Method for recovering platinum group metals, composition containing platinum group metals and ceramic material
By immobilizing and hydrolyzing the platinum group metal on the ceramic material, the problems of high energy consumption for recycling of platinum group metals and complex waste liquids in the prior art are solved, and efficient and low-cost recycling of platinum group metals are achieved.
Patent Information
- Application Number
- CN202180012033.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-30
- Filing Date
- 2021-01-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-01-29
AI Technical Summary
The existing platinum group metal recycling methods have problems such as large energy consumption, high drug cost and complex waste liquid treatment. Especially since the platinum group metal is chemically stable, it is difficult to effectively extract and recover from waste catalysts.
By immobilizing the platinum group metal on a ceramic material, the platinum group metal containing the platinum group metal is oxidized and immobilized by contacting the melt of alkali metal carbonate or hydroxide with the ceramic material to oxidize and immobilize the platinum group metal to form The water-soluble platinum group compound is then dissolved through an aqueous solvent for recovery.
The cost of aqueous solvent treatment is reduced, the efficiency of platinum group metal recovery is improved, the mixing of oxide salts is reduced, the efficient recovery of platinum group metals is achieved, and different types of platinum group metals can be selected.
Smart Images

Figure GDA0005105526640000161 
Figure GDA0005105526640000171 
Figure GDA0005105526640000181
Abstract
Description
Technical Field
[0001] The present invention relates to a method for recovering platinum group metals, a composition containing platinum group metals and a ceramic material for fixing platinum group metals. Background Art
[0002] Platinum group metals have excellent catalytic performance and are therefore used in various applications such as automobile exhaust purification catalysts and fuel vehicle catalysts. Thus, platinum group metals are indispensable elements in industry. On the other hand, due to their rarity, the production of platinum group metals is very small compared to base metals. For example, even Pt and Pd, which are produced in relatively large quantities among platinum group metals, have a production volume of about 200 tons each. Therefore, if the demand for platinum group metals increases due to the development of new materials using platinum group metals, the supply of platinum group metals will be insufficient. That is, it can be considered that the supply risk of platinum group metals is now high.
[0003] In order to cope with the supply risks caused by such uneven resource distribution, it is very important to extract and recover platinum group metals from waste products such as waste catalysts generated in Japan. In addition, the mining and smelting of natural ores are accompanied by a large environmental load. Therefore, if platinum group metals can be effectively extracted from waste products with a higher concentration of platinum group metals than natural ores, it is related to the reduction of environmental load. However, since platinum group metals are chemically very stable, in the existing dry method, it is necessary to separate and concentrate the platinum group metals from the waste products and then dissolve the concentrate with a high concentration of acid. Therefore, the energy consumption for extracting platinum group metals is large, and the cost of reagents and waste liquid treatment is also high. Therefore, there is an urgent need to develop a more effective method for recovering platinum group metals. For example, in Patent Documents 1 to 4 and Non-Patent Document 1, prior art related to methods for recovering platinum group metals is disclosed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2014-234551
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2011-252217
[0008] Patent Document 3: Japanese Patent Application Laid-Open No. 2008-202063
[0009] Patent Document 4: Japanese Patent Application Laid-Open No. 2013-249494
[0010] Non-patent literature
[0011] Non-patent document 1: Takashi Okada, Yoshiya Taniguchi, Fumihiro Nishimura, Susumu Yonezawa: Solubilization of palladium molten mixture of sodium borates and sodium carbonate, Results in Physics, vol. 13, 2019, 102281.
[0012] Next, the prior art disclosed in Patent Documents 1 to 4 and their problems will be described.
[0013] (1) Dissolving platinum group metals by aqua regia
[0014] Patent Document 1 discloses a method of dissolving platinum group metals using aqua regia. However, chlorine gas and nitrosyl chloride generated in aqua regia are highly corrosive and toxic. Since these gases promote corrosion of peripheral equipment, costs are incurred for repairing corroded parts. In addition, a large amount of neutralizer is required to treat the used aqua regia, and the nitrate ion concentration needs to be lower than the drainage standard. Therefore, the drainage treatment process becomes complicated and the drainage treatment cost is also high.
[0015] Therefore, in order to avoid the use of harmful aqua regia, the following aqua regia-free process has also been studied.
[0016] (2) Improving the solubility of platinum group metals through the reaction between platinum group metals and active metals
[0017] Patent document 2 discloses a technique for alloying a platinum group metal by reacting it with an active metal. The obtained alloy is subjected to chlorination or oxidation treatment to generate a complex compound of chloride or oxide of the platinum group metal and chloride. The platinum group metal can be extracted by treating the complex compound with salt water. However, since steps such as alloying the platinum group metal with the active metal and chlorination / oxidation treatment of the alloy are required, the process is complicated. In addition, Mg, Ca, Zn, Fe, Na, K, Pb and Li used as active metals are highly reactive and cause corrosion of peripheral equipment.
[0018] (3) Improving the solubility of platinum group metals through the reaction of platinum group metals with chlorine
[0019] In order to simplify the process of the above-mentioned technology (2), Patent Document 3 discloses a technology for converting a platinum group metal into a chloride that is easily soluble in water by reacting a platinum group metal with chlorine in a molten salt. However, in order to convert a platinum group metal into a chloride, it is necessary to react the platinum group metal with a large amount of a chlorinating agent such as chlorine. Therefore, the chlorinating agent introduced promotes corrosion of the reactor and peripheral equipment, and the cost for repairing the reactor and peripheral equipment is high.
[0020] (4) Improving the solubility of platinum group metals by reacting platinum group metals with alkali metal carbonates
[0021] Patent Document 4 discloses a technique for forming a soluble composite oxide of a platinum group metal by reacting a platinum group metal with an alkali metal carbonate. Since the generated composite oxide has high solubility in hydrochloric acid, it can be dissolved using 12M hydrochloric acid instead of aqua regia. However, the acid concentration required for dissolution is still high, and the cost of neutralizing the wastewater is high. In addition, since highly corrosive hydrogen chloride gas is generated from high-concentration hydrochloric acid, the corrosion of peripheral equipment caused by this also becomes a problem.
[0022] (5) Dissolution of platinum group metals into aqueous solvents
[0023] In order to solve the above problems (1) to (4), the present inventors disclosed the following method: heating a platinum group metal in a molten oxide to generate a water-soluble platinum group compound, and dissolving the platinum group compound into an aqueous solvent (Non-Patent Document 1). In this method, in order to carry out a treatment of immersing the molten oxide containing the water-soluble platinum group compound in an aqueous solvent to dissolve the platinum group metal into the aqueous solvent, the obtained aqueous solvent contains a high concentration of salts derived from the molten oxide in addition to the platinum group compound. Therefore, it is desirable to develop a technology for effectively recovering platinum group metals from a molten oxide containing a water-soluble platinum group compound. Summary of the invention
[0024] An object of one embodiment of the present invention is to provide a method for recovering platinum group metals that can efficiently recover platinum group metals.
[0025] In order to solve the above-mentioned problems, a method for recovering platinum group metals according to one embodiment of the present invention comprises a fixation step, wherein a melt of a raw material containing platinum group metals, a melt of carbonate or hydroxide of an alkali metal, a melt of an oxide, and a ceramic material are brought into contact with each other to fix the platinum group metals on the ceramic material.
[0026] In order to solve the above-mentioned problems, a platinum group metal-containing composition according to one embodiment of the present invention contains a platinum group metal and an amphoteric element, and contains 99% by weight or more of the platinum group metal and 1% by weight or less of the amphoteric element when the total amount of the platinum group metal and the amphoteric element is set to 100% by weight.
[0027] In order to solve the above-mentioned problems, a ceramic material according to one embodiment of the present invention has an immobilized layer containing O and an alkali metal formed on the surface, wherein a platinum group metal is immobilized in the immobilized layer.
[0028] According to one embodiment of the present invention, a method for recovering platinum group metals capable of efficiently recovering platinum group metals can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a diagram showing an image of the surface of an alumina block observed by SEM-EDS in one example.
[0030] Figure 2 This is a diagram showing an EDS spectrum of a Pd concentrated portion on the surface of an alumina block in one example.
[0031] Figure 3 is a graph showing the recovery rate of Pd from an alumina block in one example.
[0032] Figure 4 This is a diagram showing an XRD diffraction pattern of the aluminum oxide powder having Pd adsorbed thereon after heating at 900° C. in one example.
[0033] Figure 5 This is a diagram showing an XPS spectrum of an aluminum oxide powder on which Pd is adsorbed in one example.
[0034] Figure 6 This is a diagram showing an XRD diffraction pattern of an aluminum oxide powder having Pd adsorbed thereon after heating at 600° C. in one example.
[0035] Figure 7 This is a diagram showing an image of the surface of the aluminum oxide powder on which Pd is adsorbed observed by SEM-EDS after heating at 600° C. in one example.
[0036] Figure 8 This is a diagram showing an EDS spectrum of an aluminum oxide powder having Pd adsorbed thereon after heating at 600° C. in one example.
[0037] Fig. 9 This is a diagram showing an XRD diffraction pattern of an aluminum oxide powder on which Pt is adsorbed in one example.
[0038] Fig.10 This is a diagram showing an image of the surface of an aluminum oxide powder on which Pt is adsorbed observed by SEM-EDS in one example.
[0039] Fig.11 This is a diagram showing an EDS spectrum of an aluminum oxide powder on which Pt is adsorbed in one example.
[0040] Fig.12 This is a diagram showing an image of the surface of a Pd concentrate observed using SEM-EDS in one example.
[0041] Fig.13 : is a figure which shows the EDS spectrum of the Pd concentrate in one Example. DETAILED DESCRIPTION
[0042] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. In addition, the following description is for a better understanding of the subject matter of the invention, and does not limit the present invention unless otherwise specified. In addition, in this specification, "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified.
[0043] <1. Overview of methods for recovering platinum group metals>
[0044] The present inventors have discovered that: (i) a water-soluble platinum group metal (platinum group compound) is effectively immobilized on a ceramic material, and (ii) the platinum group compound immobilized on a ceramic material is effectively eluted from the ceramic material by an aqueous solvent, thereby completing the present invention.
[0045] A method for recovering platinum group metals according to one embodiment of the present invention comprises a fixation step, wherein a melt of a raw material containing platinum group metals, a melt of carbonate or hydroxide of an alkali metal, a melt of an oxide, and a ceramic material are brought into contact to fix the platinum group metals on the ceramic material.
[0046] The platinum group metal contained in the raw material is oxidized by reacting with the oxide and the carbonate or hydroxide of the alkali metal to form a melt containing the oxide and the carbonate or hydroxide of the alkali metal, thereby forming an oxidation product of the platinum group metal. The oxidation product is a water-soluble platinum group compound and is effectively fixed on the ceramic material. Thus, the platinum group compound and salts (such as alkali metals and boric acid) derived from the melt can be separated.
[0047] As described above, the platinum group compound immobilized on the ceramic material is water-soluble. When the ceramic material on which the platinum group compound is immobilized is brought into contact with an aqueous solvent, the platinum group compound is eluted from the ceramic material into the aqueous solvent. This allows the platinum group compound to be further separated from salts and the like derived from the melt.
[0048] According to the present invention, since the mixing of salts and the like into the aqueous solvent can be significantly reduced, the cost required for the treatment of the aqueous solvent after the recovery of the platinum group metal can be reduced.
[0049] As shown in the examples described below, if the type of aqueous solvent is changed, the efficiency of dissolution of the platinum group compound into the aqueous solvent changes. Therefore, by selecting the type of aqueous solvent, the target platinum group metal can be selectively recovered. In addition, for example, by subjecting the aqueous solvent containing the platinum group compound to organic solvent treatment according to the prior art, the target platinum group metal can be selectively recovered.
[0050] <2. Immobilization process>
[0051] (2-1. Preparation of melt)
[0052] When the platinum group compound is obtained, a melt containing a carbonate, hydroxide or oxide of a platinum group metal and an alkali metal is prepared. In the melt, the platinum group metal is oxidized to form a water-soluble platinum group compound. Then, the melt containing the platinum group compound is brought into contact with a ceramic material to fix the platinum group compound on the ceramic material.
[0053] Such a melt can be prepared by heating each material of (i) a platinum group metal (e.g., a raw material containing a platinum group metal), (ii) an alkali metal carbonate or hydroxide, and (iii) an oxide separately to prepare a melt, and then contacting each of the melts of (i) to (iii) with a ceramic material. In addition, a mixture of any two materials among the above (i) to (iii) can be obtained, and the mixture can be heated to prepare a melt, and the remaining material can be heated to prepare a melt, and then contacting the melt with a ceramic material. In addition, a mixture of the three materials of the above (i) to (iii) can be obtained, and the mixture can be heated to prepare a melt, and then contacting the melt with a ceramic material. In addition, a mixture of the three materials of the above (i) to (iii) and a ceramic material can be obtained, and a melt can be obtained by heating the mixture, and then contacting the melt with a ceramic material.
[0054] According to the method of making each material of (i) to (iii) above into a melt separately, for example, preparing melts of each material other than the platinum group metal in advance, the degree of freedom of the method of executing the fixing process is improved. In addition, according to the method of obtaining a melt from a mixture of the three materials of (i) to (iii) above, since the heating for obtaining the melt can be concentrated, the time and heating cost spent on the fixing process can be reduced. In addition, according to the method of obtaining a melt from a mixture of the three materials of (i) to (iii) above and a ceramic material, the time and heating cost spent on the fixing process can be further reduced.
[0055] Examples of platinum group metals include Pd, Pt, Rh, Ir, Os, and Ru. Examples of such raw materials containing platinum group metals include waste automobile catalysts and waste electronic equipment.
[0056] Examples of the alkali metal in the alkali metal carbonate or hydroxide include Na, K, Li, Rb, and Cs. From the viewpoint of more efficiently converting the platinum group metal into a water-soluble platinum group compound, among these, Na and K are preferred, and K is more preferred. The alkali metal carbonate or hydroxide may be used alone or in combination of two or more.
[0057] The oxide may be, for example, at least one selected from the group consisting of Na2O, B2O3, K2O, SiO2, Li2O, Rb2O, Cs2O and P2O5. Examples of such oxides include glass (e.g., waste glass). By using glass as the composition of the oxide, it is possible to effectively utilize glass that can be obtained cheaply. The oxide may be used alone or as a mixture of multiple oxides. In the case where the oxide is used as a mixture of multiple oxides, if it is used as a mixture containing at least B2O3, the platinum group metal can be more reliably converted into a water-soluble platinum group compound.
[0058] The carbonate or hydroxide of the alkali metal functions as an oxidizing agent for oxidizing the platinum group metal. In addition, the oxide functions as a reaction aid for oxidizing the platinum group metal.
[0059] The raw material containing a platinum group metal, the carbonate or hydroxide of an alkali metal, and the oxide are mixed as a melt by heating, and the platinum group metal is oxidized to obtain an oxidation product of the platinum group metal. Hereinafter, when simply referred to as a "melt", it means a melt containing three materials: the raw material containing a platinum group metal, the carbonate or hydroxide of an alkali metal, and the oxide, but the melt of one embodiment of the present invention is not limited to this as described above.
[0060] (2-2. Contact between melt and ceramic material)
[0061] The ceramic material in contact with the melt can be a sintered body obtained by heat treating an inorganic material, and the specific composition is not limited. The ceramic material in contact with the melt is preferably a ceramic material of a metal oxide system. Such a ceramic material can more effectively immobilize a water-soluble platinum group compound. The ceramic material can contain aluminum oxide, zeolite, zirconium oxide, silicon dioxide, iron oxide, cobalt oxide, nickel oxide, or a mixture of two or more substances selected from them.
[0062] From the viewpoint of more effectively converting platinum group metals into water-soluble platinum group compounds, the ceramic material is preferably a material containing an amphoteric element (such as aluminum oxide, etc.). The amphoteric element becomes an oxygen anion and is dissolved from such a ceramic material into the melt. By bringing the above-mentioned melt into contact with the ceramic material in the presence of such an oxygen anion of an amphoteric element, the oxidation product of the platinum group metal reacts with the oxygen anion, and the water solubility of the above-mentioned oxidation product is easily improved. If the water solubility of the oxidation product is improved, the platinum group compound can be dissolved more effectively from the ceramic material in the dissolution step described later. Examples of amphoteric elements include Al, Ti, V, Co and Zr, among which Al and Ti are more preferred. Specific examples of oxygen anions of amphoteric elements include AlO2 - 、TiO3 2- , VO4 3- and CoO2 - .
[0063] From the viewpoint of effectively immobilizing the platinum group compound, the ceramic material is preferably porous with a large surface area. When the ceramic material contains an oxide of an amphoteric element, from the viewpoint of promoting the elution of oxygen anions, the ceramic material is preferably porous.
[0064] The fixation of the platinum group compound on the ceramic material may include: (a) adsorbing the platinum group compound contained in the melt to the ceramic material by contacting the ceramic material with the melt, (b) co-precipitating the components dissolved from the ceramic material with the platinum group compound (more specifically, co-precipitating the components dissolved from the ceramic material, the platinum group compound and the ceramic material), or (c) both of the above (a) and (b). According to the above (a), the platinum group compound can be dissolved from the ceramic material on the basis of taking out the ceramic material on which the platinum group compound is adsorbed from the melt. In this case, from the viewpoint of easy removal, the shape of the ceramic material is preferably formed into a spherical, rod-shaped or plate-shaped shape. On the other hand, according to the above (b), by removing the melt from the platinum group compound co-precipitated with the components dissolved from the ceramic material, the platinum group compound co-precipitated with the components dissolved from the ceramic material and the melt can be easily separated, and after the separation, the platinum group compound can be dissolved from the ceramic material. In this case, from the viewpoint of effective co-precipitation, the shape of the ceramic material is preferably small powder or granular. Furthermore, when using a powdered ceramic material, it is preferred that an appropriate amount of the powdered ceramic material be added so that the ceramic material can be easily separated from the melt. According to this configuration, it is possible to better prevent the powdered ceramic material from reacting with the molten oxide and solidifying.
[0065] As the components dissolved from the ceramic material into the melt, for example, oxygen anions of amphoteric elements contained in the ceramic material can be cited. Specific examples of oxygen anions of amphoteric elements include AlO2- 、AlO4 5- 、AlO5 7- 、AlO6 9- 、TiO3 2- , VO4 3- and CoO2 - .
[0066] The contact between the ceramic material and the melt is preferably carried out during heating. At this time, the contact between the ceramic material and the melt is preferably carried out at a temperature of 600 to 1100°C, and more preferably at a temperature of 800 to 1100°C. According to such a configuration, the cost required for heating can be reduced. According to one embodiment of the present invention, under mild conditions, platinum group metals can be converted into water-soluble platinum group compounds. Therefore, the upper limit of the heating temperature can be 1000°C, 900°C or 800°C. The heating temperature can be appropriately selected according to the composition of the material contained in the melt.
[0067] The time of the above-mentioned heating is preferably more than 30 minutes, more preferably more than 60 minutes, and further preferably 120 minutes. The contact of the ceramic material with the melt can be carried out at any timing during the above-mentioned heating. In addition, the time of the above-mentioned heating can be appropriately selected according to the composition of the material contained in the melt. In addition, in order to promote the oxidation of the platinum group metal, the above-mentioned heating is preferably carried out under an oxygen-containing atmosphere, for example, preferably under an atmospheric atmosphere.
[0068] Furthermore, during the contact between the ceramic material and the melt, the composition of the material in the melt and / or the oxygen partial pressure in the atmosphere during the contact between the ceramic material and the melt can be appropriately adjusted, thereby adjusting the solubility of the platinum group compound when dissolving from the ceramic material into the aqueous solvent.
[0069] For example, the amount of the platinum group compound eluted from the ceramic material can be adjusted by adjusting the solubility of the platinum group compound in the aqueous solvent by changing the basicity of the melt and / or the oxygen partial pressure in the atmosphere when the ceramic material and the melt are brought into contact with each other.
[0070] Furthermore, it is preferred that a pipe for supplying a gas containing oxygen is immersed in the melt, and the gas containing oxygen is supplied to the melt from the pipe to heat the melt while bubbling and stirring the melt.
[0071] In addition, it is preferred to add high-valent cations to the melt to further increase the ability to oxidize platinum group metals. Examples of high-valent cations include Fe 3+ 、Ce 4+ and Gd 3+ .
[0072] In addition, as a container used when the ceramic material is brought into contact with the melt, a container containing an amphoteric element such as an alumina crucible is preferably used. Thus, the amphoteric element contained in the container becomes an oxygen anion and can be dissolved into the melt. In addition, when the ceramic material contains an amphoteric element, a container formed of a metal such as stainless steel and / or titanium can be used as the above-mentioned container.
[0073] In addition, as a container for the melt, a container formed of a ceramic material may also be used. That is, the contact between the container formed of a ceramic material and the melt may be a melt of a raw material containing a platinum group metal, a melt of a carbonate or hydroxide of an alkali metal, a melt of an oxide, and a ceramic material in one embodiment of the present invention. In this case, the ceramic material forming the container may contain aluminum oxide, zeolite, zirconium oxide, silicon dioxide, iron oxide, cobalt oxide, nickel oxide, or a mixture of two or more substances selected from these.
[0074] <3. Dissolution process>
[0075] The method for recovering platinum group metals according to one embodiment of the present invention comprises a dissolution step after the above-mentioned fixation step, in which the ceramic material on which the platinum group compound is fixed is brought into contact with an aqueous solvent to dissolve the platinum group compound from the ceramic material. Since the platinum group compound fixed to the ceramic material is water-soluble, by bringing the ceramic material into contact with the aqueous solvent, the platinum group compound can be easily dissolved into the aqueous solvent to obtain an eluate containing the platinum group compound.
[0076] The immobilization step preferably includes separating the ceramic material in which the platinum group compound is immobilized from the melt. Alternatively, the method for recovering platinum group metals according to one embodiment of the present invention preferably has a separation step for separating the ceramic material in which the platinum group compound (platinum group metal) is immobilized from the melt between the immobilization step and the dissolution step. As a result, salts of oxides contained in the melt are hardly brought into the dissolution step. Therefore, the mixing of salts of oxides into the aqueous solvent can be greatly reduced. As a method for separating ceramic materials from the melt, it can be a method for removing ceramic materials from the melt, or it can be a method for removing the melt from the platinum group compound co-precipitated with the components dissolved from the ceramic material in the melt. In addition, any other method can be used as long as the ceramic material can be separated from the melt.
[0077] Aqueous solvent refers to a solvent containing water as a main component, for example, refers to a solvent containing 60% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, more preferably 95% by weight or more, more preferably 98% by weight or more, and most preferably 100% by weight of water. According to such a structure, the platinum group compound can be easily dissolved into the aqueous solvent. The upper limit of the amount of water contained in the aqueous solvent is not particularly limited, for example, it can be 80% by weight, 90% by weight or 100% by weight. In addition, the aqueous solvent is preferably an aqueous solution of an acid. Regarding the type of the acid, for example, organic acids such as citric acid, malic acid, acetic acid and oxalic acid, and inorganic acids such as hydrochloric acid, nitric acid, sulfuric acid, boric acid, phosphoric acid and perchloric acid can be listed. Regarding the concentration of the acid, for example, it can be 3 mol / L or less, preferably 1 mol / L or less, more preferably 0.1 mol / L or less, and further preferably 0.01 mol / L or less. In addition, regarding the concentration of the acid, an appropriate concentration can be selected according to the type of the acid. In addition, the aqueous solvent may not contain an acid. According to such a configuration, the platinum group compound can be easily dissolved into the aqueous solvent.
[0078] The aqueous solvent may contain a component other than water in addition to the acid, and the component is preferably a polar solvent, for example, alcohols such as methanol and ethanol, or a solution containing a hydroxide complex of an amphoteric element.
[0079] When the aqueous solvent is an acid aqueous solution, the pH of the aqueous solvent may be 4 or less, preferably 3 or less, and more preferably 2 or less. In addition, the aqueous solvent does not need to have strong acidity like aqua regia, so the pH of the aqueous solvent when it is an acid aqueous solution may be 1 or more. If such an aqueous solvent is used, not only can the platinum group compound be effectively dissolved, but also adverse effects on nature can be prevented. In addition, when the aqueous solvent is a solvent that does not contain an acid, the pH of the aqueous solvent may be, for example, 6 to 8, 6 to 7, or 7 to 8.
[0080] In the dissolution step, a newly prepared aqueous solvent may be brought into contact with the ceramic material from which the platinum group compound has been dissolved using the aqueous solvent, and the same treatment may be performed to dissolve the platinum group compound. In addition, this operation may be repeated to repeatedly dissolve the platinum group compound. In such a method of repeatedly dissolving, the composition of the aqueous solvent in each of the repeated steps is not limited, and aqueous solvents of different compositions may be used in each repeated step. For example, after dissolving the platinum group compound in an aqueous solvent containing 98% by weight or more of water, the platinum group compound may be further dissolved in an aqueous solvent containing 80% by weight or more and 90% by weight or less of water.
[0081] In this way, when the platinum group compound dissolution operation is repeatedly performed using aqueous solvents of different compositions, different types of platinum group compounds can be dissolved in stages. For example, when a raw material containing multiple platinum group metals is used to perform the immobilization process, the multiple platinum group compounds are immobilized on a ceramic material. In this case, for example, after platinum group compound A is dissolved in an aqueous solvent containing 98% by weight or more of water, platinum group compound B can be further dissolved in an aqueous solvent containing 80% by weight or more and 90% by weight or less of water, and different types of platinum group compounds can be dissolved in aqueous solvents of different compositions. In addition, the aqueous solvents used in each repeated process can be used as different aqueous solvents by changing the concentration of the acid, or by changing the type of the acid.
[0082] In addition, by adjusting the composition of the melt in the fixing step by increasing or decreasing the amount of oxides contained in the melt, etc., the solubility of the platinum group compound from the ceramic material into the aqueous solvent can be adjusted in the dissolution step. For example, the amount of oxides can be adjusted so that the platinum group compound is appropriately dissolved in the aqueous solvent containing 98% by weight or more of water. In addition, by reducing the amount of oxides contained in the melt, it can be adjusted so that the platinum group compound is more appropriately dissolved in the aqueous solvent containing 80% by weight or more and 90% by weight or less of water, compared with the case where the platinum group compound is dissolved in the aqueous solvent containing 98% by weight or more of water.
[0083] In order to adjust the solubility of the platinum group compound, an oxidant other than carbonate or hydroxide of an alkali metal may be contained in the melt in the immobilization step. Examples of such oxidants include solutions containing air, oxygen, hydrogen peroxide, and high-valent cations. Oxygen or high-valent cations are preferred among the above oxidants because they have the advantage of being able to rapidly oxidize the platinum group metal. Examples of high-valent cations include Fe 3+ 、Ce 4+ and Co 3+ .
[0084] Such an oxidizing agent is preferably added to the melt before or during heating of the melt. The presence of the oxidizing agent during heating allows efficient oxidation of the platinum group metal. The oxidizing agent is not limited thereto and may be added after heating of the melt or during dissolution of the platinum group compound into an aqueous solvent.
[0085] <4. Extraction process>
[0086] The method for recovering platinum group metals of the present embodiment may include an extraction step of extracting the platinum group metals from the eluate obtained in the above-mentioned elution step into an organic solvent. This step may be performed by a conventional method for extracting platinum group metals based on organic solvent treatment.
[0087] According to this method for extracting platinum group metals, platinum group metals in waste catalysts and waste materials can be selectively extracted in a low-corrosion environment without using harmful acidic solvents such as aqua regia or highly concentrated hydrochloric acid.
[0088] As the organic solvent, for example, dialkyl sulfide, hydroxyoxime, 8-quinolinol, tertiary amine or trialkyl phosphate can be used. If hydroxyoxime is used as the organic solvent, Pd can be selectively extracted from the platinum group metals, and if tertiary amine is used as the organic solvent, Pt can be selectively extracted from the platinum group metals. In addition, after Pd and Pt are extracted from the eluate, if tertiary amine is used as the organic solvent, Ir can be selectively extracted from the remaining platinum group metals, and Rh can be obtained by purifying the eluate after the extraction. Ru and Os can be volatilized and separated by distillation in these separation steps.
[0089] <5. Compositions containing platinum group metals>
[0090] The platinum group metal-containing composition of the present embodiment contains a platinum group metal and an amphoteric element, and contains 99% by weight or more of the platinum group metal and 1% by weight or less of the amphoteric element, when the total amount of the platinum group metal and the amphoteric element is 100% by weight.
[0091] Examples of the platinum group metal include Pd, Pt, Rh, Ir, Os, and Ru.
[0092] Examples of the amphoteric element include Al, Ti, V, Co, and Zr. Among them, Al and Ti are more preferred.
[0093] Such a method for obtaining a composition containing platinum group metals can be exemplified by the methods described in the above <2. Immobilization step> and <3. Dissolution step>, but is not limited thereto. Thus, a method for recovering platinum group metals according to one embodiment of the present invention can be considered as a method for producing a composition containing platinum group metals. That is, a method for recovering platinum group metals according to one embodiment of the present invention can be considered as a method for producing a composition containing platinum group metals including a method for recovering platinum group metals, characterized in that it comprises an immobilization step, wherein the immobilization step brings a melt of a raw material containing platinum group metals, a melt of an alkali metal carbonate or hydroxide, a melt of an oxide, and a ceramic material into contact, so that the platinum group metals are immobilized on the ceramic material.
[0094] As a specific example of a composition containing a platinum group metal, for example, a composition in which a platinum group metal is dissolved into an aqueous solvent. An aqueous solvent refers to a solvent containing water as a main component, for example, a solvent containing at least 60% by weight, preferably 70% by weight, more preferably 80% by weight, more preferably 90% by weight, more preferably 95% by weight, more preferably 98% by weight, and most preferably 100% by weight of water. The upper limit of the amount of water contained in the aqueous solvent is not particularly limited, for example, it can be 80% by weight, 90% by weight or 100% by weight. In addition, the aqueous solvent is preferably an aqueous solution of an acid. Regarding the type of the acid, for example, organic acids such as citric acid, malic acid, acetic acid and oxalic acid, and inorganic acids such as hydrochloric acid, nitric acid, sulfuric acid, boric acid, phosphoric acid and perchloric acid can be listed. Regarding the concentration of the acid, for example, it can be 3 mol / L or less, preferably 1 mol / L or less, more preferably 0.1 mol / L or less, and further preferably 0.01 mol / L or less. In addition, regarding the concentration of the acid, an appropriate concentration can be selected according to the type of the acid. In addition, the aqueous solvent may not contain an acid.
[0095] The composition containing platinum group metals, for example, contains the platinum group metals and amphoteric elements dissolved from a ceramic material in which the platinum group metals are fixed in an aqueous solvent. When the total amount of the platinum group metals and the amphoteric elements is set to 100 weight %, the composition can be a platinum group metal eluate containing 99 weight % or more of the platinum group metals and 1 weight % or less of the amphoteric elements. If it is such a platinum group metal-containing composition, the platinum group metals contained in the eluate can be easily extracted by the conventional method for extracting platinum group metals based on organic solvent treatment. In addition, the composition containing platinum group metals can also be a composition (e.g., a solid substance) in the form of a platinum group metal eluate in which the aqueous solvent is removed.
[0096] Examples of a method for obtaining a platinum group metal-containing composition as a solid substance include a method of further concentrating the eluate obtained in the above <3. Elution step>.
[0097] In the concentration step, activated carbon is immersed in the eluate to adsorb the platinum group compound on the activated carbon. At this time, the eluate immersed in the activated carbon is preferably stirred. Then, the activated carbon adsorbed with the platinum group compound is taken out from the eluate and heated to burn the activated carbon. The heating of the activated carbon is not limited as long as it is a temperature at which the activated carbon burns, for example, 1000°C. The concentrate obtained after the heating of the activated carbon contains concentrated platinum group metals. This concentrate is an example of a composition containing platinum group metals according to an embodiment of the present invention.
[0098] <6. Ceramic materials with fixed platinum group metals>
[0099] The ceramic material of the present embodiment has an immobilized layer containing O (oxygen) and an alkali metal formed on the surface of the ceramic material, and a platinum group metal is immobilized in the immobilized layer.
[0100] For example, according to the method described in (2-1. Preparation of melt) above, if a melt containing a platinum group compound is brought into contact with a ceramic material, a fixed layer is formed on the surface of the ceramic material. A composite layer containing O and an alkali metal from a carbonate or hydroxide of an alkali metal is formed in the fixed layer. In addition, it is preferred that the fixed layer also contains elements from oxides contained in the above-mentioned melt. Elements from such oxides may be elements from mesh-forming oxides, elements from mesh-modifying oxides, or elements from both mesh-forming oxides and mesh-modifying oxides. Here, mesh-forming oxides refer to oxides that can form a mesh structure of glass during vitrification. In addition, mesh-modifying oxides refer to oxides that can modify the mesh structure of glass during vitrification. These oxides can be added in a vitrified state when a melt containing a platinum group compound is obtained, but vitrification is not necessary.
[0101] As the element derived from the oxide, for example, at least one selected from the group consisting of Na, B, K, Si, Li, Rb, Cs, and P can be used.
[0102] As an example of a fixed layer, when the ceramic material is aluminum oxide, the oxides contained in the above-mentioned melt are B2O3 and K2O, and the carbonate of the alkali metal is K2CO3, a K-Al-BO composite layer (for example, K2Al2(BO3)2O) can be cited, but it is not limited to this. As another example of a fixed layer, a composite layer (for example, a Na-Al-BO composite layer) in which at least one atom constituting the K-Al-BO composite layer is replaced with an atom having similar properties can be cited. In addition, the fixed layer can also be a K-Al-O composite layer that does not contain B from the oxide.
[0103] The present inventors have discovered that such an immobilization layer has the property of being able to immobilize a platinum group metal. Based on this finding, the present inventors have obtained a ceramic material on which a platinum group metal is immobilized. The method for obtaining such a ceramic material on which a platinum group metal is immobilized can be, for example, the method described in <2. Immobilization step> above, but is not limited thereto.
[0104] Examples of the platinum group metal fixed to the ceramic material include Pd, Pt, Rh, Ir, Os and Ru.
[0105] In addition, the ceramic material can be any sintered body obtained by heat treating an inorganic material, and the specific composition is not limited. The ceramic material in contact with the melt is preferably a ceramic material of a metal oxide system. Such a ceramic material can more effectively immobilize a water-soluble platinum group compound. The ceramic material can contain aluminum oxide, zeolite, zirconium oxide, silicon dioxide, iron oxide, cobalt oxide, nickel oxide, or a mixture of two or more substances selected from them.
[0106] From the viewpoint of effectively fixing the platinum group compound, the ceramic material is preferably porous and has a large surface area.
[0107] The surface of the ceramic material may be any surface that can contact the liquid when the ceramic material is immersed in a liquid such as a melt or an aqueous solvent. For example, when the ceramic material is porous, not only the surface that can be visually confirmed from the appearance of the ceramic material, but also the surface formed inside the pores is also the surface of the ceramic material.
[0108] <7. Conclusion>
[0109] A method for recovering platinum group metals according to one embodiment of the present invention comprises a fixation step, wherein a melt of a raw material containing platinum group metals, a melt of carbonate or hydroxide of an alkali metal, a melt of an oxide, and a ceramic material are brought into contact with each other to fix the platinum group metals on the ceramic material.
[0110] In the method for recovering a platinum group metal according to one embodiment of the present invention, the immobilization step may include causing the ceramic material to adsorb the platinum group metal, or causing a component eluted from the ceramic material to co-precipitate with the platinum group metal.
[0111] In the method for recovering platinum group metals according to one embodiment of the present invention, in the fixation step, after heating the raw material containing the platinum group metal, the carbonate or hydroxide of the alkali metal, and the oxide to obtain the melt, the melt may be brought into contact with the ceramic material.
[0112] In one embodiment of the method for recovering platinum group metals of the present invention, in the above-mentioned fixation step, after obtaining a mixture containing the raw material of the above-mentioned platinum group metal, the carbonate or hydroxide of the above-mentioned alkali metal, the above-mentioned oxide and the above-mentioned ceramic material, the above-mentioned melt is obtained by heating the mixture, and the melt is brought into contact with the above-mentioned ceramic material.
[0113] In the method for recovering platinum group metals according to one embodiment of the present invention, the ceramic material may contain alumina, zeolite, zirconia, silica, iron oxide, cobalt oxide, or nickel oxide.
[0114] In the method for recovering a platinum group metal according to one embodiment of the present invention, a leaching step may be provided after the immobilization step. In the leaching step, the ceramic material in which the platinum group metal is immobilized is brought into contact with an aqueous solvent, and the platinum group metal is leached from the ceramic material.
[0115] In the method for recovering a platinum group metal according to one embodiment of the present invention, the aqueous solvent may be an aqueous solution of an acid.
[0116] In the method for recovering a platinum group metal according to one embodiment of the present invention, the contact between the melt and the ceramic material may be carried out at a temperature of 600 to 1100°C.
[0117] In the method for recovering a platinum group metal according to one embodiment of the present invention, the contact between the melt and the ceramic material may be carried out in the presence of an oxygen anion of an amphoteric element.
[0118] In the method for recovering a platinum group metal according to one embodiment of the present invention, the platinum group metal may be Pd, Pt, Rh, Ir, Os, or Ru.
[0119] In the method for recovering a platinum group metal according to one embodiment of the present invention, the alkali metal may be Na, K, Li, Rb, or Cs.
[0120] In the method for recovering a platinum group metal according to one embodiment of the present invention, the oxide may be at least one selected from the group consisting of Na2O, B2O3, K2O, SiO2, Li2O, Rb2O, Cs2O, and P2O5.
[0121] A composition containing a platinum group metal according to one embodiment of the present invention contains a platinum group metal and an amphoteric element. When the total amount of the platinum group metal and the amphoteric element is set to 100% by weight, it contains 99% by weight or more of the platinum group metal and 1% by weight or less of the amphoteric element.
[0122] A ceramic material according to one embodiment of the present invention has an immobilization layer containing at least one selected from the group consisting of Na, B, K, Si, Li, Rb, Cs, and P, O, and an alkali metal formed on the surface, and a platinum group metal is immobilized in the immobilization layer.
[0123] Examples
[0124] [A. Immobilization of Platinum Group Metal Based on Alumina Block]
[0125] [A1. Specimen and Method]
[0126] (A1-1. Reaction Medium)
[0127] The K2O-B2O3 medium as an example of the oxide of the present invention is prepared using a commercially available compound standard reagent in the following manner. First, 5 g of boric acid and 2.1 g of potassium hydroxide are put into an alumina crucible with a capacity of 30 mL (hereinafter referred to as "30 mL crucible"), and the 30 mL crucible is set in an electric furnace. Then, the temperature in the electric furnace is raised to 1000°C in 30 minutes, and the 30 mL crucible is heated for 1 hour while maintaining the temperature. Then, the molten material generated in the 30 mL crucible is cooled. The obtained solidified material is used as the K2O-B2O3 medium.
[0128] This reaction medium with boron oxide as the main component has a network structure, and the network structure is based on a planar triangular BO3 structure, and the BO3 structure is combined into a mesh structure. If K2O is contained in this reaction medium, BO4 with a tetrahedral structure is generated. It is known that BO4 in the network structure has a negative charge as a whole. Therefore, BO4 in the network structure can be regarded as an oxygen anion. It can be considered that by containing oxygen anions in the reaction medium, platinum group metals can be more effectively converted into platinum group compounds. Therefore, such a K2O-B2O3 medium is used as a reaction medium for converting platinum group metals into platinum group compounds.
[0129] (A1-2. Formation of platinum group compound in comparative example)
[0130] The K2O-B2O3 medium prepared in (A1-1) above, metal Pd and potassium carbonate (an example of the carbonate or hydroxide of the alkali metal of the present invention) were mixed. The obtained mixture was added to a 30 mL crucible, and the 30 mL crucible was set in a 100 mL alumina crucible (hereinafter referred to as "100 mL crucible"). Then, the 100 mL crucible was covered and heated in an electric furnace. The following Table 1 shows the heating conditions.
[0131] In the melt obtained by the above heating, metal Pd is oxidized by reaction with potassium carbonate to generate an oxidation product of metal Pd. Then, the oxidation product is dissolved in the K2O-B2O3 medium. The product obtained by cooling such a melt is defined as a heat-treated product.
[0132] [Table 1]
[0133]
[0134] (A1-3. Production of platinum group compounds in examples of the present invention)
[0135] The K2O-B2O3 medium, metal Pd and potassium carbonate prepared in the above (A1-1) are mixed. The mixture is added to a 10mL alumina crucible (hereinafter referred to as "10mL crucible"), and the 10mL crucible is set in a 30mL crucible. The 30mL crucible is heated in an electric furnace. The above Table 1 shows the heating conditions. Through this heating, as in the above (A1-2), the Pd compound, which is an oxidation product of metal Pd, is dissolved in the K2O-B2O3 medium. Then, an alumina block (an example of the ceramic material of the present invention) is immersed in the melt in which the Pd compound is dissolved, and kept for a specified time. Then, the alumina block is taken out from the melt.
[0136] (A1-4. Evaluation of Recovery Rate of Platinum Group Compounds)
[0137] In order to evaluate the amount of Pd compound immobilized in the alumina block, the following test was performed. The heat-treated product (comparative example) or the alumina block (example) was placed in a 200 mL beaker together with a crucible, and 150 mL of ion exchange water was added to the beaker (dissolution treatment). The stirring rod was immersed in the liquid in the beaker and stirred at a stirring speed of 7000 rpm for 2 hours. Then, the liquid (dissolution liquid) in the beaker was filtered by suction with a 1 μm filter paper. On the other hand, for the solid (alumina block or heat-treated product) remaining in the beaker after filtration, 0.01M hydrochloric acid aqueous solution (0.01M HCl) was used again. After dissolution treatment, stirring and filtering were carried out in the same manner as above, the obtained solid was further dissolved, stirred and filtered in the same manner as above using 0.1M hydrochloric acid aqueous solution (0.1MHCl) and 1M hydrochloric acid aqueous solution (1M HCl). The concentration of the Pd compound in each eluate obtained by the series of operations was measured using an ICP emission spectrometer, and the recovery rate of the platinum group metal was calculated from the following formula (1).
[0138] Recovery rate (%) = amount of platinum group compound in the eluate / amount of platinum group metal added × 100 (1)
[0139] (A1-5. Immobilization Conditions of Pd Compound in Each Example and Comparative Example)
[0140] In order to clarify the relationship between the fixation conditions of the Pd compound and the Pd recovery rate, the amount of alumina blocks added to the melt and the conditions for immersing the alumina blocks in the melt were changed in Examples A1 to A4 as shown in Table 2. In contrast, in Comparative Example A1, the alumina blocks were not added to the melt, and the reaction medium was subjected to dissolution treatment together with the heat-treated product.
[0141] [Table 2]
[0142]
[0143] <A2. Result>
[0144] (Confirmation of immobilization of A2-1. Pd compound to alumina block)
[0145] After simply washing 0.6 g of alumina block taken out from the melt of Example A1 with ion-exchanged water for a short time, it was dried, and the surface of the alumina block was observed by SEM-EDS (scanning electron microscope - energy dispersive X-ray spectroscopy). Figure 1 It is a figure showing an image of observing the surface of the alumina block by SEM-EDS. As Figure 1 shown, submicron-sized particles exist on the surface of the alumina block.
[0146] Figure 2 It is a figure showing the EDS spectrum of submicron-sized particles ( Figure 1 part P) in the surface of the alumina block. According to Figure 2 the results shown and Figure 1 the Pd mapping image of EDS shown, it shows that the particles contain Pd compounds. As described above, the alumina block observed by SEM-EDS is an alumina block from which salts from the reaction medium attached to the surface have been removed by washing with ion-exchanged water. Thus, it can be considered that Pd on the surface of the alumina block is immobilized by adsorption from the reaction medium to the surface of the alumina block. In this way, according to the platinum group metal recovery method of one embodiment of the present invention, it shows that platinum group compounds can be easily separated from the melt.
[0147] (A2-2. Recovery of Pd compound immobilized on alumina block)
[0148] Figure 3 It is a figure showing the Pd recovery rate from the alumina block during the dissolution treatment of the alumina blocks of Examples A2 to A4. As shown in the above (A1-4), four kinds of aqueous solvents were used stepwise in the dissolution treatment. In the following evaluation, the total value of the Pd dissolution rate in each aqueous solvent was used as an index of the Pd recovery rate.
[0149] In Example A2, starting from the beginning of the temperature rise of an electric furnace equipped with a 30 mL crucible, alumina blocks were added to the mixture in a 10 mL crucible. Under the conditions of Example A2, the Pd recovery rate was 12%. In contrast, in Example A3, the electric furnace was heated to a temperature of 900 °C, and 30 minutes after reaching 900 °C, the alumina blocks were added to the melt in a 10 mL crucible. Under the conditions of Example A3, the Pd recovery rate was 25%. In Example A4, the dissolution treatment was carried out in such a way that the input amount of the alumina blocks was 2 g and other conditions were the same as in Example A3. Under the conditions of Example A4, the Pd recovery rate was 33%, which was increased compared with Example A3. From the above, it is shown that by changing the impregnation conditions and input amount of the alumina blocks, etc., the adsorption of Pd compounds onto the surface of the alumina blocks can be promoted.
[0150] (Concentration of boron in the Pd dissolution solution in A2-3)
[0151] Table 3 below shows the concentrations of Pd compounds and boron in the Pd dissolution solution in Comparative Example A1 and Example A3. In Comparative Example A1, a dissolution solution was obtained by subjecting the heat treatment product containing the reaction medium to a dissolution treatment with ion-exchanged water. The concentration of boron in this dissolution solution was 753 mg / L. In contrast, the concentration of boron in the dissolution solution using ion-exchanged water in Example A3 was 204 mg / L, and the boron concentration was significantly reduced compared with Comparative Example A1. In addition, the concentration of boron in a 0.01 - 1 M hydrochloric acid aqueous solution was in the range of 5.8 - 9.3 mg / L, and the boron concentration was lower compared with Comparative Example A1. Thus, according to the method for recovering platinum group metals according to one embodiment of the present invention, it is shown that the concentration of oxide salts in the dissolution solution can be effectively reduced.
[0152] [Table 3]
[0153]
[0154] In addition, in Example A3, when the alumina blocks were taken out from the melt, a part of the melt containing the K2O - B2O3 medium adhered to the alumina blocks. Therefore, it can be considered that in the dissolution treatment, boron from the K2O - B2O3 medium adhering to the alumina blocks was dissolved into the dissolution solution of ion-exchanged water. Therefore, it can be considered that by improving the separability between the alumina blocks and the K2O - B2O3 medium and reducing the adhesion of the K2O - B2O3 medium to the alumina blocks as described above, the transfer of boron into the dissolution solution can be further suppressed.
[0155] [B. Immobilization of platinum group metals on alumina powder]
[0156] [B1. Samples and methods]
[0157] 1 g of a K2O-B2O3 medium prepared in the same manner as the above (A1-1), 3.9 g of a platinum group metal, potassium carbonate, and 1 g of alumina powder (an example of the ceramic material of the present invention) were mixed. As the platinum group metal, 10 mg of metallic Pd or 12 mg of metallic Pt was used. The mixture was placed in a 10 mL crucible, and the 10 mL crucible was placed in a 30 mL crucible. The 30 mL crucible was heated in an electric furnace. The heating temperature was 900 °C or 600 °C for the mixture containing metallic Pd, and 900 °C for the mixture containing metallic Pt, and the heating time was 30 minutes. By this heating, the platinum group compound, which is an oxidation product of the platinum group metal, was dissolved in the K2O-B2O3 medium. Then, the platinum group compound dissolved in the melt was immobilized on the surface of the alumina powder. Then, a mixture of the alumina powder and the melt was obtained.
[0158] The mixture of the alumina powder and the melt was immersed in 150 mL of ion-exchanged water for 2 hours and washed, and the surface state of the alumina powder was analyzed. For the immobilization state of the platinum group metal on the surface of the alumina powder, SEM-EDS, XRD (X-ray diffractometer), or XPS (photoelectron spectrometer) was used for analysis.
[0159] <B2. Results>
[0160] (B2-1. Confirmation of immobilization of Pd compound on alumina powder heated at 900 °C)
[0161] Figure 4 The XRD diffraction pattern of the alumina powder (Example B1) washed after heating at 900 °C under the condition containing metallic Pd is shown. As Figure 4 shown, the XRD diffraction pattern of Al2O3 (the peak group indicated by the circle marks in Figure 4 ) and the XRD diffraction pattern of K2Al2(BO3)2O (the peak group indicated by the downward triangle marks in Figure 4 ) are included in the XRD diffraction pattern of Example B1. From this result, it is shown that an immobilized layer containing K2Al2(BO3)2O is formed on the surface of the alumina powder of Example B1.
[0162] Figure 5 The XPS spectrum of the alumina powder of Example B1 is shown. As Figure 5 shown, peaks indicating Pd are observed in the XPS spectrum of Example B1. In addition, the peaks indicating these Pds are shifted to the high energy side from the position of the peak of normal metallic Pd (the peak indicated by Pd Figure 5 in 0 ). This is the result indicating that Pd exists in an oxidized state on the surface of the alumina powder.
[0163] The above results show that a fixed layer containing K2Al2(BO3)2O is formed on the surface of the alumina powder of Example B1 in which the heating temperature in the melt is set to 900°C, and Pd is fixed in the fixed layer.
[0164] (B2-2. Confirmation of fixation of Pd compound to alumina powder heated at 600° C.)
[0165] Figure 6 FIG. 4 shows the XRD diffraction pattern of the aluminum oxide powder (Example B2) heated at 600° C. in the presence of metal Pd. Figure 6 As shown, when the heating temperature is set to 600°C, the XRD diffraction pattern of Al2O3 is observed from the XRD diffraction pattern of Example B2 (at Figure 6 The peak group represented by the diamond mark in the graph is not observed, but the peaks of other molecules are not observed. Therefore, the surface state of the aluminum oxide powder of Example B2 was observed using SEM-EDS.
[0166] Figure 7 This is a diagram showing an image of the surface of the aluminum oxide powder of Example B2 observed by SEM-EDS. Figure 7 The image shown in the upper left of the figure shows the secondary electron image of the surface of the aluminum oxide powder of Example B2, and the other images show the secondary electron image of the surface of the aluminum oxide powder of Example B2. Figure 7 Element mapping images of the elements shown. Figure 7 As shown, Pd, K and O were observed on the surface of the alumina powder of Example B2, respectively.
[0167] Figure 8 : is a graph showing the EDS spectrum of the aluminum oxide powder of Example B2. Figure 8 Shown in Figure 7 The EDS spectrum of the entire observation area is shown. Figure 8 As shown in FIG. 1 , C, O, Al, Pd and K are present in the alumina powder of Example B2. Figure 7 In the image shown in the upper left of , there are 47.4 wt% O, 32.3 wt% Al, 19.6 wt% Pd, and 0.71 wt% K in the range indicated by the circular frame. That is, it is shown that a composite containing at least Pd, K, Al, and O is formed on the surface of the alumina powder of Example B2.
[0168] The above results show that metal Pd is fixed on the surface of the aluminum oxide powder of Example B2 obtained by setting the heating temperature in the melt to 600° C. Therefore, it is considered that a fixing layer capable of fixing metal Pd is formed on the surface of the aluminum oxide powder of Example B2, but when the heating condition is 600° C., the fixing layer does not contain a detectable amount of B. That is, it is shown that the fixing layer can fix metal Pd even in a state where it does not contain B derived from the oxide.
[0169] (B2-3. Confirmation of fixation of Pt compound to alumina powder heated at 900° C.)
[0170] Fig. 9 FIG. 4 shows the XRD diffraction pattern of the aluminum oxide powder (Example B3) which was heated at 900° C. and then washed in the presence of metal Pt. Fig. 9 As shown, the XRD diffraction pattern of Example B3 contains the XRD diffraction pattern of Al2O3 (in Fig. 9 The peak groups indicated by diamond marks in the figure) and the XRD diffraction patterns of K2Al2(BO3)2O (in Fig. 9 The results show that a fixed layer containing K2Al2(BO3)2O is formed on the surface of the aluminum oxide powder of Example B3.
[0171] Fig.10 This is a diagram showing an image of the surface of the aluminum oxide powder of Example B3 observed by SEM-EDS. Fig.10 The image shown in the upper left corner of the figure shows the secondary electron image of the surface of the aluminum oxide powder of Example B3, and the other images show the secondary electron image of the surface of the aluminum oxide powder of Example B3. Fig.10 Element mapping images of the elements shown. Fig.10 As shown, Pt, K and O were observed on the surface of the alumina powder of Example B3, respectively.
[0172] Fig.11 : is a graph showing the EDS spectrum of the aluminum oxide powder of Example B3. Fig.11 Shown in Fig.10 The EDS spectrum of the entire observation area is shown. Fig.11 As shown in FIG. 1 , C, O, Al, Pt and K are present in the alumina powder of Example B3. Fig.10 In the image shown in the upper left of , there are 54.6 wt% O, 19.7 wt% Al, 3.2 wt% Pt, and 9.5 wt% K in the range indicated by the circular frame. That is, it is shown that a composite containing at least Pt, K, Al, and O is formed on the surface of the alumina powder of Example B3.
[0173] From the above results, it is shown that Pt metal is immobilized on the surface of the alumina powder of Example B3 obtained by setting the heating temperature in the melt at 900°C. Therefore, it is shown that not only Pd metal but also Pt metal can be immobilized on the surface of the alumina powder of Example B3, forming an immobilized layer.
[0174] 〔C. Composition of the Pd-containing composition〕
[0175] <C1. Specimen and method>
[0176] A mixture of alumina powder and melt prepared by the same method as (B1-1) above was placed in a 200 mL beaker, and 150 mL of ion-exchanged water was added to the beaker. A stir bar was immersed in the liquid in the beaker and stirred at a stirring speed of 7000 rpm for 30 minutes. Then, for the mixture remaining in the beaker, a 1M hydrochloric acid aqueous solution (1M HCl) was used and stirred in the same method as above for 30 minutes. The mixture was taken out from the treatment liquid based on the obtained 1M hydrochloric acid aqueous solution, and 3 g of activated carbon was immersed in the treatment liquid. A stir bar was immersed in the liquid in the beaker and stirred at a stirring speed of 7000 rpm for 30 minutes.
[0177] Next, the activated carbon was taken out from the beaker and heated at 1000°C for 4 hours to burn the activated carbon. The Pd concentrate (an example of the platinum group metal-containing composition of the present invention) obtained after heating was analyzed by SEM-EDS.
[0178] <C2. Results>
[0179] Fig.12 is a diagram showing an image of observing the surface of the Pd concentrate by SEM-EDS. Fig.12 The image shown in the upper left represents the secondary electron image of the surface of the Pd concentrate, and the other images respectively represent Fig.12 element mapping images of the respective elements shown. As Fig.12 shown, Pd and O are observed on the surface of the Pd concentrate.
[0180] Fig.13 is a diagram showing the EDS spectrum of the Pd concentrate. In Fig.13 is shown Fig.12 the overall EDS spectrum of the observation region shown. As Fig.13 shown, C, O, Cu, Al, Si, and Pd are present in the Pd concentrate. In addition, in Fig.12In the image shown in the upper left, within the range indicated by the circular frame, there is 84.48 wt% of Pd, 9.08 wt% of C, 3.71 wt% of O, 1.9 wt% of Cu, 0.45 wt% of Al, and 0.38 wt% of Si. Among them, since Cu and Si were not added to the melt, it can be considered that they are components from the activated carbon. In addition, it can be considered that C and O are unburned carbon from the activated carbon and the oxygen combined with it. Therefore, it can be considered that the component from the molten salt formed in the Pd concentrate and present in the melt is only Al.
[0181] Therefore, if the composition ratio is recalculated based on only Pd and Al among the components detected by the EDS spectrum of the Pd concentrate, it is 99.47 wt% of Pd and 0.53 wt% of Al.
[0182] As shown above, the platinum group metal-containing composition obtained by the recovery method of the platinum group metal according to one embodiment of the present invention contains a platinum group metal and an amphoteric element. In addition, it is shown that in such a platinum group metal-containing composition, when the total amount of the platinum group metal and the amphoteric element is set to 100 wt%, it contains 99 wt% or more of the platinum group metal.
[0183] [Platinum group metals other than Pd and ceramic materials other than alumina]
[0184] [D1. Samples and methods]
[0185] (D1-1. Generation of platinum group compounds)
[0186] Mix 1 g of the K2O-B2O3 medium prepared by the same method as above (A1-1), 10 mg of a platinum group metal (metal Pt or metal Rh), and 3.9 g of potassium carbonate. Add this mixture to a 10 mL crucible, and place this 10 mL crucible inside a 30 mL crucible. Heat the 30 mL crucible in an electric furnace. In addition, in this 10 mL crucible, there are holes smaller in diameter than alumina balls or zirconia balls. The heating temperature is 900 °C or 1000 °C, and the heating time is 30 minutes. Through this heating, the platinum group compound, which is the oxidation product of the platinum group metal, dissolves in the K2O-B2O3 medium. Then, immerse the ceramic material in the melt in which the platinum group compound is dissolved for a specified time (immersion time). As the ceramic materials, ten alumina balls with a diameter of about 4 mm or zirconia balls with a diameter of 2.8 - 3.2 mm are used respectively. These alumina balls and zirconia balls are all examples of the ceramic materials of the present invention. Then, take out the alumina balls or zirconia balls together with the 10 mL crucible from the melt.
[0187] (D1-2. Evaluation of the recovery rate of platinum group compounds)
[0188] In order to evaluate the amount of platinum group compounds immobilized on the surface of the ceramic material, the following tests were conducted. The ceramic material and the crucible were placed in a 200 mL beaker, and 150 mL of ion-exchanged water (leaching treatment) was added to the beaker. A stir bar was immersed in the liquid in the beaker, and the mixture was stirred at a stirring speed of 7000 rpm for 30 minutes. Then, the liquid in the beaker (leachate) was suction-filtered using a 1 μm filter paper.
[0189] On the other hand, for the ceramic material remaining in the beaker after filtration, a 0.01 M hydrochloric acid aqueous solution (0.01 M HCl) was used again, and the leaching treatment, stirring, and filtration were carried out in the same manner as described above. For the alumina balls of Example D11 and the zirconia balls of Example D12 shown in Table 4 below, a 0.1 M hydrochloric acid aqueous solution (0.1 M HCl) and a 1 M hydrochloric acid aqueous solution (1 M HCl) were used, and the remaining ceramic material was further subjected to leaching treatment, stirring, and filtration in the same manner as described above in sequence. The concentration of platinum group compounds in each leachate obtained through these series of operations was measured using an ICP emission analyzer, and the recovery rate of platinum group metals was calculated by the above formula (1).
[0190] (D1-3. Conditions in each example)
[0191] In order to clarify the relationship among the types of platinum group metals, the types of ceramic compounds, the immobilization conditions of platinum group compounds, and the dissolution rate of platinum group compounds, the dissolution rate was measured under each condition shown in Table 4 below. In Examples D1 to D10, metal Pt was used as the platinum group metal, and alumina balls were used as the ceramic material, and the impregnation conditions of the alumina balls into the melt were changed. In Example D11, metal Rh was used as the platinum group metal, and alumina balls were used as the ceramic material. In Example D12, metal Pt was used as the platinum group metal, and zirconia balls were used as the ceramic material.
[0192] [Table 4]
[0193]
[0194] <D2. Results>
[0195] The results of Examples D1 to D12 show that according to the recovery method of platinum group metals according to an embodiment of the present invention, metals Pt and Rh can also be recovered using an aqueous solvent. That is, it is shown that for metals Pt and Rh, immobilization can also be achieved through the immobilization layer formed on the surface of the ceramic material.
[0196] In addition, as shown in Example D1 etc., metallic Pt is mainly eluted from the surface of the ceramic material by ion-exchanged water. On the other hand, as shown in Example D11, metallic Rh is hardly eluted in ion-exchanged water and is effectively eluted by a 0.01 M hydrochloric acid aqueous solution. Thus, it is shown that although the optimal elution conditions vary depending on the type of platinum group metal, it is possible to effectively recover from the surface of the ceramic material by an aqueous solvent regardless of the type of platinum group metal. In addition, it is shown that by using a plurality of aqueous solvents, different types of platinum group metals can be separated and recovered.
[0197] In addition, as shown in Example D12, it is shown that the ceramic material is not limited to alumina, and various ceramic materials such as zirconia can be applied to the method for recovering platinum group metals according to one embodiment of the present invention.
[0198] 〔E. Types of Hydroxides and Oxides of Alkali Metals〕
[0199] <E1-1. Samples and Methods>
[0200] As the melt of the oxide, 1 g of a K2O-B2O3 medium (Example E1) prepared by the same method as above (A1-1) or 0.5 g of phosphorus pentoxide (P2O5) (Example E2), 11 mg of metallic Pt, and 4.4 g of potassium hydroxide were mixed. This mixture was placed in a 10 mL crucible, and the 10 mL crucible was placed in a 30 mL crucible. The 30 mL crucible was heated in an electric furnace. In addition, a hole smaller in diameter than the alumina ball or zirconia ball was provided in the 10 mL crucible here. The heating temperature was 900 °C and the heating time was 30 minutes. By this heating, the Pt compound, which is the oxidation product of metallic Pt, was dissolved in the melt of the oxide. Then, ten alumina balls (an example of a ceramic material) having a diameter of about 4 mm were immersed in the melt in which the Pt compound was dissolved for 60 minutes. Then, in Example E1, the alumina balls were taken out of the melt together with the 10 mL crucible, and in Example E2, only the alumina balls were taken out of the melt.
[0201] (E1-2. Evaluation of Recovery Rate of Pt Compound)
[0202] In order to evaluate the amount of the Pt compound immobilized on the surface of the alumina balls, the following test was conducted. The alumina balls together with the crucible (Example E1), or only the alumina balls (Example E2) were placed in a 200 mL beaker, and 150 mL of ion-exchanged water was added to the beaker (elution treatment). A stir bar was immersed in the liquid in the beaker, and the liquid was stirred at a stirring speed of 7000 rpm for 30 minutes. Then, the liquid in the beaker (eluate) was suction-filtered using a 1 μm filter paper.
[0203] On the other hand, regarding the alumina balls remaining in the beaker after filtration, the dissolution treatment, stirring, and filtration were successively performed again using 0.01 M hydrochloric acid aqueous solution (0.01 M HCl), 0.1 M hydrochloric acid aqueous solution (0.1 M HCl), and 1 M hydrochloric acid aqueous solution (1 M HCl) in the same manner as described above. The concentration of the Pt compound in each eluate obtained through these series of operations was measured using an ICP emission analyzer, and the recovery rate of metallic Pt was calculated by the above formula (1).
[0204] <E2. Results>
[0205] Table 5 below shows the results of Example E1 and Example E2.
[0206] [Table 5]
[0207]
[0208] From the results of Example E1 and Example E2, it is shown that in the method for recovering platinum group metals according to one embodiment of the present invention, it can be applied not only to carbonates of alkali metals but also to hydroxides of alkali metals. In addition, from the results of Example E2, it is shown that as the oxide, it is not limited to the K2O - B2O3 medium, and the method for recovering platinum group metals according to one embodiment of the present invention can also be implemented using, for example, phosphorus pentoxide (P2O5).
[0209] In addition, the carbonate or hydroxide of an alkali metal functions as an oxidizing agent for oxidizing platinum group metals as described above. As the alkali metal, in addition to K, using Na, Li, Rb, or Cs also functions as an oxidizing agent in the same manner as K and forms soluble platinum group compounds in the medium. Therefore, it is considered that the carbonates or hydroxides of Na, Li, Rb, or Cs are equally suitable as oxidizing agents as the carbonates or hydroxides of K.
[0210] The present invention is not limited to the above-described embodiments and examples, and various modifications can be made within the scope shown in the claims. Embodiments obtained by appropriately combining the technical means separately disclosed in different embodiments and examples are also included in the technical scope of the present invention.
[0211] Industrial Applicability
[0212] The present invention can be used for recovering platinum group metals from raw materials containing platinum group metals (such as waste catalysts, etc.).
Claims
1. A method for recovering platinum group metals, characterized in that: The method comprises the step of fixing the platinum group metal on the ceramic material by contacting a melt of a raw material containing a platinum group metal, a melt of a carbonate or hydroxide of an alkali metal, a melt of an oxide, and a ceramic material. In the fixing step, after heating the raw material containing the platinum group metal, the carbonate or hydroxide of the alkali metal and the oxide to obtain the melt, the melt is brought into contact with the ceramic material. The contact between the melt and the ceramic material is carried out at a temperature of 600 to 1100° C. The above ceramic materials include alumina, The above-mentioned oxide is at least one selected from the group consisting of B2O3, K2O, SiO2, Li2O, Rb2O, Cs2O and P2O5.
2. The method for recovering platinum group metals according to claim 1, characterized in that: The fixing step includes causing the ceramic material to adsorb the platinum group metal, or causing a component eluted from the ceramic material to co-precipitate with the platinum group metal.
3. The method for recovering platinum group metals according to claim 1 or 2, characterized in that: The ceramic material may further contain zeolite, zirconium oxide, silicon dioxide, iron oxide, cobalt oxide or nickel oxide.
4. The method for recovering platinum group metals according to claim 1 or 2, characterized in that: The immobilization step is followed by an elution step of bringing the ceramic material on which the platinum group metal is immobilized into contact with an aqueous solvent to elute the platinum group metal from the ceramic material.
5. The method for recovering platinum group metals according to claim 4, characterized in that: The above aqueous solvent is an aqueous acid solution.
6. The method for recovering platinum group metals according to claim 1 or 2, characterized in that: The contact between the melt and the ceramic material is carried out in the presence of oxygen anions of an amphoteric element.
7. The method for recovering platinum group metals according to claim 1 or 2, characterized in that: The platinum group metal is Pd, Pt, Rh, Ir, Os or Ru.
8. The method for recovering platinum group metals according to claim 1 or 2, characterized in that: The above-mentioned alkali metal is K, Li, Rb or Cs.
9. A ceramic material, characterized in that: The ceramic material is a ceramic material obtained by the method for recovering platinum group metals according to any one of claims 1 to 8, A fixed layer containing O and alkali metals is formed on the surface. The platinum group metal is immobilized in the above-mentioned immobilization layer. The above-mentioned alkali metal is K, Li, Rb or Cs.