Resin laminate, dielectric layer, metal foil with resin, capacitor element, and capacitor built-in printed circuit board
By using the resin laminate composed of the first resin composition and the second resin composition in the capacitor, the challenges of noise reduction and electrostatic capacity improvement in printed circuit boards are solved, and higher electrostatic capacity and good circuit adhesion are achieved. properties and withstand voltage, promoting the miniaturization and thinning of capacitors.
Patent Information
- Application Number
- CN202180011529.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Existing capacitors have challenges in reducing noise and increasing electrostatic capacity in printed circuit boards. In particular, it is difficult to achieve miniaturization and thinning while taking into account circuit tightness, voltage resistance and interlayer insulation reliability.
A resin laminate composed of a first resin composition containing an epoxy resin, a polyimide resin and a composite metal oxide and a second resin composition containing a cyclic ring is used as the dielectric layer. Oxygen resins and diamine compounds, but not polyimide resins, improve dielectric properties and circuit adhesion through this laminated structure.
It achieves higher electrostatic capacity, good circuit adhesion, voltage resistance and interlayer insulation reliability, taking into account the compromise effect of dielectric characteristics and circuit adhesion, and promotes the miniaturization and thinning of capacitors.
Smart Images

Figure CN115023348B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin laminate, a dielectric layer, a metal foil with resin, a capacitor element, and a capacitor-embedded printed circuit board. Background Art
[0002] As the resin composition used in the manufacture of copper-clad laminates and printed circuit boards, there is known a resin composition for a built-in printed circuit board of a capacitor. The resin composition is a substance that acts as a dielectric layer in a capacitor by curing. For example, a resin composition is disclosed in patent document 1 (WO2019 / 150994A1), comprising: a resin component containing an epoxy resin, a diamine compound and a polyimide resin; and a dielectric filler, comprising at least two kinds of composite metal oxides selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta and Bi, and having a solid content of 60 parts by weight and less than 85 parts by weight relative to 100 parts by weight of the resin composition. The document records that the above-mentioned resin composition, when used as a dielectric layer of a capacitor, can ensure excellent dielectric properties and circuit adhesion, and there is no reduction in capacitance at high temperatures, and the dielectric constant can be suppressed from decreasing.
[0003] In addition, capacitors using a resin laminate having multiple resin composition layers as dielectric layers are known. For example, Patent Document 2 (Japanese Patent Application Publication No. 2003-039595) discloses a double-sided copper-clad laminate for forming a capacitor layer having a resin layer as a dielectric and a copper foil layer as a conductor provided on both sides of the resin layer, wherein the resin layer has a three-layer structure of a thermosetting resin layer / a heat-resistant film layer / a thermosetting resin layer, and the heat-resistant film layer has a Young's modulus of 300 kg / mm. 2 Above, tensile strength is 20kg / mm 2 The double-sided copper-clad laminate has a normal characteristic of 5% or more and a tensile elongation of 5%. Furthermore, when a high voltage of 500V or more is applied between the copper foil surfaces, discharge between the roughened portions of the opposing copper foils can be reliably prevented. Furthermore, Patent Document 3 (Japanese Patent Application Publication No. 2006-165400) describes a method for manufacturing a capacitor layer forming material for forming a capacitor layer of a printed circuit board. The capacitor layer of the printed circuit board comprises: conductive layers located on both outer surfaces, and a three-layer dielectric layer having a thermosetting polymer layer / polymerization reaction layer / thermosetting polymer layer structured by the conductive layers.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: WO2019 / 150994A1
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2003-039595
[0008] Patent Document 3: Japanese Patent Application Laid-Open No. 2006-165400 Summary of the Invention
[0009] On the other hand, printed circuit boards are widely used in electronic communication equipment such as portable electronic devices. In particular, with the recent trend of lightweight miniaturization and high functionality of portable electronic communication equipment, the reduction of noise in printed circuit boards has become a topic. Capacitors that can reduce noise have become important, but in order to achieve high performance, it is expected that such capacitors can be assembled to the inner layer of the printed circuit board to a degree of miniaturization and thinning. In this regard, although the dielectric layer composed of the resin composition disclosed in patent document 1 (WO2019 / 150994A1) can bring good performance to a certain extent, further improvement of electrostatic capacitance is expected. On the other hand, it is also expected to ensure the closeness between the resin layer and the circuit (i.e., circuit closeness), voltage resistance and interlayer insulation reliability.
[0010] The present inventors have now discovered that by using a resin laminate having a first layer composed of a predetermined first resin composition and a second layer composed of a predetermined second resin composition as the dielectric layer of a capacitor, dielectric properties such as electrostatic capacitance can be improved while ensuring good circuit adhesion, voltage resistance, and interlayer insulation reliability.
[0011] Therefore, an object of the present invention is to provide a resin laminate that, when used as a dielectric layer of a capacitor, can improve dielectric properties and ensure good circuit adhesion, withstand voltage, and interlayer insulation reliability.
[0012] According to one embodiment of the present invention, there is provided a resin laminate comprising a first layer composed of a first resin composition and a second layer composed of a second resin composition provided on one surface of the first layer.
[0013] The first resin composition comprises:
[0014] a resin component comprising an epoxy resin, a diamine compound, and a polyimide resin; and
[0015] a dielectric filler comprising at least two composite metal oxides selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta, and Bi, wherein the dielectric filler comprises 60 parts by weight or more and 85 parts by weight relative to 100 parts by weight of the solid content of the first resin composition;
[0016] The content of the polyimide resin in the first resin composition is 20 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the resin component.
[0017] The second resin composition comprises:
[0018] a resin component containing an epoxy resin and a diamine compound but not containing a polyimide resin; and
[0019] The dielectric filler is a composite metal oxide containing at least two selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta, and Bi, and the content thereof is 70 parts by weight to 90 parts by weight based on 100 parts by weight of the solid content of the second resin composition.
[0020] According to another aspect of the present invention, there is provided a dielectric layer including the resin laminate, wherein the first resin composition and the second resin composition are cured.
[0021] According to another aspect of the present invention, there is provided a metal foil with resin, including a metal foil and the resin laminate provided on at least one surface of the metal foil.
[0022] According to another aspect of the present invention, there is provided a capacitor element including the above-described dielectric layer.
[0023] According to another aspect of the present invention, there is provided a printed wiring board with built-in capacitors, the printed wiring board including the above-described dielectric layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic cross-sectional view showing an example of the resin laminate according to the present invention.
[0025] Figure 2 This is a schematic cross-sectional view showing another example of the resin laminate according to the present invention.
[0026] Figure 3 To show Figure 1 FIG. 1 is a diagram showing an example of a manufacturing process of a resin laminate and a metal foil with resin.
[0027] Figure 4 To show Figure 1 FIG. 1 is a diagram showing another example of the production process of the resin laminate and the resin-coated metal foil.
[0028] Figure 5 To show Figure 2 FIG. 1 is a diagram showing an example of a manufacturing process of a resin laminate and a metal foil with resin. DETAILED DESCRIPTION
[0029] Resin laminate
[0030] Figure 1The resin laminate 10 of the present invention is schematically shown. The resin laminate 10 includes a first layer 12 and a second layer 14 provided on one side of the first layer 12. The first layer 12 is composed of a first resin composition. The first resin composition contains a resin component and a dielectric filler. The resin component contains an epoxy resin, a diamine compound, and a polyimide resin. The dielectric filler of the first resin composition is a composite metal oxide containing at least two selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta, and Bi, and is contained in the first resin composition in an amount of 60 parts by weight or more and 85 parts by weight or less relative to 100 parts by weight of the solid content of the first resin composition. The content of the polyimide resin in the first resin composition is 20 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the resin component. On the other hand, the second layer 14 is composed of a second resin composition. The second resin composition contains a resin component and a dielectric filler. The resin component contains an epoxy resin and a diamine compound, but does not contain a polyimide resin. The dielectric filler in the second resin composition is a composite metal oxide containing at least two elements selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta, and Bi, and is contained in the second resin composition in an amount of 70 parts by weight to 90 parts by weight, based on 100 parts by weight of the solid content of the second resin composition. Thus, by using the resin laminate 10 comprising a first layer 12 composed of a predetermined first resin composition and a second layer 14 composed of a predetermined second resin composition as the dielectric layer of a capacitor, dielectric properties such as capacitance can be improved, while ensuring good circuit adhesion, voltage resistance, and interlayer insulation reliability.
[0031] As mentioned above, although the dielectric layer consisting of the resin combination disclosed in patent documentation 1 can provide good performance to a certain extent, it is desirable to further improve electrostatic capacitance. About this point, although electrostatic capacitance can be improved by increasing the content of the dielectric filler in the resin combination, the increase of dielectric filler can cause the adhesion (i.e. circuit adhesion) of resin layer and circuit to reduce. Therefore, how to take into account the dielectric properties such as electrostatic capacitance and circuit adhesion becomes a problem. Not only that, when being used as the dielectric layer of a capacitor, it is also desirable that resin combination ensures withstand voltage and interlayer insulation reliability. These problems can be solved just right by the resin laminate 10 of the present invention. Particularly for the resin laminate 10 of the present invention, the circuit adhesion of the first resin combination constituting the first layer 12 is particularly excellent, on the other hand, the dielectric properties of the second resin combination constituting the second layer 14 are particularly excellent, and in this respect, dielectric properties such as electrostatic capacitance that are originally in a compromise relationship and circuit adhesion can be suitably taken into account.
[0032] Therefore, the first layer 12 can be made thinner as long as the desired circuit adhesion is achieved, and at the same time, the second layer 14 having excellent dielectric properties can be made as thick as possible, thereby achieving a higher electrostatic capacitance in the form of a resin laminate. For example, the thickness of the first layer 12 is preferably 0.5% or more and 100% or less of the thickness of the second layer 14, more preferably 15% or more and 100% or less, further preferably 25% or more and 75% or less, and particularly preferably 35% or more and 50% or less. Of course, the first layer 12 can also be made thicker than the second layer 14 as long as the desired characteristics can be obtained. From the perspective of circuit adhesion, the thickness of the first layer 12 is preferably 0.1 μm or more and 5 μm or less, more preferably 0.1 μm or more and 3 μm or less, particularly preferably 0.1 μm or more and 2 μm or less, and most preferably 0.5 μm or more and 2 μm or less. From the viewpoint of ensuring high electrostatic capacitance, the thickness of the second layer 14 is preferably 0.1 μm to 25 μm, more preferably 0.4 μm to 17 μm, particularly preferably 0.9 μm to 8 μm, and most preferably 1 μm to 4 μm.
[0033] The resin laminate 10 may have any layer structure as long as it includes the first layer 12 and the second layer 14. Figure 1 As shown in FIG, it is a two-layer structure consisting of a first layer 12 and a second layer 14. Alternatively, it can also be as shown in FIG. Figure 2 The resin laminate 10' shown in FIG. Specifically, according to another preferred embodiment of the present invention, the resin laminate 10' may further include another first layer 12 composed of the first resin composition on the surface of the second layer 14 facing away from the first layer 12. By adopting such a three-layer structure of first layer 12 / second layer 14 / first layer 12, improved circuit adhesion can be achieved on both surfaces of the resin laminate 10.
[0034] The first resin composition constituting the first layer 12 includes a resin component and a dielectric filler. The resin component includes an epoxy resin, a diamine compound, and a polyimide resin. The first resin composition contributes to dielectric properties, circuit adhesion, voltage resistance, and interlayer insulation reliability, and is particularly excellent in circuit adhesion. The first resin composition or the first layer 12 may further include any other components as long as they do not impair the desired functions.
[0035] For the epoxy resin used in the first resin combination, as long as there are more than 2 epoxy groups in the molecule and it can be used for electrical and electronic materials, it is not particularly limited. The preferred content of the epoxy resin in the first resin combination is more than 15 weight parts and less than 80 weight parts relative to 100 weight parts of resin components, more preferably more than 40 weight parts and less than 65 weight parts, more preferably more than 45 weight parts and less than 60 weight parts. As the example of the epoxy resin in the first resin combination, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, biphenyl novolac type epoxy resin, cresol novolac type epoxy resin, alicyclic epoxy resin, glycidylamine type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, dicyclopentadiene type epoxy resin and their combination in any. From the viewpoint of maintaining heat resistance of the cured product, aromatic epoxy resins or polyfunctional epoxy resins are preferred, and bisphenol A epoxy resins, phenol novolac epoxy resins, naphthalene epoxy resins, cresol novolac epoxy resins, or biphenyl novolac epoxy resins are more preferred.
[0036] For the diamine compound used in the first resin composition, as long as it acts as a curing agent for the epoxy resin, has two amino groups in the molecule, and can be used for electrical and electronic materials, there is no particular limitation. The preferred content of the diamine compound in the first resin composition is as follows: when the number of epoxy groups in the epoxy resin is set to 1, the number of active hydrogen groups of the diamine compound becomes an amount of more than 0.5 and less than 1.5, more preferably an amount in which the number of active hydrogen groups of the diamine compound becomes more than 0.5 and less than 1.0, and further preferably an amount in which the number of active hydrogen groups of the diamine compound becomes more than 0.65 and less than 1.0. Here, the "number of epoxy groups of the epoxy resin" refers to the value obtained by dividing the solid content mass of the epoxy resin present in the resin component by the epoxy equivalent. In addition, the "number of active hydrogen groups of the diamine compound" refers to the value obtained by dividing the solid content mass of the diamine compound present in the resin component by the active hydrogen group equivalent. Examples of the diamine compound include 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis(4-aminophenoxy)biphenyl, and bis[4-(4-aminophenoxy)phenyl]ether. , 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(aminomethyl)cyclohexane and any combination thereof, preferably 4,4'-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane.
[0037] In the first resin composition, the total content of the epoxy resin and the diamine compound is preferably 40 parts by weight or more and 80 parts by weight or less, more preferably 50 parts by weight or more and 80 parts by weight or less, further preferably 50 parts by weight or more and 70 parts by weight or less, and particularly preferably 60 parts by weight or more and 70 parts by weight or less, relative to 100 parts by weight of the resin component. Such a content can improve circuit adhesion and heat resistance.
[0038] The polyimide resin used in the first resin combination not only contributes to the reduction of dielectric loss tangent, also contributes to the raising of circuit adhesion.The content of the polyimide resin in the first resin combination is below 60 weight parts more than 20 weight parts relative to 100 weight parts resin composition, preferably above 20 weight parts and below 50 weight parts, more preferably above 30 weight parts and below 50 weight parts, further preferably above 30 weight parts and below 40 weight parts.By being such content, good heat resistance can be guaranteed, and show excellent dielectric properties and circuit adhesion.Polyimide resin is just not particularly limited as long as dielectric properties, circuit adhesion and the heat resistance that can realize expectation, but from the aspect that can form varnish well compatible with epoxy resin and filming, is preferably the polyimide resin (hereinafter referred to as organic solvent soluble polyimide) that is soluble in organic solvent. The solubility parameter (SP value) of this organic solvent that polyimide resin is soluble is preferably more than 7.0 and below 17.0, as the preferred example of such organic solvent, can enumerate methyl ethyl ketone, toluene, dimethylbenzene, N-Methyl pyrrolidone, dimethylacetamide, dimethylformamide, cyclopentanone, cyclohexanone, cyclohexane, methylcyclohexane, ethylene glycol, ethylene glycol dimethyl ether, glycol acetate and their combination in any.Particularly from the aspect of the thermotolerance after keeping solidification, preferably molecular end has the polyimide resin of at least one functional group that can react with epoxy group.Specifically, polyimide resin preferably has at least one functional group selected from the group consisting of carboxyl, sulfonic acid group, thiol group and phenolic hydroxyl group as the functional group of its end and / or side chain.By having such functional group, can keep the thermotolerance of polyimide resin, and improve organic solvent solubility and with the compatibility of epoxy resin. Among these, it is more preferable to use a polyimide resin having a carboxyl group as a terminal or side chain functional group.
[0039] Preferred organic solvent-soluble polyimides include those obtained by imidizing tetracarboxylic dianhydride with a diamine compound. Examples of tetracarboxylic dianhydrides include 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenyl)phenyl]propane dianhydride, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'- Benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 2,3,5,6-pyridinetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, or compounds having an alkyl group or a halogen atom substituent on the aromatic ring thereof, and any combination thereof. Among these, polyimide resins mainly composed of 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenyl)phenyl]propane dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, or 2,2',3,3'-biphenyltetracarboxylic dianhydride are preferred from the perspective of improving the heat resistance of the resin composition. On the other hand, examples of diamine compounds include those described above.
[0040] The dielectric filler used in the first resin composition is a component that imparts a desired high electrostatic capacitance to the resin laminate serving as the dielectric layer, and is a composite metal oxide comprising at least two selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta, and Bi. Preferred examples of composite metal oxides include particles comprising at least one selected from the group consisting of BaTiO3, SrTiO3, Pb(Zr, Ti)O3, PbLaTiO3, PbLaZrO, and SrBi2Ta2O9, which have high electrostatic capacitance and can be mixed into the first resin composition, with BaTiO3 being more preferred. It should be noted that Pb(Zr, Ti)O3 represents Pb(Zr x Ti 1-x)O3 (wherein 0≤x≤1, typically 0<x<1). The content of the dielectric filler in the first resin composition is 60 parts by weight or more and 85 parts by weight or less, preferably 70 parts by weight or more and 85 parts by weight or less, and more preferably 75 parts by weight or more and 85 parts by weight or less, relative to 100 parts by weight of the solid content of the first resin composition. In addition, the particle size of the dielectric filler is not particularly limited. From the viewpoint of maintaining the adhesion between the resin composition and the metal foil, the average particle size D measured by laser diffraction scattering particle size distribution measurement is preferably 0. 50 The thickness is 0.01 μm or more and 2.0 μm or less, more preferably 0.05 μm or more and 1.0 μm or less, and even more preferably 0.1 μm or more and 0.5 μm or less.
[0041] The second resin composition constituting the second layer 14 comprises a resin component and a dielectric filler. The resin component comprises an epoxy resin and a diamine compound, but does not contain a polyimide resin. The second resin composition contributes to dielectric properties, circuit adhesion, voltage resistance, and interlayer insulation reliability, but is particularly excellent in dielectric properties (electrostatic capacitance). The second resin composition or the second layer 14 may further contain any other component (excluding the polyimide resin) as long as it does not impair the desired function.
[0042] About the epoxy resin used in the second resin combination, as long as there are more than 2 epoxy groups in the molecule and it can be used for electrical and electronic materials, there is no particular limitation. The preferred content of the epoxy resin in the second resin combination is more than 15 parts by weight and less than 85 parts by weight relative to 100 parts by weight of resin components, more preferably more than 25 parts by weight and less than 80 parts by weight, and further preferably more than 35 parts by weight and less than 75 parts by weight. As the example of the epoxy resin in the second resin combination, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, biphenyl novolac type epoxy resin, cresol novolac type epoxy resin, alicyclic epoxy resin, glycidylamine type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, dicyclopentadiene type epoxy resin and their arbitrary combination can be listed. From the viewpoint of maintaining heat resistance of the cured product, aromatic epoxy resins or polyfunctional epoxy resins are preferred, and bisphenol A epoxy resins, phenol novolac epoxy resins, naphthalene epoxy resins, cresol novolac epoxy resins, or biphenyl novolac epoxy resins are more preferred.
[0043] For the diamine compound used in the second resin composition, as long as it acts as a curing agent for the epoxy resin, has two amino groups in the molecule, and can be used for electrical and electronic materials, there is no particular limitation. The preferred content of the diamine compound in the second resin composition is the following amount: when the number of epoxy groups in the epoxy resin is set to 1, the amount in which the active hydrogen groups of the diamine compound are 0.5 or more and 1.5 or less, more preferably the amount in which the active hydrogen groups of the diamine compound are 0.5 or more and 1.0 or less, and further preferably the amount in which the active hydrogen groups of the diamine compound are 0.65 or more and 1.0 or less. Here, the "number of epoxy groups of the epoxy resin" refers to the value obtained by dividing the solid content mass of the epoxy resin present in the resin component by the epoxy equivalent. In addition, the "number of active hydrogen groups of the diamine compound" refers to the value obtained by dividing the solid content mass of the diamine compound present in the resin component by the active hydrogen group equivalent. Examples of the diamine compound include 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(aminomethyl)cyclohexane, and any combination thereof, preferably 4,4'-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane.
[0044] In the second resin composition, the total content of the epoxy resin and the diamine compound is preferably 100 parts by weight relative to 100 parts by weight of the resin component. Unlike the first resin composition, the second resin composition does not contain a polyimide resin, so the resin component is typically composed of two components: the epoxy resin and the diamine compound.
[0045] The dielectric filler used in the second resin composition is a component that imparts a desired high electrostatic capacitance to the resin laminate, and is a composite metal oxide containing at least two selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta and Bi. As a preferred example of the composite metal oxide, there can be cited particles containing at least one selected from the group consisting of BaTiO3, SrTiO3, Pb(Zr, Ti)O3, PbLaTiO3, PbLaZrO and SrBi2Ta2O9 that have high electrostatic capacitance and can be mixed into the second resin composition, more preferably BaTiO3. It should be noted that Pb(Zr, Ti)O3 represents Pb(Zr x Ti 1-x )O3 (wherein 0≤x≤1, typically 0<x<1). The content of the dielectric filler in the second resin composition is 70 parts by weight or more and 90 parts by weight or less, preferably 75 parts by weight or more and 90 parts by weight or less, and more preferably 80 parts by weight or more and 90 parts by weight or less, relative to 100 parts by weight of the solid content of the second resin composition. In addition, the particle size of the dielectric filler is not particularly limited. From the viewpoint of maintaining the adhesion between the resin composition and the metal foil, the average particle size D measured by laser diffraction scattering particle size distribution measurement is preferably 0. 50 The thickness is 0.01 μm or more and 2.0 μm or less, more preferably 0.05 μm or more and 1.0 μm or less, and even more preferably 0.1 μm or more and 0.5 μm or less.
[0046] The first resin composition and / or the second resin composition may further include a filler dispersant. By further including a filler dispersant, the dispersibility of the dielectric filler can be improved when the resin varnish and the dielectric filler are mixed. The filler dispersant can appropriately use a known filler dispersant that can be used, without particular limitation. As examples of preferred filler dispersants, in addition to phosphonic acid type, cationic type, carboxylic acid type, and anionic dispersants belonging to ionic dispersants, ether type, ester type, sorbitan ester type, diester type, glycerol monoester type, ethylene oxide addition type, ethylenediamine base type, phenol type dispersants, etc. belonging to nonionic dispersants can also be listed. In addition, coupling agents such as silane coupling agents, titanate coupling agents, and aluminate coupling agents can be listed.
[0047] In order to promote the solidification of the resin composition, a curing accelerator may also be added to the first resin combination and / or the second resin combination. As preferred examples of curing accelerators, imidazole-based and amine-based curing accelerators may be listed. From the perspective of the storage stability and efficiency of the resin combination, the content of the curing accelerator is preferably 0.01 parts by weight and below 3 parts by weight relative to the non-volatile component in 100 parts by weight of the resin combination, more preferably 0.1 parts by weight and below 2 parts by weight.
[0048] After the curing reaction with the epoxy resin, the imidazole curing accelerator does not dissociate as an ion but instead becomes part of the epoxy resin's molecular structure. This allows the resin layer to exhibit excellent dielectric properties and insulation reliability. The amount of imidazole curing accelerator can be appropriately determined to achieve the desired cure, taking into account various factors such as the resin layer's composition, and is not particularly limited. Examples of the imidazole curing accelerator include 2-undecyl imidazole, 2-heptadecylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-undecyl imidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 1,2-dimethylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecyl imidazoleium trimellitate, 1 -cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and any combination thereof. Preferred examples of imidazole-based curing accelerators include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. From the perspective of chemical stability of the resin layer in a semi-cured (B-stage) state, more preferred examples include 2-phenyl-4-methylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole, which are imidazole-based curing accelerators having a phenyl group. Among these, 2-phenyl-4-methyl-5-hydroxymethylimidazole is particularly preferred.
[0049] Examples of amine-based curing accelerators include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, and any combination thereof.
[0050] Metal foil with resin
[0051] The resin laminate of the present invention is preferably used as the resin of the metal foil with resin. By pre-forming the form of the metal foil with resin, it is possible to efficiently carry out the manufacture of capacitor elements and capacitor built-in printed circuit boards without separately forming a resin laminate or a dielectric layer. That is, according to a preferred embodiment of the present invention, a metal foil with resin is provided comprising a metal foil and a resin laminate arranged on at least one side of the metal foil. In addition, in the metal foil with resin, the metal foil can be arranged on both sides of the resin laminate, and this formation is equivalent to a metal-clad laminate. Typically, the resin laminate is in the form of a resin layer, and the first resin composition and / or the second resin composition constituting the resin laminate are coated on the metal foil and dried using a gravure coating method in such a way that the thickness of the resin layer after drying becomes a specified value, thereby obtaining the metal foil with resin. The coating method is arbitrary, and in addition to the gravure coating method, a die coating method, a blade coating method, etc. can also be adopted. In addition, a scraper, a rod coater, etc. can also be used for coating.
[0052] The lamination of the first layer 12 and the second layer 14 can be performed by any method without particular limitation. Figure 3 As shown, a first resin composition can be applied to a metal foil 16 to form a first layer 12, thereby producing a first resin-coated metal foil 20; on the other hand, a second resin composition can be applied to another metal foil 16' to form a second layer 14, thereby producing a second resin-coated metal foil 22, and the first layer 12 and the second layer 14 can be laminated so that they face each other. Figure 4 As shown in FIG. 1 , a first resin composition may be applied to a metal foil 16 to form a first layer 12, and then a second resin composition may be applied to the first layer 12 to form a second layer 14, thereby producing a metal foil 24 with two layers of resin. In this case, another metal foil 16' may be laminated on the second layer 14 to produce a metal-clad laminate 30. Alternatively, when a three-layer resin laminate is produced, as shown in FIG. Figure 5 As shown, it is preferred that a metal foil 20 with a first resin having a first layer 12 formed on a metal foil 16 and a metal foil 24' with two resin layers having a first layer 12 and a second layer 14 formed on another metal foil 16' be laminated so that the first layer 12 and the second layer 14 face each other. From the perspective of forming a resin laminate or a dielectric layer by laminating them in such a manner as described above, the first resin composition and the second resin composition are preferably semi-cured during lamination.
[0053] The metal foil is preferably a copper foil. The metal foil such as copper foil can be a metal foil in the state of electrolytic foil or rolled foil (so-called raw foil), or it can be a form of surface-treated foil in which at least any one side has been subjected to surface treatment. The surface treatment can be various surface treatments carried out in order to improve or impart a certain property (such as rust resistance, moisture resistance, chemical resistance, acid resistance, heat resistance, and adhesion to the substrate) to the surface of the metal foil. The surface treatment can be carried out on at least one side of the metal foil or on both sides of the metal foil. Examples of the surface treatment carried out on the metal foil include rust prevention treatment, silane treatment, roughening treatment, shielding formation treatment, etc.
[0054] The ten-point height of microscopic roughness Rzjis on the surface of the metal foil on the resin laminate side, as measured in accordance with JIS B0601-2001, is preferably 2.0 μm or less, more preferably 1.5 μm or less, even more preferably 1.0 μm or less, and particularly preferably 0.5 μm or less. Within this range, the thickness of the resin laminate can be made thinner. The lower limit of the ten-point height of microscopic roughness Rzjis on the surface of the metal foil on the resin laminate side is not particularly limited. From the perspective of improving adhesion to the resin laminate, Rzjis is preferably 0.005 μm or more, more preferably 0.01 μm or more, and even more preferably 0.05 μm or more.
[0055] The thickness of the metal foil is not particularly limited, but is preferably 0.1 μm or more and 100 μm or less, more preferably 0.5 μm or more and 70 μm or less, further preferably 2 μm or more and 70 μm or less, particularly preferably 10 μm or more and 70 μm or less, and most preferably 10 μm or more and 35 μm or less. When the thickness is within the above range, methods such as the MSAP (semi-additive) method, the SAP (semi-additive) method, and the subtractive method, which are common patterning methods for forming wiring for printed circuit boards, can be used. Of course, when the thickness of the metal foil is, for example, 10 μm or less, in order to improve handling, the resin-coated metal foil of the present invention may also be a metal foil with a carrier having a release layer and a carrier, in which a resin laminate is formed on the surface of the metal foil.
[0056] dielectric layer
[0057] The resin laminate of the present invention is preferably cured to form a dielectric layer. That is, according to a preferred embodiment of the present invention, a dielectric layer is provided, which comprises the resin laminate of the present invention, and the first resin composition and the second resin composition are cured. The curing of the resin composition can be carried out based on a well-known method, preferably by hot vacuum pressing. The thickness of the dielectric layer is not particularly limited as long as the desired electrostatic capacitance can be ensured, and is preferably 0.2 μm or more and 30 μm or less, more preferably 0.5 μm or more and 20 μm or less, particularly preferably 1 μm or more and 10 μm or less, and most preferably 2 μm or more and 6 μm or less. When the thickness is within the above range, it has the advantages of being easy to achieve high electrostatic capacitance, easy to form a resin laminate by coating the resin composition, easy to ensure sufficient adhesion with the metal foil, and easy to obtain stable interlayer insulation.
[0058] Capacitor element and capacitor-built-in printed circuit board
[0059] The resin laminate of the present invention or the dielectric layer containing the same is preferably assembled in a capacitor element. That is, according to a preferred embodiment of the present invention, a capacitor element having the above-mentioned dielectric layer is provided. The composition of the capacitor element is not particularly limited, and a known composition can be adopted. A particularly preferred embodiment is a capacitor-built-in printed circuit board in which a capacitor or its dielectric layer is assembled as an inner layer portion of a printed circuit board. That is, according to a particularly preferred embodiment of the present invention, a capacitor-built-in printed circuit board having the above-mentioned dielectric layer is provided. In particular, by using the resin-coated metal foil of the present invention, capacitor elements and capacitor-built-in printed circuit boards can be efficiently manufactured based on known methods.
[0060] Example
[0061] The present invention is further described in detail through the following examples.
[0062] Example 1
[0063] (1) Preparation of resin varnish
[0064] First, as raw material components for a resin varnish, the following resin components and an imidazole-based curing accelerator were prepared.
[0065] -Epoxy resin: DIC Corporation, 850-S (bisphenol A type, epoxy equivalent 188 g / eq)
[0066] -Diamine compound: BAPP (2,2-bis[4-(4-aminophenoxy)phenyl]propane, active hydrogen group equivalent 102 g / Eq) manufactured by Wakayama Seika Kogyo Co., Ltd.
[0067] -Polyimide resin: PIAD-300 manufactured by Arakawa Chemical Industries, Ltd. (terminal functional group: carboxyl group, solvent: a mixed solution of cyclohexanone, methylcyclohexane, and ethylene glycol dimethyl ether)
[0068] - Imidazole curing accelerator: 2P4MHZ (2-phenyl-4-methyl-5-hydroxymethylimidazole, 100 wt % relative to the resin component) manufactured by Shikoku Chemical Industry Co., Ltd., added in an amount of 1.0 wt %
[0069] Two resin varnishes, one for the first resin composition and one for the second resin composition, were prepared as follows. The raw material components for the resin varnish were weighed at the blending ratio (weight ratio) shown in Table 1. Cyclopentanone solvent was then weighed, and the raw material components and cyclopentanone solvent were placed in a flask and stirred at 60°C. After confirming that there was no undissolved raw material in the resin varnish and that the resin varnish was transparent, the resin varnish was recovered.
[0070] (2) Mixing with fillers
[0071] Next, the dielectric filler and dispersant shown below were prepared.
[0072] - Dielectric filler: BaTiO3, manufactured by Nippon Chemical Industry Co., Ltd., AKBT-S (average particle size D measured by laser diffraction scattering particle size distribution measurement) 50 =0.3μm)
[0073] -Dispersant: Titanate coupling agent, Ajinomoto Fine-Techno Co., Inc., KR-44 (1.5 parts by weight per 100 parts by weight of dielectric filler)
[0074] To prepare the first resin composition and the second resin composition, respectively, cyclopentanone solvent, dielectric filler, and dispersant are weighed. The weighed solvent, dielectric filler, and dispersant are slurried using a disperser. After confirming the slurry, the resin varnish for the first resin composition or the second resin composition is weighed so that the final dielectric filler has the mixing ratio (weight ratio) shown in Table 1, and the resin varnish is mixed with the slurry containing the dielectric filler using a disperser. Confirm that the dielectric filler does not agglomerate after mixing. In this way, a coating liquid containing the first resin composition and a coating liquid containing the second resin composition are obtained.
[0075] (3) Resin coating
[0076] like Figure 3As shown, the first resin composition was applied to copper foil 16 (manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 18 μm, surface roughness Rzjis = 0.5 μm) using a bar coater so that the thickness of the dried first layer 12 was 2.0 μm. The copper foil 16 was then dried in an oven heated to 130° C. for 3 minutes to semi-cure the resin. This yielded copper foil 20 coated with the first resin.
[0077] Likewise, Figure 3 As shown, the second resin composition was applied to a copper foil 16' (manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 18 μm, surface roughness Rzjis = 0.5 μm) using a bar coater so that the thickness of the dried second layer 14 was 2.0 μm. The foil was then dried in an oven heated to 130°C for 3 minutes to semi-cure the resin. This yielded a copper foil 22 coated with the second resin.
[0078] (4) Suppression
[0079] like Figure 3 As shown, the copper foil 20 with the first resin and the copper foil 22 with the second resin are stacked in such a manner that their resin-coated surfaces face each other, and the layers are stacked under a pressure of 40 kgf / cm 2 The first and second resin compositions were cured by vacuum pressing at 200°C for 90 minutes. This yielded a metal-clad laminate 30 using copper foil, comprising a resin laminate 10 formed from the cured first and second resin compositions as a dielectric layer, the dielectric layer having a thickness of 4.0 μm.
[0080] (5) Circuit formation and evaluation
[0081] One surface of the obtained metal-clad laminate 30 was etched to form circuits 32 for evaluation, and the following various evaluations were performed.
[0082] <Evaluation 1: Peel Strength (Circuit Adhesion)>
[0083] A single surface of a metal-clad laminate 30 was etched to create a linear circuit 32 with a width of 3 mm. The circuit 32 was then peeled off using an autograph at a peeling rate of 50 mm / minute, and its peel strength was measured. This measurement was conducted in accordance with IPC-TM-650 2.4.8. The measured peel strength was evaluated according to the following criteria. The results are shown in Table 1.
[0084] -Evaluation AA: 0.7kgf / cm or more (best)
[0085] -Evaluation A: 0.6 kgf / cm or more and less than 0.7 kgf / cm (good)
[0086] -Evaluation B: 0.4 kgf / cm3 or more and less than 0.6 kgf / cm3 (pass)
[0087] -Evaluation C: less than 0.4kgf / cm (failed)
[0088] <Evaluation 2: Capacitance (Cp)>
[0089] After etching one side of the metal-clad laminate 30 to produce a circular circuit with a diameter of 0.5 inches (12.6 mm), the electrostatic capacitance at a frequency of 1 kHz was measured using an LCR meter (LCR High tester 3532-50 manufactured by Hioki Electric Co., Ltd.). This measurement was performed in accordance with IPC-TM-650 2.5.2. The results are shown in Table 1. It should be noted that in the application of the present invention, the electrostatic capacitance is 30 nF / in 2 The above is necessary for achieving higher filtering performance and is therefore particularly important.
[0090] - Rating AA: 50nF / in 2 Above (Best)
[0091] - Rating A: 40nF / in 2 Above and less than 50nF / in 2 (excellent)
[0092] - Rating B: 30nF / in 2 Above and less than 40nF / in 2 (qualified)
[0093] - Rating C: less than 30nF / in 2 (Unqualified)
[0094] <Evaluation 3: Dielectric Breakdown Voltage (BDV)>
[0095] A circular circuit with a diameter of 0.5 inches (12.6 mm) was fabricated by etching one side of the metal-clad laminate 30. The dielectric breakdown voltage was measured at a voltage increase rate of 80 V / s using an insulation resistance tester (Super Insulator SM7110, manufactured by Hioki Electric Co., Ltd.). This measurement was conducted in accordance with IPC-TM-650 2.5.6.2. The results are shown in Table 1.
[0096] - Rating AA: 100V or above (best)
[0097] - Rating A: 50V or higher and less than 100V (excellent)
[0098] -Evaluation B: 30V or higher and less than 50V (pass)
[0099] -Evaluation C: less than 30V (failed)
[0100] <Evaluation 4: Leakage Current>
[0101] A circular circuit with a diameter of 0.5 inches (12.6 mm) was fabricated by etching one side of the metal-clad laminate 30. The leakage current was then measured under 50 V application using an insulation resistance tester (Super Insulation Tester SM7110, manufactured by Hioki Electric Co., Ltd.). This measurement was conducted in accordance with IPC-TM-650 2.5.7.2. The results are shown in Table 1.
[0102] -Evaluation AA: less than 10μA (optimal)
[0103] -Evaluation A: 10μA or more and less than 30μA (excellent)
[0104] -Evaluation B: 30μA or more and less than 50μA (pass)
[0105] -Evaluation C: 50μA or more (failed)
[0106] <Evaluation 5: Interlayer Insulation (B-HAST)>
[0107] After etching both sides of the metal-clad laminate 30 to create a circular circuit with a diameter of 0.5 inches (12.6 mm), the wiring was soldered to the upper and lower electrodes, and the wiring was connected to a tester for migration measurement. The evaluation circuit was placed in a constant temperature and humidity chamber at 130°C and 85% RH, and a 3V applied voltage was applied between the upper and lower electrodes. At this time, the measurement was maintained at 1×10 5 The insulation resistance was maintained for a period of time exceeding Ω, and changes in the insulation resistance were observed. The measured interlayer insulation retention time and changes in insulation resistance were evaluated according to the following criteria. This measurement was performed in accordance with JESD22-A110. The results are shown in Table 1.
[0108] - Rating AA: Maintains insulation resistance for more than 96 hours without degradation (best)
[0109] -Evaluation A: Deterioration of insulation resistance was observed after maintaining the insulation for more than 96 hours (Excellent)
[0110] -Evaluation B: Maintain for more than 48 hours and less than 96 hours (pass)
[0111] -Evaluation C: Maintained for less than 48 hours (failed)
[0112] <Comprehensive Evaluation>
[0113] The comprehensive evaluation was determined by applying the evaluation results of evaluations 1 to 5 to the following criteria. The results are shown in Table 1.
[0114] - AA rating: All ratings are AA or A (best)
[0115] - Evaluation A: No C rating and only one B rating (Excellent)
[0116] -Evaluation B: No C judgment, but 2 or more B judgments (pass)
[0117] - Evaluation C: At least one of the C judgments is unqualified
[0118] Example 2 (Compare)
[0119] A metal-clad laminate was produced and evaluated in the same manner as in Example 1 except that the second resin-coated copper foil 22 was not used and two first resin-coated copper foils 20 were laminated with their resin-coated surfaces facing each other.
[0120] Example 3 (Compare)
[0121] A metal-clad laminate was produced and evaluated in the same manner as in Example 1, except that the first resin-coated copper foil 20 was not used and two second resin-coated copper foils 22 were laminated with their resin-coated surfaces facing each other.
[0122] Examples 4 to 10
[0123] In the above (1), the raw material components for the resin varnish were weighed in the mixing ratio (weight ratio) shown in Table 2, the resin coating of the above (3) was carried out in the following manner, and the pressing of the above (4) was carried out in the following manner. Except for this, the metal-clad laminate was prepared and evaluated in the same manner as in Example 1.
[0124] (3') Resin coating
[0125] like Figure 5 As shown, the first resin composition was applied to copper foil 16 (manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 18 μm, surface roughness Rzjis = 0.5 μm) using a bar coater so that the thickness of the dried first layer 12 would be 1.0 μm. The composition was then dried in an oven heated to 130°C for 3 minutes to semi-cure the resin. This produced two copper foils 20 and 20' coated with the first resin.
[0126] In addition, if Figure 5 As shown, the second resin composition was applied to the surface of the first layer 12 of the first resin-coated copper foil 20' using a bar coater so that the thickness of the dried second layer 14 would be 2.0 μm. The copper foil was then dried in an oven heated to 130°C for 3 minutes to semi-cure the resin. This resulted in a two-layered copper foil 24' having, in this order, a first layer 12 composed of the first resin composition and a second layer 14 composed of the second resin composition on a copper foil 16'.
[0127] (4') Suppression
[0128] like Figure 5 As shown, the copper foil 20 with the first resin and the copper foil 24' with the two layers of resin are stacked with their resin-coated surfaces facing each other, and the pressure is 40 kgf / cm 2 The resin composition was cured by vacuum pressing at 200°C for 90 minutes. This resulted in a metal-clad laminate 30' comprising a resin laminate 10' formed from the cured first and second resin compositions as a dielectric layer, with the dielectric layer having a thickness of 4.0 μm. The dielectric layer of the resin laminate 10' thus obtained had a three-layer structure comprising, in this order, a first layer 12 composed of the first resin composition, a second layer 14 composed of the second resin composition, and a first layer 12 composed of the first resin composition.
[0129] Example 11 (Compare)
[0130] In the above (3'), a metal-clad laminate was prepared and evaluated in the same manner as in Example 4 except that a polyimide film (Kapton (registered trademark), 4 μm thick, manufactured by Toray DuPont Co., Ltd.) was laminated as a second layer 14 on the surface of the first layer 12 of the copper foil 20' with the first resin instead of coating the second resin composition, thereby producing a copper foil 24' with two layers of resin.
[0131] [Table 1]
[0132]
[0133] [Table 2]
[0134]
Claims
1. A resin laminate comprising a first layer composed of a first resin composition and a second layer composed of a second resin composition provided on one surface of the first layer, The first resin composition comprises: a resin component comprising an epoxy resin, a diamine compound and a polyimide resin; and a dielectric filler comprising at least two composite metal oxides selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta and Bi, and containing 60 parts by weight or more and 85 parts by weight or less relative to 100 parts by weight of the solid content of the first resin composition, The content of the polyimide resin in the first resin composition is 20 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the resin component. The second resin composition comprises: a resin component containing an epoxy resin and a diamine compound but not containing a polyimide resin; and The dielectric filler is a composite metal oxide containing at least two selected from the group consisting of Ba, Ti, Sr, Pb, Zr, La, Ta and Bi, and the content of the dielectric filler is 70 parts by weight or more and 90 parts by weight or less based on 100 parts by weight of the solid content of the second resin composition.
2. The resin laminate according to claim 1, in, The second layer further includes another first layer made of the first resin composition on a surface of the second layer that is away from the first layer.
3. The resin laminate according to claim 1 or 2, in, The total content of the epoxy resin and the diamine compound in the first resin composition is 40 parts by weight or more and 80 parts by weight or less relative to 100 parts by weight of the resin component.
4. The resin laminate according to claim 1 or 2, in, In the first resin composition, when the number of epoxy groups of the epoxy resin is 1, the content of the diamine compound is an amount such that the number of active hydrogen groups of the diamine compound becomes 0.5 or more and 1.5 or less.
5. The resin laminate according to claim 1 or 2, in, In the first resin composition, when the number of epoxy groups of the epoxy resin is 1, the content of the diamine compound is an amount such that the number of active hydrogen groups of the diamine compound becomes 0.65 or more and 1.0 or less.
6. The resin laminate according to claim 1 or 2, in, The composite metal oxide contained in the first resin composition comprises a compound selected from the group consisting of BaTiO 3 、SrTiO 3 、Pb(Zr、Ti)O 3 、PbLaTiO 3 , PbLaZrO and SrBi 2 Ta 2 O 9 At least one of the group consisting of.
7. The resin laminate according to claim 1 or 2, in, The composite metal oxide contained in the first resin composition is BaTiO 3 .
8. The resin laminate according to claim 1 or 2, in, In the second resin composition, when the number of epoxy groups of the epoxy resin is 1, the content of the diamine compound is an amount such that the number of active hydrogen groups of the diamine compound becomes 0.5 or more and 1.5 or less.
9. The resin laminate according to claim 1 or 2, in, In the second resin composition, when the number of epoxy groups of the epoxy resin is 1, the content of the diamine compound is an amount such that the number of active hydrogen groups of the diamine compound becomes 0.65 or more and 1.0 or less.
10. The resin laminate according to claim 1 or 2, in, The composite metal oxide contained in the second resin composition comprises a metal selected from the group consisting of BaTiO 3 、SrTiO 3 、Pb(Zr、Ti)O 3 、PbLaTiO 3 , PbLaZrO and SrBi 2 Ta 2 O 9 At least one of the group consisting of.
11. The resin laminate according to claim 1 or 2, in, The composite metal oxide contained in the second resin composition is BaTiO 3 . 12 . A dielectric layer comprising the resin laminate according to claim 1 , wherein the first resin composition and the second resin composition are cured.
13. The dielectric layer according to claim 12, in, The dielectric layer has a thickness of 0.2 μm or more and 30 μm or less. 14 . A metal foil with resin, comprising a metal foil and the resin laminate according to claim 1 provided on at least one surface of the metal foil.
15. The metal foil with resin according to claim 14, in, The metal foil is provided on both surfaces of the resin laminate.
16. The metal foil with resin according to claim 14 or 15, in, The metal foil is copper foil. 17 . A capacitor element comprising the dielectric layer according to claim 12 or 13 .
18. A capacitor-built-in printed circuit board comprising the dielectric layer according to claim 12 or 13.
Citation Information
Patent Citations
Double-sided copper-clad laminate for forming capacitor layer and manufacturing method thereof
JP2003039595A
Manufacturing method of capacitor layer forming material, and the material obtained by the method
JP2006165400A
Double side conductor laminates and its manufacture
WO2007097585A1
Resin composition, copper foil with resin, dielectric layer, copper-clad laminate, capacitor element, and printed wiring board with built-in capacitor