A cathode two-component electrophoretic paint coating process

Through the cathode two-component electrophoretic paint coating process, including substrate pretreatment and vacuum coating, the problems of poor surface pretreatment of the substrate and unstable tank liquid performance are solved, and high-quality paint film and protection effect are achieved, avoiding loss of Paint and magnetism are reduced.

CN115044905BActive Publication Date: 2024-11-22JIANGSU RENSHENG AUTO PARTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210849653.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-19
Publication Date
2024-11-22
Estimated Expiration
2042-07-19

AI Technical Summary

Technical Problem

The surface pretreatment effect of the substrate is poor, resulting in failure of coating protection and coloring, waste of spraying materials and evaporation of harmful gases, unstable performance of the cathode electrophoresis tank liquid, resulting in paint loss of substrate, and it is difficult for single-layer coating to ensure wear resistance, especially It has a serious impact on magnetic substrates.

Method used

The cathode two-component electrophoretic paint coating process is adopted, including substrate pretreatment (cutting, oil removal, etching, chemical polishing, cleaning), the electrophoresis tank pH value is controlled between 4.5-6.5, vacuum coating is carried out, and bisphenol A type is used. Medium-high molecular weight epoxy resin is used as a film forming material, magnetron sputtering coating, and double-layer coating protective substrate.

Benefits of technology

Stabilize and control the pH value of the tank liquid, improve the quality of the paint film, avoid paint loss and the impact strength of the paint film, protect the substrate, improve the coating bonding and corrosion resistance, maintain magnetic properties, and reduce material waste and harmful gas volatility.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a cathode two-component electrophoretic paint coating process, and specifically relates to the technical field of electrophoretic paint coating processes. By cutting, degreasing, etching, chemical polishing and cleaning the substrate, a protective film layer is formed on the surface of the substrate, the outer surface of the substrate is effectively protected, the flatness and corrosion resistance of the substrate are effectively improved, and the influence on the performance of the substrate during the coating process is avoided, so as to protect and color the coating. By regulating the parameters in the cathode electrophoresis process, the bath liquid is always within a stable pH value range, the film thickness conversion is easy, the quality of the paint film is effectively guaranteed, and the paint is not easy to fall off and the impact strength of the paint film is reduced. At the same time, the substrate is protected by a double-layer coating method, which further protects the substrate and is not easy to affect its own magnetism, so that the process effectively solves the problems of coating bonding force, cracking, plating leakage and discoloration, and further improves the coating effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrophoretic paint coating technology, and more specifically, to a cathode two-component electrophoretic paint coating technology. Background Art

[0002] Electrophoretic paint, also known as electrophoretic coating, is still used by many people instead of "electrophoretic coating". As the defects of conventional spraying continue to emerge, electrophoresis has become more and more popular. Electrophoretic paint has also been constantly updated, from anode electrophoretic paint to cathode electrophoretic paint, from single-component electrophoretic paint to two-component electrophoretic paint. The development of electrophoretic paint has also promoted the development of electrophoretic coating, so that more products no longer use spraying technology but electrophoresis. Electrophoretic coatings and coating methods have been industrially applied since the 1960s. Electrophoretic coatings can be used for fully closed circulation system operation, and the coating utilization rate can reach about 95%. Electrophoretic coatings use water-soluble or water-dispersible ionic polymers as film-forming materials. The coated workpiece can be used as an anode or a cathode. Electrophoretic coatings can be divided into anode electrophoretic coatings and cathode electrophoretic coatings according to the electrode of the coated workpiece; according to the ion form of the film-forming material in water, they can be divided into anionic electrophoretic coatings and cationic electrophoretic coatings. Cathodic electrophoretic coatings can be divided into single-component electrophoretic coatings and two-component electrophoretic coatings according to their water dispersion state; they can also be divided into thin-film type, medium-thick film type and thick film type cathodic electrophoretic coatings according to film thickness.

[0003] New decorative green and environmentally friendly metal surface treatment processes such as electrophoretic paint and vacuum plating have been increasingly used. Existing insulation and anti-corrosion functions mostly use coating processes. Commonly used coating treatments include surface cleaning and other processes. If the surface pretreatment of the substrate is not effective, it cannot protect and color the coating, which can easily lead to waste of spray materials and volatilization of harmful gases. In the cathode electrophoretic process, with different electrophoretic coatings, it is often easy to ignore the various adjustments of electrophoretic parameters, resulting in unstable tank performance, making the substrate prone to paint peeling and falling off in flakes. At the same time, it is difficult to ensure the wear resistance of a single-layer coating. Coating a magnetic substrate can easily reduce the magnetic properties, seriously affecting product quality. Therefore, a cathode two-component electrophoretic paint coating process is needed to solve the above problems. Summary of the invention

[0004] In order to overcome the above-mentioned defects of the prior art, the present invention provides a cathode two-component electrophoretic paint coating process. The technical problem to be solved by the present invention is: the surface pretreatment effect of the substrate is not good, and the coating cannot be protected and colored, which easily causes waste of spraying materials and volatilization of harmful gases. In the cathode electrophoretic process, with different electrophoretic coatings, the various adjustments of the electrophoretic parameters are often easily ignored, resulting in unstable tank liquid performance, making the substrate prone to paint peeling and falling off in flakes. At the same time, it is difficult to ensure the wear resistance of a single-layer coating. Coating on a magnetic substrate can easily reduce the magnetic properties, seriously affecting product quality.

[0005] To achieve the above object, the present invention provides the following technical solution: a cathode two-component electrophoretic paint coating process, comprising the following steps:

[0006] S1. Substrate pretreatment: Pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing, etching, chemical polishing and cleaning of the substrate.

[0007] S2. After the pretreatment of the substrate is completed, its surface is completely dried and the substrate is subjected to cathodic electrophoresis. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is controlled at 4.5-6.5.

[0008] S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then using an ultraviolet high-pressure mercury lamp to reheat and cure the surface of the substrate, so that the temperature is controlled at 130-150°C.

[0009] S4. For vacuum coating, first select the cathode two-component electrophoretic paint with bisphenol A medium and high molecular weight epoxy resin as the main film-forming material as the target material, and perform magnetron sputtering coating. After the substrate is loaded into the furnace, the parameters of the furnace are set to make the vacuum environment 3.8×10-4Pa, the argon partial pressure 1.8-2.2Pa, the sputtering power controlled at 65-95W, the current 0.5-1.2A, and the sputtering time controlled at 15-35min.

[0010] S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm. After the substrate is cooled, vacuum coating is performed on the basis of the single-layer coating. The specific coating steps are the same as those described in S4, and the thickness of the secondary coating is maintained at 1-5 μm.

[0011] S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

[0012] As a further solution of the present invention: the pretreatment steps of the substrate are as follows:

[0013] S101, firstly cutting the selected base material to meet the processing specification requirements.

[0014] S102. Next, the substrate is degreased by using an electrolytic aqueous solution, and the substrate is placed in a container and soaked for 3-5 minutes, and aeration and ultrasonic wave are used to efficiently degrease the substrate.

[0015] S103, etching the degreased substrate. First, prepare an etching solution to etch the substrate. The etching time is controlled at 5-8 minutes and the etching temperature is controlled at 70-80°C.

[0016] S104, chemically polishing the etched substrate. Dry the substrate surface before polishing, and control the drying temperature at 70-90° C. Use a polishing liquid to polish the substrate. If the substrate surface is dark yellow during polishing, add nitric acid to remove scratches and burrs on the substrate surface. The polishing time is controlled at 5-8 minutes.

[0017] S105, cleaning the substrate after chemical polishing, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

[0018] As a further solution of the present invention: in S102, the electrolytic aqueous solution is mixed by sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100°C, and the mixing time is controlled at 1-3 minutes, and aeration mixing is performed during the mixing process.

[0019] As a further solution of the present invention: in S103, the etching solution is prepared by mixing nitric acid, hydrofluoric acid and deionized water at 50-60°C, and the mixing time is controlled to be 3-5 minutes.

[0020] As a further solution of the present invention: in S104, the polishing liquid is mixed by an oxidant, a metal complexing agent, a metal corrosion inhibitor and a builder, and is mixed for 3-5 minutes at room temperature.

[0021] As a further solution of the present invention: in S1, before the polishing process, the substrate is immersed in a 100-200 g / L chromic anhydride solution for a time of 10-20 seconds to remove the contact copper on the surface of the substrate.

[0022] As a further solution of the present invention: in S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

[0023] As a further solution of the present invention: the cathode two-component electrophoretic paint is prepared by mixing bisphenol A type medium- and high-molecular-weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether.

[0024] The beneficial effects of the present invention are:

[0025] The present invention controls the parameters in the cathode electrophoresis process so that the bath solution is always within a stable pH range, the film thickness conversion is easy, the paint film quality is effectively guaranteed, and the paint is not easily peeled off or the impact strength of the paint film is reduced. At the same time, during the vacuum coating process, a double-layer coating method is used to protect the substrate, which further protects the substrate and is not easily affected by its own magnetism, so that the process effectively solves the problems of coating bonding strength, cracking, leakage and discoloration, and further improves the coating effect.

[0026] The present invention forms a protective film layer on the surface of the substrate by performing cutting, degreasing, etching, chemical polishing and cleaning steps on the substrate, thereby effectively protecting the outer surface of the substrate, effectively improving the flatness and corrosion resistance of the substrate, and being beneficial to improving the coating effect, avoiding affecting the performance of the substrate during the coating process, playing a role in protecting and coloring the coating, and not easily causing waste of coating materials and volatilization of harmful gases in the organic solvent during the coating process. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0028] A cathode two-component electrophoretic paint coating process comprises the following steps:

[0029] S1. Substrate pretreatment: Pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing, etching, chemical polishing and cleaning of the substrate.

[0030] S2. After the pretreatment of the substrate is completed, its surface is completely dried and the substrate is subjected to cathodic electrophoresis. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is controlled at 4.5-6.5.

[0031] S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then using an ultraviolet high-pressure mercury lamp to reheat and cure the surface of the substrate, so that the temperature is controlled at 130-150°C.

[0032] S4. For vacuum coating, first select the cathode two-component electrophoretic paint with bisphenol A medium and high molecular weight epoxy resin as the main film-forming material as the target material, and perform magnetron sputtering coating. After the substrate is loaded into the furnace, the parameters of the furnace are set to make the vacuum environment 3.8×10-4Pa, the argon partial pressure 1.8-2.2Pa, the sputtering power controlled at 65-95W, the current 0.5-1.2A, and the sputtering time controlled at 15-35min.

[0033] S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm. After the substrate is cooled, vacuum coating is performed on the basis of the single-layer coating. The specific coating steps are the same as those in S4, and the thickness of the secondary coating is maintained at 1-5 μm.

[0034] S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

[0035] The steps for pretreatment of the substrate are as follows:

[0036] S101, firstly cutting the selected base material to meet the processing specification requirements.

[0037] S102. Next, the substrate is degreased by using an electrolytic aqueous solution, and the substrate is placed in a container and soaked for 3-5 minutes, and aeration and ultrasonic wave are used to efficiently degrease the substrate.

[0038] S103, etching the degreased substrate. First, prepare an etching solution to etch the substrate. The etching time is controlled at 5-8 minutes and the etching temperature is controlled at 70-80°C.

[0039] S104, chemically polishing the etched substrate. Dry the substrate surface before polishing, and control the drying temperature at 70-90° C. Use a polishing liquid to polish the substrate. If the substrate surface is dark yellow during polishing, add nitric acid to remove scratches and burrs on the substrate surface. The polishing time is controlled at 5-8 minutes.

[0040] S105, cleaning the substrate after chemical polishing, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

[0041] In S102, the electrolytic aqueous solution is mixed with sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100°C, and the mixing time is controlled at 1-3 minutes, and aeration mixing is performed during the mixing process.

[0042] In S103, the etching solution is mixed with nitric acid, hydrofluoric acid and deionized water at 50-60° C., and the mixing time is controlled at 3-5 minutes.

[0043] In S104, the polishing liquid is mixed with an oxidant, a metal complexing agent, a metal corrosion inhibitor and a builder, and is mixed for 3-5 minutes at room temperature.

[0044] In S1, before the polishing process, the substrate is immersed in a 100-200 g / L chromic anhydride solution, and the immersion time is controlled to be 10-20 seconds to remove the contact copper on the surface of the substrate.

[0045] In S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

[0046] The cathode two-component electrophoretic paint is a mixture of bisphenol A type medium and high molecular weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether. Example

[0047] A cathode two-component electrophoretic paint coating process comprises the following steps:

[0048] S1. Substrate pretreatment: Pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing, etching, chemical polishing and cleaning of the substrate.

[0049] S2. After the pretreatment of the substrate is completed, its surface is completely dried and cathode electrophoresis is performed on the substrate. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is 9.

[0050] S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then using an ultraviolet high-pressure mercury lamp to reheat and cure the surface of the substrate, so that the temperature is controlled at 130-150°C.

[0051] S4. For vacuum coating, first select the cathode two-component electrophoretic paint with bisphenol A medium and high molecular weight epoxy resin as the main film-forming material as the target material, and perform magnetron sputtering coating. After the substrate is loaded into the furnace, the parameters of the furnace are set to make the vacuum environment 3.8×10-4Pa, the argon partial pressure 1.8-2.2Pa, the sputtering power controlled at 65-95W, the current 0.5-1.2A, and the sputtering time controlled at 15-35min.

[0052] S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm. After the substrate is cooled, vacuum coating is performed on the basis of the single-layer coating. The specific coating steps are the same as those in S4, and the thickness of the secondary coating is maintained at 1-5 μm.

[0053] S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

[0054] The steps for pretreatment of the substrate are as follows:

[0055] S101, firstly cutting the selected base material to meet the processing specification requirements.

[0056] S102. Next, the substrate is degreased by using an electrolytic aqueous solution, and the substrate is placed in a container and soaked for 3-5 minutes, and aeration and ultrasonic wave are used to efficiently degrease the substrate.

[0057] S103, etching the degreased substrate. First, prepare an etching solution to etch the substrate. The etching time is controlled at 5-8 minutes and the etching temperature is controlled at 70-80°C.

[0058] S104, chemically polishing the etched substrate. Dry the substrate surface before polishing, and control the drying temperature at 70-90° C. Use a polishing liquid to polish the substrate. If the substrate surface is dark yellow during polishing, add nitric acid to remove scratches and burrs on the substrate surface. The polishing time is controlled at 5-8 minutes.

[0059] S105, cleaning the substrate after chemical polishing, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

[0060] In S102, the electrolytic aqueous solution is mixed with sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100°C, and the mixing time is controlled at 1-3 minutes, and aeration mixing is performed during the mixing process.

[0061] In S103, the etching solution is mixed with nitric acid, hydrofluoric acid and deionized water at 50-60° C., and the mixing time is controlled at 3-5 minutes.

[0062] In S104, the polishing liquid is mixed with an oxidant, a metal complexing agent, a metal corrosion inhibitor and a builder, and is mixed for 3-5 minutes at room temperature.

[0063] In S1, before the polishing process, the substrate is immersed in a 100-200 g / L chromic anhydride solution, and the immersion time is controlled to be 10-20 seconds to remove the contact copper on the surface of the substrate.

[0064] In S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

[0065] The cathode two-component electrophoretic paint is a mixture of bisphenol A type medium and high molecular weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether. Example

[0066] A cathode two-component electrophoretic paint coating process comprises the following steps:

[0067] S1. Substrate pretreatment: Pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing and cleaning of the substrates.

[0068] S2. After the pretreatment of the substrate is completed, its surface is completely dried and cathode electrophoresis is performed on the substrate. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is 4.

[0069] S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then using an ultraviolet high-pressure mercury lamp to reheat and cure the surface of the substrate, so that the temperature is controlled at 130-150°C.

[0070] S4. For vacuum coating, first select the cathode two-component electrophoretic paint with bisphenol A medium and high molecular weight epoxy resin as the main film-forming material as the target material, and perform magnetron sputtering coating. After the substrate is loaded into the furnace, the parameters of the furnace are set to make the vacuum environment 3.8×10-4Pa, the argon partial pressure 1.8-2.2Pa, the sputtering power controlled at 65-95W, the current 0.5-1.2A, and the sputtering time controlled at 15-35min.

[0071] S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm. After the substrate is cooled, vacuum coating is performed on the basis of the single-layer coating. The specific coating steps are the same as those in S4, and the thickness of the secondary coating is maintained at 1-5 μm.

[0072] S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

[0073] The steps for pretreatment of the substrate are as follows:

[0074] S101, firstly cutting the selected base material to meet the processing specification requirements.

[0075] S102. Next, the substrate is degreased by using an electrolytic aqueous solution, and the substrate is placed in a container and soaked for 3-5 minutes, and aeration and ultrasonic wave are used to efficiently degrease the substrate.

[0076] S105, cleaning the substrate, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

[0077] In S102, the electrolytic aqueous solution is mixed with sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100°C, and the mixing time is controlled at 1-3 minutes, and aeration mixing is performed during the mixing process.

[0078] In S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

[0079] The cathode two-component electrophoretic paint is a mixture of bisphenol A type medium and high molecular weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether. Example

[0080] A cathode two-component electrophoretic paint coating process comprises the following steps:

[0081] S1. Substrate pretreatment: Pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing and cleaning of the substrates.

[0082] S2. After the pretreatment of the substrate is completed, its surface is completely dried and cathode electrophoresis is performed on the substrate. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is 9.

[0083] S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then using an ultraviolet high-pressure mercury lamp to reheat and cure the surface of the substrate, so that the temperature is controlled at 130-150°C.

[0084] S4. For vacuum coating, first select the cathode two-component electrophoretic paint with bisphenol A medium and high molecular weight epoxy resin as the main film-forming material as the target material, and perform magnetron sputtering coating. After the substrate is loaded into the furnace, the parameters of the furnace are set to make the vacuum environment 3.8×10-4Pa, the argon partial pressure 1.8-2.2Pa, the sputtering power controlled at 65-95W, the current 0.5-1.2A, and the sputtering time controlled at 15-35min.

[0085] S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm.

[0086] S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

[0087] The steps for pretreatment of the substrate are as follows:

[0088] S101, firstly cutting the selected base material to meet the processing specification requirements.

[0089] S102. Next, the substrate is degreased by using an electrolytic aqueous solution, and the substrate is placed in a container and soaked for 3-5 minutes, and aeration and ultrasonic wave are used to efficiently degrease the substrate.

[0090] S105, cleaning the substrate, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

[0091] In S102, the electrolytic aqueous solution is mixed with sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100°C, and the mixing time is controlled at 1-3 minutes, and aeration mixing is performed during the mixing process.

[0092] In S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

[0093] The cathode two-component electrophoretic paint is a mixture of bisphenol A type medium and high molecular weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether.

[0094] The following table is obtained based on Examples 1-4:

[0095] Whether etching or chemical polishing Number of coating layers pH value of bath solution Film impact strength / kg·cm Example 1 yes 2 6 ≥50 Example 2 yes 2 9 <40 Example 3 no 2 4 <30 Example 4 no 1 9 <25

[0096] From the comparison in the above table, we can see that:

[0097] By adjusting the parameters in the cathode electrophoresis process, the bath liquid is always within a stable pH range, the film thickness can be easily converted, and the quality of the paint film is effectively guaranteed. Paint peeling and reduced impact strength of the paint film are not likely to occur. At the same time, during the vacuum coating process, a double-layer coating method is used to protect the substrate, which further protects the substrate and is not easily affected by its own magnetism. This process effectively solves the problems of coating adhesion, cracking, missing plating and discoloration, and further improves the coating effect.

[0098] By cutting, degreasing, etching, chemically polishing and cleaning the substrate, a protective film layer is formed on the surface of the substrate, which effectively protects the outer surface of the substrate, effectively improves the flatness and corrosion resistance of the substrate, is beneficial to improve the coating effect, avoids affecting the performance of the substrate during the coating process, and plays a role in protecting and coloring the coating.

[0099] Finally, a few points should be explained: Although the present invention has been described in detail above with general descriptions and specific embodiments, on the basis of the present invention, the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit it; although the present invention has been described in detail with reference to the aforementioned embodiments, ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cathode two-component electrophoretic paint coating process, characterized in that: The following steps are involved: S1. Substrate pretreatment: pretreatment is performed according to the surface conditions of different substrates, including cutting, degreasing, etching, chemical polishing and cleaning of the substrate; S2. After the pretreatment of the substrate is completed, its surface is completely dried, and the substrate is subjected to cathode electrophoresis. The solid content of the cathode two-component electrophoretic paint is 10%-15%, and the pH value in the electrophoresis tank is controlled at 4.5-6.5; S3, drying the substrate pretreated in S2 at 80-90°C for 15-25 minutes until the surface of the substrate is free of moisture and completely dry, and then reheating and curing the surface of the substrate using an ultraviolet high-pressure mercury lamp to control the temperature at 130-150°C; S4, vacuum coating, first select bisphenol A type medium and high molecular weight epoxy resin as the main film-forming cathode two-component electrophoretic paint as the target material, and perform magnetron sputtering coating, after the substrate is loaded into the furnace, the furnace parameters are set to make the vacuum environment 3.8×10-4Pa, argon partial pressure 1.8-2.2Pa, sputtering power controlled at 65-95W, current 0.5-1.2A, sputtering time controlled at 15-35min; S5. During the single-layer coating process in S4, the thickness of the magnetron sputtering coating is maintained at 0.05-4.5 μm. After the substrate is cooled, vacuum coating is performed on the basis of the single-layer coating. The specific coating steps are the same as those described in S4. The thickness of the secondary coating is maintained at 1-5 μm. S6. Bake the coated substrate at 110-150°C for 30-40 minutes to completely cure the coating and adhere to the surface of the substrate. After cooling, the cathode two-component electrophoretic paint coating process is completed.

2. A cathode two-component electrophoretic paint coating process according to claim 1, characterized in that: The pretreatment steps of the substrate are as follows: S101, firstly cutting the selected base material to meet the processing specification requirements; S102, degreasing the substrate, using an electrolytic aqueous solution to degreasing the substrate, placing the substrate in a container and soaking it for 3-5 minutes, aerating and ultrasonically removing the oil efficiently; S103, etching the degreased substrate, firstly preparing an etching solution to etch the substrate, the etching time is controlled within 5-8 minutes, and the etching temperature is controlled within 70-80° C.; S104, chemically polishing the etched substrate, drying the substrate surface before polishing, and controlling the drying temperature at 70-90° C., polishing the substrate with a polishing liquid, and if the substrate surface is dark yellow during polishing, adding nitric acid to remove scratches and burrs on the substrate surface, and controlling the polishing time at 5-8 minutes; S105, cleaning the substrate after chemical polishing, placing the substrate in a cleaning tank for ultrasonic cleaning, using flowing pure water, and the conductivity of the pure water is less than 4us / cm, and the cleaning time is controlled within 3-5min.

3. A cathode two-component electrophoretic paint coating process according to claim 2, characterized in that: In S102, the electrolytic aqueous solution is mixed with sodium carbonate, sodium hydroxide solution and paraffin emulsifier at 80-100° C., and the mixing time is controlled at 1-3 minutes. During the mixing process, aeration mixing is performed.

4. A cathode two-component electrophoretic paint coating process according to claim 2, characterized in that: In S103, the etching solution is prepared by mixing nitric acid, hydrofluoric acid and deionized water at 50-60°C, and the mixing time is controlled to be 3-5 minutes.

5. The cathode two-component electrophoretic paint coating process according to claim 2, characterized in that: In S104, the polishing liquid is mixed with an oxidant, a metal complexing agent, a metal corrosion inhibitor and a builder, and is mixed for 3-5 minutes at room temperature.

6. A cathode two-component electrophoretic paint coating process according to claim 1, characterized in that: In S1, before the polishing process, the substrate is immersed in a 100-200 g / L chromic anhydride solution for 10-20 seconds to remove the contact copper on the surface of the substrate.

7. The cathode two-component electrophoretic paint coating process according to claim 1, characterized in that: In S2, the conductivity of the electrophoresis tank solution is controlled at 280-800 us / cm, the temperature of the tank solution is controlled at 23-28° C., the electrophoresis voltage is 35-90 v, and the electrophoresis time is controlled at 20-90 s.

8. The cathode two-component electrophoretic paint coating process according to claim 1, characterized in that: The cathode two-component electrophoretic paint is prepared by mixing bisphenol A type medium- and high-molecular-weight epoxy resin, ethanolamine, isocyanate, acetic acid and alcohol ether.