refractory material sample according to the mass change data; obtaining the size change of the refractory material sample according to the morphology change data, and calculating the volume change rate and erosion degree of the refractory material sample according to the size change.

6. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S5, the calculation formula of the erosion degree is as follows: Wherein, Δd is the erosion degree of the refractory sample, mm / h; t is the reaction time of the simulation experiment, h; d1 is the diameter of the refractory sample before the experiment, mm; d2 is the diameter of the refractory sample after the experiment, mm.

7. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S3, the mixed gas is prepared by injecting deionized water into a gas mixing tank using a syringe pump, mixing and heating the mixed gas with the carrier gas injected therein to obtain the mixed gas; the content percentage of water vapor in the mixed gas is 0 to 100%.

8. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 7, characterized in that: The injection speed of the deionized water is 0.1-1500 mL / h; the heating temperature is 300-400° C.

9. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: The water vapor content in the mixed gas in step S3 is set to different gradients, and the simulation experiment is repeated to obtain a curve of the influence of the change in water vapor content on the erosion rate of the refractory sample.

10. The method for evaluating the resistance of blast furnace refractory materials to water vapor oxidation corrosion according to claim 1, characterized in that: In step S1, the pretreatment includes grinding, polishing, and alcohol cleaning the surface of the refractory material sample, and drying it.

Citation Information

Patent Citations

  • Test device and method for evaluating alkali metal corrosion resistance of refractory material

    CN108195746A

  • Test device and method used for evaluating molten iron erosion resistance of refractory materials

    CN108279246A

  • Test device and evaluation method for evaluating molten iron corrosion resistance of blast furnace carbon brick

    CN113624794A

  • Method of evaluating corrosion resistance, abrasion resistance and oxidation resistance of carbon-containing refractory material

    JP2007298433A