A long-life positive electrode material, preparation method thereof and lithium ion battery
By using wet co-precipitation coating of Al2O3 and LiF on the surface of high-nickel ternary positive electrode material, the deformation and cycle failure of the positive electrode material after the nickel content is increased, the battery life and energy efficiency are improved, and the high-nickel positive electrode is realized Long life and high energy efficiency of materials.
Patent Information
- Application Number
- CN202210723077.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-24
AI Technical Summary
After the nickel content of the existing positive electrode material increases, the material deforms during the charging and discharge process, resulting in cracks and cycle failures, increase in ion impedance, decrease in average voltage, and worsens in energy efficiency ratio, and the coating solution cannot be fully covered, resulting in safety and Poor rate performance.
High nickel ternary cathode material and Al2O3 and LiF are used as the cladding layer, and a dense cladding layer is formed on the surface of the material through wet co-precipitation technology to improve the safety and stability of the material.
It improves the battery life, safety and rate performance, reduces high-temperature storage gas production, enhances energy density and energy conversion efficiency, and achieves the long life and high energy efficiency of high-nickel cathode materials.
Smart Images

Figure BDA0003712356940000111 
Figure BDA0003712356940000112 
Figure HDA0003712356950000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion electrodes, and in particular relates to a long-life positive electrode material, a preparation method thereof and a lithium ion battery. Background Art
[0002] As people's requirements for electric vehicle range are getting higher and higher, the high specific energy of positive electrode materials is becoming more and more important. At present, the gram capacity is mainly increased by increasing the nickel content. For example, when the nickel content is increased to 80% molar ratio, the gram capacity can reach 200mAh / g, and when the nickel content is increased to 90% molar ratio, the gram capacity can reach 218mAh / g. However, with the increase of nickel content, the positive electrode material has a larger deformation during the charge and discharge process, which causes cracks in the material in a short time and cycle failure.
[0003] The increase in nickel content leads to an increase in the ionic impedance of the material, a lower average voltage of the material, and a worse energy efficiency ratio. In particular, as the nickel content increases, the safety of the material's specific energy improvement decreases. The existing solution is to coat the surface of the material with a layer of nanoparticles to prevent the material from excessively detaching during the cycle and destroying the material structure. However, even nanoparticles are only a few hundred nanometers in size and cannot be completely covered during coating. Instead, they are dotted and part of the material is exposed outside the coating. Rapid attenuation will still occur during the cycle. If the coating is complete, the coating layer will be too thick, increasing its surface impedance and deteriorating the rate performance. Summary of the invention
[0004] The purpose of the present invention is to provide a long-life positive electrode material, a preparation method thereof and a lithium ion battery. The positive electrode material in the present invention can improve the high safety, life and rate performance of the battery, and there is a high-nickel secondary ball material with high energy efficiency ratio and high discharge platform in the battery, which can solve the problems of low life, low gas production, low energy efficiency ratio and low discharge platform that exist at this stage.
[0005] The present invention provides a long-life positive electrode material, comprising a high-nickel ternary positive electrode material and a coating layer coated on the surface of the high-nickel ternary positive electrode material;
[0006] The coating layer includes Al2O3 and LiF.
[0007] Preferably, the molecular formula of the high-nickel ternary positive electrode material is as shown in Formula I:
[0008] LiNi a Co b Mn c O2 Formula I;
[0009] Among them, 0.5≤a<1, 0<b<0.5, 0<c<0.2, a+b+c=1.
[0010] Preferably, the mass ratio of Al2O3 to LiF in the coating layer is (0.1-2):1.
[0011] Preferably, the specific surface area of the positive electrode material is 0.2 to 1.0 m 2 / g, Li2CO3 content ≤ 3000ppm, LiOH content ≤ 5000ppm, Free Li + Content ≤2000ppm.
[0012] The present invention provides a method for preparing the long-life positive electrode material as described above, comprising the following steps:
[0013] A) mixing the precursor and the lithium source uniformly, and sieving to obtain a mixed raw material;
[0014] B) in an oxygen-containing atmosphere, heating the mixed raw material to 300-500° C., keeping the temperature for 2-10 hours, and performing a first-stage sintering; then heating the mixed raw material to 500-600° C., keeping the temperature for 1-2 hours, and performing a second-stage sintering; finally heating the mixed raw material to 700-800° C., keeping the temperature for 1-20 hours, and performing a third-stage sintering, and cooling the mixed raw material to room temperature with the furnace after the third-stage sintering is completed;
[0015] C) mixing the material obtained by the three-stage sintering with the LiAlO2 aqueous solution, then adding the HF aqueous solution and stirring until the reaction is complete;
[0016] D) subjecting the system obtained by the complete reaction in step C) to solid-liquid separation and drying to obtain an intermediate;
[0017] E) sintering the intermediate at 200-350° C. for 1-15 hours to obtain a positive electrode material with a long lifespan.
[0018] Preferably, the precursor is Ni a Co b Mn c (OH)2; 0.5≤a<1, 0<b<0.5, 0<c<0.2, and a+b+c=1;
[0019] The lithium source is one or more of LiOH, Li2CO3, LiNO3 and CH3COOLi;
[0020] The molar ratio of the precursor to the lithium source is 1:(0.8-1.2).
[0021] Preferably, in the oxygen-containing atmosphere in step B), the concentration of oxygen is 85-100%.
[0022] Preferably, the mass ratio of the material obtained by the three-stage sintering to the LiAlO2 aqueous solution is 1:(0.5-10);
[0023] The mass ratio of the material obtained by the three-stage sintering to the HF aqueous solution is 1:(0.5-10).
[0024] Preferably, the drying temperature in step D) is 20-500°C.
[0025] The present invention provides a lithium ion battery, characterized by comprising the above-mentioned long-life positive electrode material.
[0026] The present invention provides a long-life positive electrode material, comprising a high-nickel ternary positive electrode material and a coating layer coated on the surface of the high-nickel ternary positive electrode material; the coating layer comprises Al2O3 and LiF. The present invention coats a dense layer of Al2O3 and LiF on the surface of the high-nickel ternary positive electrode material by wet coprecipitation, thereby improving the safety and stability of the ternary material, while improving the rate performance and average discharge voltage of the battery, and reducing the high-temperature storage gas generation of the material, so that the battery composed of this material has stronger practicality, higher energy density, and higher energy conversion efficiency. The 2430 button cell made of the material of the present invention has an initial coulombic efficiency of more than 90% ((initial discharge capacity / initial charge capacity)*100%), a gram capacity of more than 200mAh / g; it is assembled into an 800mAh soft-pack battery with an average voltage (discharge energy / discharge capacity) of more than 3.65V at 0.2C charge and discharge, a 300-cycle capacity retention rate of more than 94% at 45°C ((300-cycle discharge capacity / first-cycle discharge capacity)*100%), and an energy efficiency ratio of more than 85% ((discharge energy÷charge energy)*100%). BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 The graph is a cycle curve of the lithium-ion battery in the embodiment of the present invention and the comparative example at 45°C. DETAILED DESCRIPTION
[0029] The present invention provides a long-life positive electrode material, comprising a high-nickel ternary positive electrode material and a coating layer coated on the surface of the high-nickel ternary positive electrode material;
[0030] The coating layer includes Al2O3 and LiF.
[0031] In the present invention, the high nickel ternary positive electrode material has a chemical formula shown in Formula I:
[0032] LiNi a Co b Mn c O2 Formula I;
[0033] Among them, 0.5≤a<1, preferably, 0.6≤a≤0.9, such as a is 0.83; 0<b<0.5, preferably, 0.1≤b≤0.2, such as b is 0.12; 0<c<0.2, preferably, 0.05≤c≤0.1, such as c is 0.05; a+b+c=1.
[0034] In the present invention, the mass ratio of the high nickel ternary positive electrode material to the coating layer is preferably (100-1000):1, preferably (300-800):1, such as 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, 1000:1, preferably a range value with any of the above values as the upper or lower limit. The thickness of the coating layer is preferably 10-500 nm.
[0035] The coating layer includes Al2O3 and LiF, and is a coating layer formed on the surface of the high-nickel ternary positive electrode material by the reaction and co-precipitation of LiAlO2 and HF in an aqueous solution. Due to the wet co-precipitation coating of Al2O3 and LiF, most of the LiF surface is wrapped by Al2O3, LiF can exist stably on the positive electrode surface, and the surface of the positive electrode is more stable. The mass ratio of Al2O3 to LiF is (0.1-2):1, more preferably (0.5-1.5):1, such as 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, preferably a range value with any of the above values as the upper or lower limit.
[0036] In the present invention, the specific surface area of the long-life positive electrode material is 0.2 to 1.0 m 2 / g, Li2CO3 content ≤ 3000ppm, LiOH content ≤ 5000ppm, Free Li + Content ≤2000ppm, tap density ≥2.2g / cm 3 .
[0037] The present invention also provides a method for preparing a long-life positive electrode material, comprising the following steps:
[0038] A) mixing the precursor and the lithium source uniformly, and sieving to obtain a mixed raw material;
[0039] B) in an oxygen-containing atmosphere, heating the mixed raw material to 300-500° C., keeping the temperature for 2-10 hours, and performing a first-stage sintering; then heating the mixed raw material to 500-600° C., keeping the temperature for 1-2 hours, and performing a second-stage sintering; finally heating the mixed raw material to 700-800° C., keeping the temperature for 1-20 hours, and performing a third-stage sintering, and cooling the mixed raw material to room temperature with the furnace after the third-stage sintering is completed;
[0040] C) mixing the material obtained by the three-stage sintering with the LiAlO2 aqueous solution, then adding the HF aqueous solution and stirring until the reaction is complete;
[0041] D) subjecting the system obtained by the complete reaction in step C) to solid-liquid separation and drying to obtain an intermediate;
[0042] E) sintering the intermediate at 200-350° C. for 1-15 hours to obtain a positive electrode material with a long lifespan.
[0043] The present invention firstly prepares a polycrystalline precursor Ni a Co b Mn c (OH)2 and the lithium source are mixed evenly and sieved to obtain a mixed raw material.
[0044] In the present invention, the polycrystalline precursor Ni a Co b Mn c In (OH)2, 0.5≤a<1, preferably, 0.6≤a≤0.9, such as a is 0.83; 0<b<0.5, preferably, 0.1≤b≤0.2, such as b is 0.12; 0<c<0.2, preferably, 0.05≤c≤0.1, such as c is 0.05; and a+b+c=1.
[0045] In the present invention, the lithium source is preferably one or more of Li(OH), Li2CO3, LiNO3 and CH3COOLi; the molar ratio of the polycrystalline precursor to the lithium source is preferably 1:(0.8-1.2), more preferably 1:(0.95-1.05), such as 1:1.05, 1:1.04, 1:1.03, 1:1.02, 1:1.01, 1:1, preferably a range value with any of the above values as the upper or lower limit.
[0046] In the present invention, the mesh size of the sieving is preferably 200 to 400 meshes.
[0047] After obtaining the mixed raw material, the present invention puts the mixed raw material into a sagger and sintering is carried out in a muffle furnace filled with an oxygen-containing atmosphere.
[0048] In the present invention, the sintering is a three-stage sintering process, the temperature of the first stage sintering is preferably 300-500°C, more preferably 350-450°C, such as 300°C, 350°C, 400°C, 450°C, 500°C, preferably a range value with any of the above values as the upper or lower limit; the holding time of the first stage sintering is preferably 2-10 hours, more preferably 5-8 hours, such as 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, preferably a range value with any of the above values as the upper or lower limit. The heating rate of the first stage sintering is preferably 1-10°C / min, more preferably 3-8°C / min, such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, preferably a range value with any of the above values as the upper or lower limit.
[0049] After the first stage of sintering, the temperature is raised for the second stage of sintering, and the temperature of the second stage of sintering is preferably 500-600°C, more preferably 530-580°C, such as 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, preferably a range value with any of the above values as the upper or lower limit; the holding time of the second stage of sintering is preferably 1-2 hours. The heating rate of the first stage of sintering is preferably 1-10°C / min, more preferably 3-8°C / min, such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, preferably a range value with any of the above values as the upper or lower limit.
[0050] After the second stage sintering, the temperature is continued to be raised for the third stage sintering. The temperature of the three stage sintering is preferably 700-800°C, more preferably 730-780°C, such as 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, preferably a range value with any of the above values as the upper or lower limit; the holding time of the three stage sintering is preferably 1-20 hours, more preferably 5-15 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, preferably a range value with any of the above values as the upper or lower limit; the heating rate of the one-stage sintering is preferably 1-10°C / min, more preferably 3-8°C / min, such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, preferably a range value with any of the above values as the upper or lower limit.
[0051] In the present invention, in the three-stage sintering process, the heating rates of the first stage sintering, the second stage sintering and the third stage sintering show a decreasing trend, so that the temperature of the material at various locations in the sagger is uniform, ensuring the consistency of the material.
[0052] In the present invention, the three-stage sintering process is carried out in an oxygen-containing atmosphere, and the concentration of oxygen in the oxygen-containing atmosphere is preferably 85-100%, more preferably 90-95%, such as 90%, 91%, 92%, 93%, 94%, 95%, preferably a range value with any of the above values as the upper or lower limit.
[0053] After the three-stage sintering process is completed, the sintered material is crushed and sieved, mixed with a LiAlO2 aqueous solution, and stirred evenly. Then, an HF aqueous solution is added and stirred continuously to perform a coprecipitation reaction, and Al(OH)3 and LiF precipitates generated by the reaction of lithium metaaluminate and HF are attached to the surface of the high-nickel ternary material, and HF can neutralize the alkali on the surface of the material.
[0054] In the present invention, the molar concentration of the LiAlO2 aqueous solution is preferably 0.05-0.5 mol / L, more preferably 0.1-0.4 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, preferably any of the above values as the upper limit or lower limit. The concentration of the HF aqueous solution is preferably 0.05-0.5 mol / L, more preferably 0.1-0.4 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, preferably with any of the above values as the upper or lower limit.
[0055] The mass ratio of the sintered material to the LiAlO2 aqueous solution is preferably 1:(0.5-10), more preferably 1:(1-8), such as 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, preferably a range value with any of the above values as the upper or lower limit.
[0056] The mass ratio of the sintered material to the HF aqueous solution is preferably 1:(0.5-10), more preferably 1:(1-8), such as 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, preferably a range value with any of the above values as the upper or lower limit.
[0057] The molar ratio of LiAlO2 to HF is preferably 1:(0.5-4), more preferably 1:(1-3), such as 1:1, 1:1.5, 1:2, 1:2.5, 1:3, preferably a range value with any of the above values as the upper or lower limit.
[0058] The present invention has no special limitation on the time of the mixing and stirring, as long as it can ensure uniform mixing or complete reaction. Specifically, in an embodiment of the present invention, the stirring time may be 30 minutes.
[0059] After the coprecipitation reaction, the present invention performs solid-liquid separation on the obtained coprecipitation system, such as suction filtration, and dries the obtained filter cake, such as by oven drying, to obtain an intermediate material.
[0060] In the present invention, the drying temperature is preferably 20-500°C, more preferably 120-240°C, such as 100°C, 120°C, 150°C, 180°C, 200°C, 220°C, 240°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, preferably a range value with any of the above values as the upper or lower limit.
[0061] The dried intermediate material is sintered again, and after sintering, it is cooled to room temperature in the furnace to obtain a positive electrode material with a layer of Al2O3 and LiF coated on the surface. LiF on the positive electrode surface can stabilize the positive electrode structure and has good Li + conductivity and can stabilize the interface, so the material has a higher capacity and a more stable structure.
[0062] In the present invention, the sintering temperature is preferably 200-350°C, more preferably 250-300°C, such as 200°C, 250°C, 300°C, 350°C, preferably a range value with any of the above numerical values as the upper or lower limit; the sintering holding time is preferably 1-15 hours, more preferably 5-10 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, preferably a range value with any of the above numerical values as the upper or lower limit; the heating rate of the one-stage sintering is preferably 1-10°C / min, more preferably 3-8°C / min, such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 10°C / min, preferably a range value with any of the above numerical values as the upper or lower limit.
[0063] The present invention also provides a lithium-ion battery, comprising the long-life positive electrode material mentioned above.
[0064] The present invention provides a long-life positive electrode material, comprising a high-nickel ternary positive electrode material and a coating layer coated on the surface of the high-nickel ternary positive electrode material; the coating layer comprises Al2O3 and LiF. The present invention coats a dense layer of Al2O3 and LiF on the surface of the high-nickel ternary positive electrode material by wet coprecipitation, thereby improving the safety and stability of the ternary material, while improving the rate performance and average discharge voltage of the battery, and reducing the high-temperature storage gas generation of the material, so that the battery composed of this material has stronger practicality, higher energy density, and higher energy conversion efficiency. The 2430 button cell made of the material of the present invention has an initial coulombic efficiency of more than 90% ((initial discharge capacity / initial charge capacity)*100%), a gram capacity of more than 200mAh / g; it is assembled into an 800mAh soft-pack battery with an average voltage (discharge energy / discharge capacity) of more than 3.65V at 0.2C charge and discharge, a 300-cycle capacity retention rate of more than 94% at 45°C ((300-cycle discharge capacity / first-cycle discharge capacity)*100%), and an energy efficiency ratio of more than 85% ((discharge energy÷charge energy)*100%).
[0065] In order to further illustrate the present invention, a long-life positive electrode material, a preparation method thereof and a lithium-ion battery provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0066] Example 1
[0067] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.05 and passed through a 200-mesh sieve.
[0068] The temperature was raised to 450°C at a heating rate of 5°C / min and kept at this temperature for 2 hours; the temperature was raised to 550°C at a heating rate of 2°C / min and kept at this temperature for 2 hours; the temperature was raised to 750°C at a heating rate of 1°C / min and kept at this temperature for 10 hours, and then the furnace was cooled to room temperature; the oxygen concentration needed to be maintained at 95%±2% during the sintering process.
[0069] The obtained material was crushed and sieved, mixed with LiAlO2 aqueous solution (LiAlO2 concentration 0.2 mol / L) at a ratio of 1:10, stirred for 30 minutes, and HF solution was added at a molar ratio of LiAlO2 to HF of 1:2.5, with a HF solution concentration of 0.1 mol / L. Stirring was continued for half an hour and then ended.
[0070] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dry-dried at 200°C;
[0071] The dried material was heated to 300°C at a heating rate of 5°C / min, kept at this temperature for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material;
[0072] Example 2
[0073] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.02 and passed through a 200-mesh sieve.
[0074] Heating to 450℃ at a rate of 5℃ / min, keeping warm for 2h; then heating to 550℃ at a rate of 2℃ / min, keeping warm for 2h; then heating to 750℃ at a rate of 1℃ / min, keeping warm for 10h, and then cooling to room temperature with the furnace; the oxygen concentration needs to be maintained at 95%±2% during the sintering process
[0075] The obtained material was crushed and sieved, mixed with LiAlO2 aqueous solution at a ratio of 1:10, stirred for 30 minutes, and HF solution was added, wherein the LiAlO2 concentration was 0.2 mol / L, the HF solution concentration was 0.1 mol / L, and the LiAlO2 and HF were added at a molar ratio of 1:2.5. Stirring was continued for half an hour and then ended.
[0076] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dried at 200°C;
[0077] The dried material was heated to 300°C at a heating rate of 5°C / min, kept at this temperature for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material;
[0078] Example 3
[0079] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.02 and passed through a 200-mesh sieve.
[0080] Heating to 450℃ at a rate of 5℃ / min, keeping warm for 2h; then heating to 550℃ at a rate of 2℃ / min, keeping warm for 2h; then heating to 750℃ at a rate of 1℃ / min, keeping warm for 10h, and then cooling to room temperature with the furnace; the oxygen concentration needs to be maintained at 95%±2% during the sintering process
[0081] The obtained material was crushed and sieved, mixed with LiAlO2 aqueous solution at a ratio of 1:5, stirred for 30 minutes, and HF solution was added, wherein the concentration of LiAlO2 was 0.3 mol / L, the concentration of HF solution was 0.1 mol / L, and the ratio of LiAlO2 to HF was 1:2.5. Stirring was continued for half an hour and then ended.
[0082] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dried at 200°C;
[0083] The dried material was heated to 300°C at a heating rate of 5°C / min, kept at this temperature for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material;
[0084] Comparative Example 1
[0085] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.02 and passed through a 200-mesh sieve.
[0086] Heating to 450℃ at a rate of 5℃ / min, keeping warm for 2h; then heating to 550℃ at a rate of 2℃ / min, keeping warm for 2h; then heating to 750℃ at a rate of 1℃ / min, keeping warm for 10h, and then cooling to room temperature with the furnace; the oxygen concentration needs to be maintained at 95%±2% during the sintering process
[0087] The obtained material was crushed and sieved, mixed with water, and stirred for 30 minutes;
[0088] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dried at 200°C;
[0089] The dried material was mixed with nano-Al2O3 (content 500ppm) and then sieved, heated to 300°C at a heating rate of 5°C / min, kept warm for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material;
[0090] Comparative Example 2
[0091] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.02 and passed through a 200-mesh sieve.
[0092] Heating to 450℃ at a rate of 5℃ / min, keeping warm for 2h; then heating to 550℃ at a rate of 2℃ / min, keeping warm for 2h; then heating to 750℃ at a rate of 1℃ / min, keeping warm for 10h, and then cooling to room temperature with the furnace; the oxygen concentration needs to be maintained at 95%±2% during the sintering process
[0093] The obtained material was crushed and sieved, mixed with water, and stirred for 30 minutes;
[0094] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dried at 200°C;
[0095] The dried material was mixed evenly with nano-Al2O3 (content 500ppm) and LiF (content 800ppm) and then sieved. The temperature was increased to 300°C at a heating rate of 5°C / min, kept warm for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material.
[0096] Comparative Example 3
[0097] The polycrystalline precursor Ni 0.83 Co 0.12 Mn 0.05 (OH)2 and LiOH were mixed in a molar ratio of 1:1.02 and passed through a 200-mesh sieve.
[0098] Heating to 450℃ at a rate of 5℃ / min, keeping warm for 2h; then heating to 550℃ at a rate of 2℃ / min, keeping warm for 2h; then heating to 750℃ at a rate of 1℃ / min, keeping warm for 10h, and then cooling to room temperature with the furnace; the oxygen concentration needs to be maintained at 95%±2% during the sintering process
[0099] The obtained material was crushed and sieved, mixed with 0.2 mol / L AlCl3 aqueous solution at a ratio of 1:10, stirred for 30 min, and then washed with water to remove the residual Cl - After washing off, it's over.
[0100] After filtration, a high-nickel ternary filter cake is obtained, and the filter cake is dried at 200°C;
[0101] The dried material was heated to 300°C at a heating rate of 5°C / min, kept at this temperature for 10 hours, and finally cooled to room temperature in the furnace to obtain a high-nickel positive electrode material.
[0102] Test method:
[0103] 1.BET: Tested using N2 adsorption method;
[0104] 2. Tap density: Tested using a tap density meter
[0105] 3. Residual alkali: Use an automatic potentiometric titrator to test the Li2CO3 and LiOH content and calculate the Free Li + content.
[0106] 4. Button test: Mix and slurry according to high nickel ternary: SP: PVDF = 90%: 5%: 5%, and coat the slurry on 16μm aluminum foil. The surface density is controlled at 17mg / cm 2 After roller pressing, the compaction is controlled at 3.4mg / cm 3 , assembled into 2430 button cells, the battery test was carried out at 0.1C charge and discharge test capacity, the test voltage range was 2.5V-4.3V, and the first coulomb efficiency was (first discharge capacity) / first charge capacity.
[0107] 5. Full electric test: According to the high nickel ternary: SP: KS-6: PVDF = 94.5%: 2%: 1%: 2.5% mixture to make positive electrode slurry, through coating and rolling process to make positive electrode sheet, the surface density of the electrode sheet is controlled at 16mg / cm 2 The negative electrode uses artificial graphite, which is homogenized according to the ratio of graphite: SP: CMC: SBR = 95.5%: 1%: 1.5%: 2%, and the coating surface density is controlled at 10mg / cm 2 The diaphragm uses a 20μm dry PP / PE / PP diaphragm, the electrolyte is a conventional electrolyte, the main components are EC, DMC, DEC, and contains additives such as VC and PS, the lithium salt is 1mol / L LiPF6, and it is assembled into a 503048 model battery with a battery capacity of about 800mAh. The voltage range for testing is 3.0-4.25V;
[0108] 5.1 1C charge and discharge calculation of the average voltage of the battery cell, the calculation method is discharge energy / discharge capacity;
[0109] 5.2 0.5C charging, 0.2C, 0.5C, 1C, 2C discharging test the discharge rate performance of the battery cell. The calculation method is 0.2C / 0.2C; 0.5C / 0.2C; 1C / 0.2C; 2C / 0.2C to calculate the capacity ratio;
[0110] 5.3 The battery cell is charged and discharged at the standard capacity of 1C. After being fully charged, it is discharged at 0.2C for 2.5h, and then at 4C / 30s. The voltage before and after discharge is recorded. The ratio of the difference to the current is the DCR value, in mΩ.
[0111] 5.4 The battery cell is fully charged and stored at 70°C for 7 days to test the volume change before and after storage, and the gas production volume is compared in ml / Ah;
[0112] 5.5 1C charge and discharge cycle 45℃ cycle 500 weeks to compare its capacity retention rate (such as Figure 1 ).
[0113] The test results are shown in Tables 1 and 2.
[0114] Table 1 Physical property test data of the embodiments of the present invention and the comparative examples
[0115]
[0116] Table 2 Electrochemical performance test data of the embodiments of the present invention and the comparative examples
[0117]
[0118] The above data show that the wet coating has a slightly higher gram capacity than the dry coating, has better gas production than the dry coating, and has a 500-week capacity retention rate that is about 1.5% higher than the dry coating.
[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a long-life positive electrode material, comprising the following steps: A) mixing the precursor and the lithium source uniformly, and sieving to obtain a mixed raw material; B) in an oxygen-containing atmosphere, heating the mixed raw material to 300-500° C., keeping the temperature for 2-10 hours, and performing a first-stage sintering; then heating the mixed raw material to 500-600° C., keeping the temperature for 1-2 hours, and performing a second-stage sintering; finally heating the mixed raw material to 700-800° C., keeping the temperature for 1-20 hours, and performing a third-stage sintering, and cooling the mixed raw material to room temperature with the furnace after the third-stage sintering is completed; C) mixing the material obtained by the three-stage sintering with the LiAlO2 aqueous solution, then adding the HF aqueous solution and stirring until the reaction is complete; The molar ratio of LiAlO2 to HF is 1:(1.5-4); D) subjecting the system obtained by the complete reaction in step C) to solid-liquid separation and drying to obtain an intermediate; E) sintering the intermediate at 200-350° C. for 1-15 hours to obtain a positive electrode material with a long life; The long-life positive electrode material comprises a high-nickel ternary positive electrode material and a coating layer coated on the surface of the high-nickel ternary positive electrode material; The coating layer includes Al2O3 and LiF, and a surface portion of LiF is coated by Al2O3.
2. The preparation method according to claim 1, characterized in that: The molecular formula of the high-nickel ternary positive electrode material is shown in Formula I: LiNi a Co b Mn c O2 Formula I; Among them, 0.5≤a<1, 0<b<0.5, 0<c<0.2, a+b+c=1.
3. The preparation method according to claim 1, characterized in that: The mass ratio of Al2O3 to LiF in the coating layer is (0.1-2):
1.
4. The preparation method according to claim 1, characterized in that: The specific surface area of the positive electrode material is 0.2 to 1.0 m 2 / g, Li2CO3 content ≤ 3000ppm, LiOH content ≤ 5000ppm, Free Li + Content ≤2000ppm.
5. The preparation method according to claim 1, characterized in that: The precursor is Ni a Co b Mn c (OH)2; 0.5≤a<1, 0<b<0.5, 0<c<0.2, and a+b+c=1; The lithium source is one or more of LiOH, Li2CO3, LiNO3 and CH3COOLi; The molar ratio of the precursor to the lithium source is 1:(0.8-1.2).
6. The preparation method according to claim 1, characterized in that: In the oxygen-containing atmosphere in step B), the concentration of oxygen is 85-100%.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the material obtained by the three-stage sintering to the LiAlO2 aqueous solution is 1:(0.5-10); The mass ratio of the material obtained by the three-stage sintering to the HF aqueous solution is 1:(0.5-10).
8. The preparation method according to claim 1, characterized in that: The drying temperature in step D) is 20-500°C.
9. A lithium ion battery, characterized in that: A long-life positive electrode material prepared by the preparation method according to any one of claims 1 to 8.