Method for producing fiber-containing sheet and fiber-containing sheet

By using resin containing fiber material as the core layer and resin not containing fiber material as the leather layer in the T-shaped mold, the fiber orientation is suppressed, and the problem of the fiber-containing sheet is reduced in the vertical direction is solved, and the strength of the fiber-containing sheet is achieved in all directions. Strong sheet molding simplifies the process and reduces costs.

CN115038569BActive Publication Date: 2024-11-08HITACHI ZOSEN CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180011983.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-13
Filing Date
2021-01-27
Publication Date
2024-11-08
Estimated Expiration
2041-01-27

AI Technical Summary

Technical Problem

The strength of the fiber-containing sheet formed by T-shaped molds increases in the longitudinal direction, but the strength of the vertical direction is significantly reduced, and the prior art requires special technology, time and cost to suppress fiber orientation.

Method used

In the T-shaped mold, resin containing fiber material is used as the core layer and resin containing fiber material is not as the leather layer. By laminated structure and hot pressing, the orientation of the fiber is suppressed, thereby forming a sheet with strength in all directions.

Benefits of technology

The fiber orientation is easily and precisely suppressed, resulting in fiber-containing sheets with strength in all directions, simplifying the molding process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115038569B_ABST
    Figure CN115038569B_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a fiber-containing sheet. In the method, when a resin is extruded into a sheet using a T-die, extrusion molding is performed by extruding a first resin for forming a core layer and a second resin for forming two skin layers located on both surfaces of the core layer. At this time, a resin containing a fiber material is used as the first resin, and a resin not containing a fiber material is used as the second resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a fiber-containing sheet and the fiber-containing sheet. Background Art

[0002] When a plastic composite material containing fiber materials such as carbon fiber or glass fiber in a resin is molded, the fibers are sometimes oriented in the longitudinal direction (MD) of the molded body. The occurrence of this orientation is particularly prominent in sheet extrusion molded products using a T-die. Due to the orientation in the MD, the strength of the molded sheet in the MD direction increases. This technology of molding a plastic composite material containing fiber materials using a T-die is described, for example, in JPH08-269210A. Summary of the invention

[0003] Technical Problems to be Solved by the Invention

[0004] However, as described above, a sheet formed by this method and oriented in the MD has a tendency to have a significantly reduced strength in the direction perpendicular to the MD (TD) while having a high strength in the MD.

[0005] As a countermeasure, multiple sheets oriented in the MD are stacked while changing their angles and integrated by hot pressing to obtain a sheet with strength in all directions. However, this method requires special technology, molding time and cost.

[0006] Therefore, an object of the present invention is to solve such a technical problem and to make it possible to easily and reliably obtain a fiber-containing sheet with suppressed orientation.

[0007] Technical means to solve technical problems

[0008] In order to achieve this object, the manufacturing method of the fiber-containing sheet of the present invention is characterized in that when a resin is extruded into a sheet using a T-die, extrusion molding is performed by extruding a first resin for forming a core layer and a second resin for forming two skin layers located on both surfaces of the core layer in a stacked state, and at this time, a resin containing a fiber material is used as the first resin, and a resin not containing a fiber material is used as the second resin.

[0009] That is, the present invention is completed based on the following knowledge: the reason why the fibers in the resin of the composite material containing fibers are oriented is that when the molten resin and the fibers flow into the T-die in a mixed state and finally expand into a sheet in the T-die, the fibers are oriented in the direction along the MD due to the resistance of the wall surface of the flow path. According to the present invention, when extrusion molding using the T-die is performed, the skin layers are arranged on both surfaces of the core layer, and the core layer is molded with the resin containing the fiber material, and the two skin layers are molded with the resin not containing the fiber material, so that the resin containing the fiber material of the core layer is extruded from the T-die in a manner that does not contact the wall surface of the flow path of the T-die, and thus, it is molded into a sheet in a state where the orientation of the fibers is suppressed.

[0010] According to the method for producing a fiber-containing sheet of the present invention, the first resin of the core layer and the second resin of the two skin layers are preferably molded into one body in a mutually removable state. Thus, by peeling the skin layer from the core layer after molding, a sheet with a fiber-containing resin with suppressed orientation exposed on the surface can be obtained.

[0011] According to the method for producing a fiber-containing sheet of the present invention, in order to achieve good separation between the first resin of the core layer and the second resin of the two skin layers, it is preferred that the first resin for forming the core layer and the second resin for forming the skin layers are incompatible resins.

[0012] According to the method for producing a fiber-containing sheet of the present invention, a sheet having a fiber-containing resin with suppressed orientation exposed on the surface can be easily obtained by peeling at least one skin layer from a molded body obtained in an integrally laminated state.

[0013] According to the method for producing a fiber-containing sheet of the present invention, it is also preferred that the first resin of the core layer and the second resin of the two skin layers are integrally molded in a mutually non-peelable state. Thus, a fiber-containing sheet with suppressed orientation can be easily obtained without a peeling step.

[0014] According to the method for manufacturing a fiber-containing sheet of the present invention, it is also preferable to use compatible resins as the first resin for forming the core layer and the second resin for forming the skin layer. This makes it easy to form the first resin of the core layer and the second resins of the two skin layers into one body in a state that they cannot be separated from each other.

[0015] The fiber-containing sheet of the present invention is characterized by comprising a core layer made of a first resin containing a fiber material and skin layers made of a second resin containing no fiber material disposed on both surfaces of the core layer, wherein the skin layers are releasable from the core layer.

[0016] Another fiber-containing sheet of the present invention is characterized in that a first resin core layer containing a fiber material and second resin skin layers not containing a fiber material and arranged on both surfaces of the core layer are integrally formed.

[0017] Effects of the Invention

[0018] According to the present invention, a fiber-containing sheet with suppressed orientation can be easily and reliably obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a diagram showing the cross-sectional structure of key components of a fiber-containing sheet according to an embodiment of the present invention.

[0020] Figure 2 This is a diagram showing a structural example of a T-die that can be used in the method for producing a fiber-containing sheet according to an embodiment of the present invention.

[0021] Figure 3 This is a diagram showing a comparison between an enlarged image of the surface of the core layer in Example 2 and an enlarged image of the surface of the molded body in Comparative Example 1. DETAILED DESCRIPTION

[0022] right Figure 2 The detailed structure of the T-die shown in the figure is described. The T-die 11 shown in the figure is formed by joining a die 12 and a feed block 13 to each other and integrating them.

[0023] The feed block 13 is provided with a first path 14 for supplying a molten fiber-containing resin material for the core layer, and a pair of second paths 15, 15 for supplying a molten resin material for the skin layer. Reference numeral 16 is a confluence portion where the molten resin materials from the paths 14, 15, 15 are confluenced. At this time, the molten resin material for the skin layer from the second path 15 is supplied to both sides of the molten fiber-containing resin material for the core layer from the first path 14. As a result, these molten resin materials are transported to the mold 12 in a three-layer state.

[0024] The die 12 has a narrow nozzle 18 and is formed by moving the nozzle 18 perpendicular to the Figure 2 19 is a guide path for the resin delivered from the feed block 13, and 20 is a manifold. The manifold 20 is configured so that the flow path for the molten resin material from the guide path 19 is perpendicular to the paper surface. Figure 2 in the direction of the paper so that it can be expanded in the above perpendicular Figure 2 The structure is configured so as to supply a sufficient amount of resin to the long nozzle 18 in the direction of the paper surface.

[0025] In the T-shaped die 11 shown in the figure, the resin material flows perpendicular to the Figure 2 The core layer is expanded once in the direction of the paper surface (for example, a width of about 100 mm), and after being stacked at the confluence portion 16, it is expanded again at the manifold 20 of the mold 12. By adopting this structure, it is possible to prevent the core layer from contacting the wall surface of the resin flow path in a thin state, so that the orientation can be further suppressed on the basis of the orientation suppression effect described later.

[0026] In the manufacturing method of the present invention, the T-die 11 is not limited to the above-mentioned structure, and any structure of the T-die can be used as long as it can extrude a sheet having a laminated structure in which skin layers are arranged on both surfaces of a core layer.

[0027] For example, Figure 2 Although not shown, the T-shaped die in which the resin material is expanded to the width of the product at the first path 14 and the second path 15, 15 and then stacked can also implement the manufacturing method of the present invention. Figure 2 The molding is shown in the above two stages. At this time, a confluence of the resin material after the width is expanded can be set immediately after the manifold 20. When the method of the present invention is implemented using such a T-die, although the orientation of the sheet is slightly deteriorated, the sheet can be manufactured in a state where the thickness is controlled with good accuracy.

[0028] According to the present invention, using Figure 2 The T-die 11 of the structure shown feeds the molten fiber-containing resin material for the core layer from the outside of the system into the first path 14 in the feed block 13, and feeds the molten resin material for the skin layer from the outside of the system into a pair of second paths 15, 15. Thus, these resin materials are extruded in the form of sheets in a stacked state from the nozzle 18 of the T-die 11 in the above-mentioned manner.

[0029] Figure 1 The cross-sectional structure of the key parts of the sheet-shaped molded body formed by the resin extruded from the T-die 11 and then cooled and solidified is shown. 25 is the core layer. 26 and 26 are skin layers, which are formed in a state of contacting both surfaces of the core layer 25.

[0030] The core layer 25 has a structure in which a fiber material 28 is contained in a resin 27. The skin layers 26, 26 have a structure in which no fiber material is contained in the resin.

[0031] As the resin forming the core layer 25, any thermoplastic resin can be used as long as it can be extruded from the T-die 11 in a molten state. For example, polyolefins such as polyethylene or polypropylene, polyamide, polyester, polycarbonate, polystyrene, polylactic acid, polyvinyl chloride, liquid crystal polymer, polyphenylene sulfide, polyetheretherketone, polyetherimide, etc. can be listed. The fiber material 28 is a component added mainly for strengthening the resin 27. As long as this purpose can be achieved, any fiber material can be used as appropriate. For example, carbon fiber, glass fiber, boron fiber, high-strength resin fiber, cellulose fiber, etc. can be listed.

[0032] As described above, the skin layers 26, 26 are formed in contact with both surfaces of the core layer 25. As the resin constituting the skin layers 26, 26, there can be listed a resin that is incompatible with the resin constituting the core layer 25 or a resin that is compatible with the resin constituting the core layer 25. When the resin constituting the skin layers 26, 26 is a resin that is incompatible with the resin constituting the core layer 25, such as Figure 1 As shown by the dotted line, at least one skin layer 26, 26 can be peeled off from the surface of the sheet-like molded body, and the molded body is composed of only the core layer 25. When the resin constituting the skin layers 26, 26 is a resin that is compatible with the resin constituting the core layer 25, as shown in FIG. Figure 1 As shown by the solid line in the middle, a molded body having a structure in which the core layer 25 and the skin layers 26, 26 are integrated in a non-separable manner can be obtained.

[0033] As an example of a combination of compatible resins, for example, the resin constituting the core layer 25 and the resin constituting the skin layers 26, 26 are both polypropylene, that is, the case where both are the same resin. As an example of a combination of incompatible resins, for example, the case where the resin constituting the core layer 25 is polypropylene and the resin constituting the skin layers 26, 26 is high-density polyethylene; or the case where the resin constituting the core layer 25 is polypropylene and the resin constituting the skin layers 26, 26 is polycarbonate, etc. can be cited.

[0034] Forming Figure 1 When the molded body shown in Figure 2 In the T-die 11 shown, the resins constituting the skin layers 26, 26 are sandwiched with the resin constituting the core layer 25, and these resins are extruded and molded by the T-die 11. Therefore, the resins constituting the skin layers 26, 26 are in contact with the wall surface of the resin flow path in the T-die 11, but the resin constituting the core layer 25 is not in contact with the wall surface of the resin flow path in the T-die 11, and is extruded by the T-die 11. Therefore, the resin constituting the core layer 25 does not receive resistance from the wall surface of the resin flow path, and thus, the core layer 25 as a molded body can be formed in a state where the orientation of the fiber material 28 on the surface of the core layer 25 and its vicinity is suppressed.

[0035] The skin layers 26, 26 are layers that prevent the resin constituting the core layer 25 from contacting the wall surface of the resin flow path when the resin flows in a molten state along the resin flow path in the T-die 11. Therefore, it is sufficient as long as it has the minimum thickness required to exert this function. For example, as long as the thickness of the skin layer 26 is more than 10μm, it can be said to be effective, but when its thickness is between 10 and 50μm, there is a problem of interlayer disorder (flow marks) or the orientation of the fiber material 28 is not suppressed. Therefore, the thickness of the skin layer is preferably more than 50μm. The total thickness of the core layer 25 and a pair of skin layers 26, 26 can be appropriately set in combination with the purpose of the molded product.

[0036] As described above, the skin layers 26, 26 only need to be layers that prevent the resin constituting the core layer 25 from contacting the wall surface of the resin flow path when the resin flows in a molten state along the resin flow path in the T-die 11. Therefore, although the skin layers 26, 26 do not contain fiber materials in principle, as long as the fiber materials can be prevented from being oriented in the core layer 25, it is acceptable even if the skin layers 26, 26 contain some fiber materials. In the present invention, the skin layers 26, 26 that do not contain fiber materials in the resin broadly include such cases.

[0037] Example

[0038] In the following Examples and Comparative Examples, various physical properties were measured in the following manner.

[0039] (1) Degree of orientation

[0040] The molten resin discharged from the core layer extruder and the skin layer extruder (Hitachi Zosen Corporation: HMT57, SHT65) was stacked in a feed block (Hitachi Zosen Corporation: FB3), expanded to a width of 1020 mm in a T-die (Hitachi Zosen Corporation: TFS102F), and then squeezed and solidified by the roll of a sheet forming machine (Hitachi Zosen Corporation: GOMP120.3) to form the sheet. The formed sheet was cut into a length of 1 m, and the surface of a 30 mm square piece cut from the sheet was observed using an optical microscope (KEYENCE CORPORATION: VHX-900) to confirm the orientation with the naked eye.

[0041] (2) Peelability of the core layer and the skin layer

[0042] The peelability was confirmed by making an incision in a part of the cortex with a sharp knife such as a utility knife, grabbing one part of the cortex and the other part of the cortex by hand, pulling them in different directions to peel them off.

[0043] (Example 1)

[0044] As a material for constituting the core layer, a polypropylene resin containing 30% by mass of carbon fibers (manufactured by Mitsubishi Chemical Corporation, product name / product number: PYROFIL PP-C-30) was used, and as a material for constituting the two skin layers, a polypropylene resin (manufactured by Japan Polypropylene Corporation, product number: EA9) was used. Figure 2 The T-shaped die of the structure shown was used to produce a sheet-shaped molded body with a thickness of 0.7 mm and a width of 1002 mm by extrusion molding. The thickness ratio of the two skin layers to the core layer was skin layer: core layer: skin layer = 1:6:1.

[0045] In the obtained molded body, the core layer and the skin layer were firmly integrated and could not be separated by the above method. The surface of the core layer was observed from above the surface of the skin layer under a microscope. As a result, no obvious directionality was confirmed for the orientation of the carbon fibers, and it was considered that the carbon fibers were randomly oriented.

[0046] Table 1 shows the production conditions and the measurement results of physical properties of Example 1.

[0047]

[0048] (Examples 2 to 4)

[0049] Compared with Example 1, the production conditions were changed as shown in Table 1. Other conditions were the same as those of Example 1.

[0050] Table 1 shows the production conditions and the measurement results of physical properties of Examples 2 to 4.

[0051] (Example 5)

[0052] Compared with Example 4, the material constituting the skin layer was changed to high-density polyethylene (manufactured by Japan Polypropylene Corporation, product number: HF313) which is incompatible with the resin constituting the core layer.

[0053] Table 1 shows the production conditions and the measurement results of physical properties of Example 5.

[0054] (Example 6)

[0055] Compared with Example 3, the material for constituting the skin layer was changed to the following material. That is, the material obtained by blending the above-mentioned polypropylene and high-density polyethylene in a mass ratio of polypropylene:high-density polyethylene=2:1 was used as the material for constituting the skin layer. Other than this, the same as Example 3 was used.

[0056] Table 1 shows the production conditions and the measurement results of physical properties of Example 6.

[0057] (Example 7)

[0058] Compared with Example 3, the material constituting the skin layer was changed to polycarbonate resin (manufactured by Mitsubishi Engineering-Plastics Corporation, product number: E-2000).

[0059] Table 1 shows the production conditions and the measurement results of physical properties of Example 7.

[0060] (Comparative Example 1)

[0061] Only the material for constituting the core layer used in Example 1 was used to obtain a sheet-shaped molded body having no skin layer.

[0062] Table 1 shows the production conditions and the measurement results of physical properties of Comparative Example 1.

[0063] As shown in Table 1, no obvious directionality was confirmed for the orientation of the carbon fibers in the sheet-like molded bodies of Examples 1 to 7, and the carbon fibers were randomly oriented. However, in Comparative Example 1, since the molded body was formed without using a material for constituting the skin layer, the carbon fibers in the resin in the molded body were strongly oriented in the MD direction. Figure 3 The enlarged images of the surfaces of the core layers of Example 2 and Comparative Example 1 are shown. In the figure, the upper side is the image of Example 2, and the lower side is the image of Comparative Example 1. From the image, it can be confirmed that the carbon fibers in Comparative Example 1 have obvious directionality, while the carbon fibers in Example 2 do not have obvious directionality but are randomly oriented.

[0064] In Examples 1 to 4 and 6, the material for constituting the core layer and the material for constituting the skin layer are the same material and are compatible with each other, so the skin layer and the core layer are firmly integrated. However, in Examples 5 and 7, the material for constituting the core layer and the material for constituting the skin layer are different materials and are not compatible with each other, so the skin layer can be easily peeled off from the core layer after molding. Thus, a sheet-shaped molded body can be formed only of a material containing a fiber material in a resin.

Claims

1. A method for producing a fiber-containing sheet, characterized in that: When a resin is extruded into a sheet using a T-die, extrusion molding is performed by extruding a first resin for forming a core layer and a second resin for forming two skin layers located on both surfaces of the core layer in a stacked state. At this time, a resin containing a fiber material is used as the first resin, and a resin not containing a fiber material is used as the second resin. As the first resin for molding into the core layer and the second resin for molding into the two skin layers, resins that are incompatible with each other are used, and the first resin for the core layer and the second resin for molding into the two skin layers are molded into a whole in a state where they can be peeled off from each other. In the molded body obtained in the integrated stacked state, the thickness of each skin layer is 50 μm or more, and at least one skin layer is peeled off from the molded body obtained in the integrated stacked state.