Seawater-resistant lens and preparation method thereof

By forming two reinforcement layers on the surface of the lens substrate, the existing anti-seawater lenses are solved easily and have low strength problems in acidic environments, improving the anti-seawater corrosion performance and scratch resistance of the lenses, and extending their service life.

CN114994810BActive Publication Date: 2024-11-22XIAMEN JS POLARIZERS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210678293.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-16
Publication Date
2024-11-22
Estimated Expiration
2042-06-16

AI Technical Summary

Technical Problem

The existing functional coating material of seawater resistant lenses is sensitive to acidic environments, easy to scrape, and the lens strength is low, making it difficult to use in acidic environments.

Method used

Two reinforcement layers are formed on the surface of the lens substrate. First, a reinforcement treatment is performed to form the base layer, then vacuum coating is performed on the seawater resistance layer, and finally a secondary reinforcement treatment is performed to improve the bonding force between the film layer and the substrate and the overall strength of the lens. .

Benefits of technology

It significantly improves the lens's seawater corrosion resistance and scratch resistance, reduces the defective yield, and safely uses the lens in an acidic environment and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003697294030000071
    Figure BDA0003697294030000071
  • Figure BDA0003697294030000072
    Figure BDA0003697294030000072
  • Figure BDA0003697294030000081
    Figure BDA0003697294030000081
Patent Text Reader

Abstract

The present invention relates to a seawater-resistant lens and a preparation method thereof. The preparation method comprises the following steps: obtaining a substrate with a clean surface; performing a primary strengthening treatment on the surface of the substrate, immersing the substrate in a strengthening liquid, and drying at 80-100°C to form a primary strengthening layer on the surface of the substrate; performing vacuum coating to form a seawater-resistant layer; the conditions of the vacuum coating include: the film material is chromium oxide, titanium oxide or nickel oxide, and the pressure of the vacuum chamber is 1.0×10 ‑3 Pa~1.0×10 ‑5 Pa, the temperature is 85-110°C; a secondary strengthening treatment is performed, the coated substrate is immersed in a strengthening liquid, and dried at 80-100°C to form a secondary strengthening layer on the surface of the anti-seawater layer. The lens has the advantages of being resistant to seawater and scratch-resistant, meets the needs of consumers, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation technology of a functional lens, in particular to a seawater-resistant lens and a preparation method thereof. Background Art

[0002] Seawater-resistant lenses generally contain functional coating layers, which are used to prevent seawater from corroding the main lens material. These functional coating layers are made of metal oxides, organic polymers, corrosion-resistant nanopolymers, etc. These materials are generally alkaline and more sensitive to acidic environments, so the outer surface of the lens needs to be treated for strength.

[0003] For example, patent application CN113580478A discloses a method for producing lenses that protect against blue light, ultraviolet rays, radiation, reflection and seawater, including step S101, in which a certain amount of a catalyst composed of solid organic tin, such as monobutyl tin oxide, and solid inorganic tin and aromatic diisocyanate are pre-added in an automatic stirring reactor, after mixed and dissolved, a certain amount of polythiol is added and mixed evenly; step S102, the oven temperature is adjusted to an optimal temperature and maintained for a certain period of time to cause polymerization reaction and solidification to obtain a high-refractive index polymer optical resin material; step S103, in an automatic stirring device, a certain amount of high-refractive index polymer optical resin, ultraviolet absorber and anti-blue light absorber are added, mixed evenly and filtered through a filter membrane; step S104, in an At a certain pressure and temperature, after degassing for a certain period of time, after returning to normal pressure, the oven temperature is adjusted to the optimal temperature and maintained for a certain period of time, the material is dried, and then it is molded into the lens mold by high-temperature injection molding; step S105, the mold is cooled down, and when the temperature reaches the demoulding temperature, the demoulding program is started to demould, and a multifunctional lens substrate is obtained; step S106, simulate the film layer design, adjust to the optimal film layer state, dry the multifunctional lens substrate and send it to the coating equipment, vacuumize, and flush with oxygen to evaporate the reflective film layer; step S107, both sides of the lens are coated with a radiation-proof film; step S108, a fluoride film is coated on the lens radiation-proof film; step S109, after the fluoride film is coated, the lens is sent to the surface treatment production line, and the lens is immersed in a nanomaterial strengthening liquid for surface strengthening treatment. This kind of lens has a variety of functional film materials, poor stacking fusion, and limited bonding between the coating layer and the substrate. Although a strengthening layer is designed on the outermost layer, there is still a problem that the film layer is easy to scrape off. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem of easy scratching of existing seawater-resistant lenses and to provide a method for preparing seawater-resistant lenses. Two strengthening layers are formed on the surface of a substrate, and a seawater-resistant layer is arranged in the middle of the strengthening layers. While improving the bonding strength between the film layer and the substrate, the overall strength of the lens is also improved, which has the advantage of wear resistance.

[0005] Usually, strengthening treatment is performed on the lens after coating, but this method can only protect the coating layer, and the strength of the lens is low and has no wear resistance advantage. The present invention strengthens before coating and introduces the coating process between the secondary strengthening, which can well solve the problem that the seawater resistant layer is not acid-resistant, so that the lens can be used in an acidic environment. On the other hand, the strength of the lens is greatly improved.

[0006] Since the coating is carried out after the primary strengthening, the primary strengthening layer is formed and hardened before the anti-seawater layer. After the anti-seawater layer is formed, the primary strengthening layer is covered, and the anti-seawater layer is formed on the surface of the primary strengthening layer. The inventor found that when the secondary strengthening is carried out, defective products such as cracking of the lens film are prone to occur, and the defective products account for 25-40%. For this reason, the inventor has continuously tried and improved the strengthening liquid and vacuum coating conditions, respectively, and increased the lens yield to 98% and above, and finally completed the present invention.

[0007] The specific plan is as follows:

[0008] A method for preparing a seawater-resistant lens comprises the following steps:

[0009] (1) obtaining a substrate with a clean surface;

[0010] (2) performing a primary strengthening treatment on the surface of the substrate, immersing the substrate in a strengthening solution, and drying at 80-100° C. to form a primary strengthening layer on the surface of the substrate;

[0011] (3) performing vacuum coating to form a seawater resistant layer on the surface of the primary strengthening layer; the conditions for the vacuum coating include: the film material is chromium oxide, titanium oxide or nickel oxide, the pressure of the vacuum chamber is 1.0×10 -3 Pa~1.0×10 -5 Pa, temperature is 85-110℃;

[0012] (4) performing a secondary strengthening treatment, immersing the coated substrate in a strengthening solution, and drying at 80-100° C. to form a secondary strengthening layer on the surface of the seawater-resistant layer, thereby obtaining a seawater-resistant lens.

[0013] Furthermore, the substrate is a glass substrate or a nylon substrate with a thickness of 0.5-2 mm.

[0014] Furthermore, in step (1), the substrate is ultrasonically cleaned with an organic solvent and then dried; the outer surface of the dried lens is bombarded with an ion gun to obtain a substrate with a clean surface.

[0015] Furthermore, the strengthening liquid in step (2) and / or step (3) contains at least one of polysiloxane, polysilazane or fluorocarbon resin.

[0016] Furthermore, in step (3), the vacuum coating is first performed by bombarding the surface with an ion gun and then coating, and the film thickness of the vacuum coating is 100-7500nm, preferably 2000-5000nm.

[0017] Furthermore, the pressure of the vacuum chamber in step (3) is 1.0×10 -4 Pa~1.0×10 -5 Pa, temperature is 90-100℃.

[0018] Furthermore, the temperature of the vacuum chamber in step (3) is at least 0.1-10°C, preferably 2-6°C, higher than the drying temperature of the secondary strengthening treatment in step (4).

[0019] Furthermore, the drying temperature of the secondary strengthening treatment in step (4) is 80-90°C for 2-10 hours, preferably 80-85°C for 4-8 hours.

[0020] The present invention also protects the seawater-resistant lens prepared by the preparation method of the seawater-resistant lens.

[0021] The present invention also protects a pair of glasses comprising the seawater-resistant lenses.

[0022] Beneficial effects:

[0023] In the present invention, the lens obtained by the preparation method of the seawater-resistant lens has good seawater corrosion resistance and is scratch-resistant, which can effectively extend the service life of the lens, exert the seawater-resistant effect for a long time, and has good market application prospects. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the examples, those without specifying specific techniques or conditions are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those without specifying the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially. In the following examples, if not clearly stated, "%" refers to weight percentage.

[0025] The test methods used below include:

[0026] Seawater resistance test: Soak the lens in a 5wt% sodium chloride aqueous solution and observe whether there are any visible changes in the film layer on the lens surface.

[0027] Scratch resistance test: refer to the lens surface wear resistance requirements GB 10810.5-2012.

[0028] Example 1

[0029] The method for preparing seawater-resistant lenses is as follows: a glass sheet with a thickness of 1 mm is used as a substrate, the substrate is immersed in ethanol, an ultrasonic source is started with a power of 1000 W, and ultrasonic treatment is performed for 30 minutes, then the lens is taken out, blown dry, and set aside.

[0030] The strengthening liquid is a conventional polysiloxane strengthening liquid with a viscosity of 10-15 cp. The clean substrate is immersed in the tank containing the strengthening liquid for 10 seconds, taken out and dried at 80° C. for 30 minutes to form a primary strengthening layer.

[0031] The vacuum coating machine was used for vacuum coating, and the pressure in the vacuum coating chamber was maintained at 1.0×10 -3 Pa~1.0×10 -5 Pa, while maintaining the temperature in the vacuum coating chamber at 95°C, use an ion gun to bombard the surface for 2 to 3 minutes, and then use resistance heating to heat the chromium oxide of the film material to form a seawater resistant layer with a thickness of 2000 nanometers on the surface of the primary strengthening layer.

[0032] The coated lens was taken out for secondary strengthening treatment, and after cooling, it was placed in a tank containing strengthening liquid for 10 seconds, and after taking it out, it was dried at 85° C. for 7 hours to obtain a seawater-resistant lens.

[0033] Example 2

[0034] The method for preparing seawater-resistant lenses is as follows: a nylon sheet with a thickness of 0.5 mm is used as a substrate, the substrate is immersed in ethanol, an ultrasonic source is started with a power of 1000 W, and ultrasonic treatment is performed for 30 minutes, then the lens is taken out, blown dry, and set aside.

[0035] The strengthening liquid uses conventional polysilazane strengthening liquid with a viscosity of 10-15cp. The clean substrate is immersed in the tank containing the strengthening liquid for 10 seconds, taken out and dried at 100°C for 30 minutes to form a primary strengthening layer.

[0036] The vacuum coating machine was used for vacuum coating, and the pressure in the vacuum coating chamber was maintained at 1.0×10 -4 Pa~1.0×10 -5 Pa, while maintaining the temperature in the vacuum coating chamber at 100°C, use an ion gun to bombard the surface for 2 to 3 minutes, and then use resistance heating to heat the chromium oxide of the film material to form a seawater resistant layer with a thickness of 4000 nanometers on the surface of the primary strengthening layer.

[0037] The coated lens was taken out for secondary strengthening treatment, and after cooling, it was placed in a tank containing strengthening liquid for 10 seconds, and then taken out and dried at 85° C. for 4 hours to obtain a seawater-resistant lens.

[0038] Example 3

[0039] The method for preparing seawater-resistant lenses is as follows: a nylon sheet with a thickness of 1.5 mm is used as a substrate, the substrate is immersed in ethanol, an ultrasonic source is started with a power of 1000 W, and ultrasonic treatment is performed for 30 minutes, then the lens is taken out, blown dry, and set aside.

[0040] The strengthening liquid uses conventional fluorocarbon resin strengthening liquid with a viscosity of 10-15cp. The clean substrate is immersed in the tank containing the strengthening liquid for 10 seconds, taken out and dried at 90°C for 30 minutes to form a primary strengthening layer.

[0041] The vacuum coating machine was used for vacuum coating, and the pressure in the vacuum coating chamber was maintained at 1.0×10 -3 Pa~1.0×10 -4 Pa, while maintaining the temperature in the vacuum coating chamber at 90°C, use an ion gun to bombard the surface for 2 to 3 minutes, and then use resistance heating to heat the chromium oxide of the film material to form a seawater resistant layer with a thickness of 5000 nanometers on the surface of the primary strengthening layer.

[0042] The coated lens was taken out for secondary strengthening treatment, and after cooling, it was placed in a tank containing strengthening liquid for 10 seconds, and after taking it out, it was dried at 80° C. for 5 hours to obtain a seawater-resistant lens.

[0043] Comparative Example 1

[0044] The method for preparing seawater-resistant lenses is as follows: a glass sheet with a thickness of 1 mm is used as a substrate, the substrate is immersed in ethanol, an ultrasonic source is started with a power of 1000 W, and ultrasonic treatment is performed for 30 minutes, then the lens is taken out and blown dry for later use.

[0045] The strengthening liquid is a conventional polysiloxane strengthening liquid with a viscosity of 10-15 cp. The clean substrate is immersed in the tank containing the strengthening liquid for 10 seconds, taken out and dried at 80° C. for 30 minutes to form a primary strengthening layer.

[0046] The vacuum coating machine was used for vacuum coating, and the pressure in the vacuum coating chamber was maintained at 1.0×10 -3 Pa~1.0×10 -5 Pa, while maintaining the temperature in the vacuum coating chamber at 60°C, use an ion gun to bombard the surface for 2 to 3 minutes, and then use resistance heating to heat the chromium oxide of the film material to form a seawater resistant layer with a thickness of 2000 nanometers on the surface of the primary strengthening layer.

[0047] A secondary strengthening treatment was carried out. The coated lens was taken out, cooled and placed in a tank containing strengthening liquid for 10 seconds. After being taken out, it was dried at 85°C for 7 hours. Obvious cracks were found on the surface of the lens.

[0048] Comparative Example 2

[0049] The method for preparing seawater-resistant lenses is as follows: a glass sheet with a thickness of 1 mm is used as a substrate, the substrate is immersed in ethanol, an ultrasonic source is started with a power of 1000 W, and ultrasonic treatment is performed for 30 minutes, then the lens is taken out, blown dry, and set aside.

[0050] The strengthening liquid is a conventional polysiloxane strengthening liquid with a viscosity of 10-15 cp. The clean substrate is immersed in the tank containing the strengthening liquid for 10 seconds, taken out and dried at 80° C. for 30 minutes to form a primary strengthening layer.

[0051] The vacuum coating machine was used for vacuum coating, and the pressure in the vacuum coating chamber was maintained at 1.0×10 -3 Pa~1.0×10 -5 Pa, while maintaining the temperature in the vacuum coating chamber at 85°C, use an ion gun to bombard the surface for 2 to 3 minutes, and then use resistance heating to heat the chromium oxide of the film material to form a seawater resistant layer with a thickness of 2000 nanometers on the surface of the primary strengthening layer.

[0052] A secondary strengthening treatment was performed, and the coated lens was taken out, cooled, and placed in a tank containing strengthening liquid for 10 seconds. After being taken out, it was dried at 85° C. for 7 hours to obtain a comparison lens.

[0053] Performance Testing

[0054] The lenses prepared in Example 1 and Comparative Example 2 were tested, and the results are shown in Tables 1 and 2.

[0055] Table 1 Seawater resistance test results

[0056]

[0057] Table 2 Scratch resistance test results

[0058]

[0059]

[0060] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0061] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0062] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a seawater-resistant lens, characterized in that: The following steps are involved: (1) obtaining a substrate with a clean surface; (2) performing a primary strengthening treatment on the surface of the substrate, immersing the substrate in a strengthening solution, and drying at 80-100° C. to form a primary strengthening layer on the surface of the substrate; (3) performing vacuum coating to form a seawater resistant layer on the surface of the primary strengthening layer; the conditions for the vacuum coating include: the film material is chromium oxide, titanium oxide or nickel oxide, the pressure of the vacuum chamber is 1.0×10 -3 Pa~1.0×10 -5 Pa, temperature is 85-110℃; (4) performing a secondary strengthening treatment, immersing the coated substrate in a strengthening solution, and drying at 80-100° C. to form a secondary strengthening layer on the surface of the seawater-resistant layer, thereby obtaining a seawater-resistant lens.

2. The method for preparing the seawater resistant lens according to claim 1, characterized in that: The substrate is a glass substrate or a nylon substrate with a thickness of 0.5-2 mm.

3. The method for preparing the seawater resistant lens according to claim 1, characterized in that: In step (1), the substrate is ultrasonically cleaned with an organic solvent and then dried to obtain a substrate with a clean surface.

4. The method for preparing the seawater resistant lens according to claim 1, characterized in that: The strengthening liquid in step (2) and / or step (3) contains at least one of polysiloxane, polysilazane or fluorocarbon resin.

5. The method for preparing the seawater resistant lens according to any one of claims 1 to 4, characterized in that: In step (3), the vacuum coating is first performed by bombarding the surface with an ion gun and then coating. The thickness of the vacuum coated film is 100-7500nm.

6. The method for preparing the seawater resistant lens according to claim 5, characterized in that: The vacuum coating has a film thickness of 2000-5000nm.

7. The method for preparing the seawater resistant lens according to claim 5 or 6, characterized in that: The pressure of the vacuum chamber in step (3) is 1.0×10 -4 Pa~1.0×10 -5 Pa, temperature is 90-100℃.

8. The method for preparing the seawater resistant lens according to claim 5 or 6, characterized in that: The temperature of the vacuum chamber in step (3) is at least 0.1-10° C. higher than the drying temperature of the secondary strengthening treatment in step (4).

9. The method for preparing the seawater resistant lens according to claim 8, characterized in that: The temperature of the vacuum chamber in step (3) is at least 2-6°C higher than the drying temperature of the secondary strengthening treatment in step (4).

10. The method for preparing the seawater resistant lens according to any one of claims 1 to 4, characterized in that: The drying temperature of the secondary strengthening treatment in step (4) is 80-90° C. and the drying time is 2-10 hours.

11. The method for preparing the seawater resistant lens according to claim 10, characterized in that: The drying temperature of the secondary strengthening treatment in step (4) is 80-85° C. and the drying time is 4-8 hours.

12. The seawater-resistant lens prepared by the method for preparing the seawater-resistant lens according to any one of claims 1 to 11.

13. A pair of glasses comprising the seawater-resistant lens according to claim 12.