A smoke exhaust device for a pyrometallurgical furnace and a method for eliminating iron nodules in a flue

By using SiO2, Cu2O, and CuO slag removers in pyrometallurgy to react with Fe3O4 in the flue, the problem of difficult elimination of nodules in the smelting furnace flue is solved, and efficient and safe flue cleaning and continuity of the copper smelting process are achieved. .

CN115046397BActive Publication Date: 2024-10-15LIANGSHAN MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210674368.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-15
Publication Date
2024-10-15
Estimated Expiration
2042-06-15

AI Technical Summary

Technical Problem

Existing methods for eliminating nodules in smelting furnace flues in pyrometallurgy have problems such as difficulty in completely eliminating nodules, low safety, and affected production efficiency.

Method used

SiO2, Cu2O, and CuO are used as slag removal agents. By adding the slag removal agent from the discharge port during the smelting process, it reacts with Fe3O4 in the flue to generate low melting point products, reduce adhesion, and achieve natural shedding.

Benefits of technology

It achieves efficient and safe elimination of flue nodules, ensures the continuity and production efficiency of the copper smelting process, and is simple to operate and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115046397B_ABST
    Figure CN115046397B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of pyrometallurgy. Aiming at the problems of serious nodules in existing pyrometallurgical flues, low efficiency in removing nodules in flues and low safety, a smoke exhaust device for a pyrometallurgical furnace and a method for eliminating iron nodules in flues are disclosed. During the smelting process, a slag remover is added from a discharge port, and the discharge port is located at an end of the iron nodule away from a discharge port of the flue; the slag remover includes one or more of SiO2, Cu2O and CuO; the smoke exhaust device for a pyrometallurgical furnace includes a material conveyor belt, a furnace lining and a flue connected in sequence, a slag remover discharge port is provided on the top of the furnace lining, and the slag remover discharge port is located between the feed port and the discharge port. Powdered SiO2, Cu2O, CuO, etc. are put into the slag remover through the slag remover discharge port. The slag remover enters the flue with the rising flue gas, contacts and reacts with the nodules, and obtains Fe2SiO4, CuFe2O4, CuFe2O4 and other products with loose structure and low adhesion, so that they can fall off naturally from the inner pipe wall of the flue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pyrometallurgy, and in particular to a smoke exhaust device for a pyrometallurgical furnace and a method for eliminating iron nodules in a flue. Background Art

[0002] Pyrometallurgy refers to placing ores or concentrates under high temperature conditions, and after a series of treatments such as roasting and smelting, the raw materials undergo physical and chemical changes, thereby separating the metals from the buried stones or other impurities, and finally obtaining high-purity metal products. Pyrometallurgy is mostly applicable to non-ferrous metals such as lead and copper. It has the characteristics of wide adaptability of raw materials, simple equipment, and high production efficiency. It is a common smelting method in industrial metallurgy. Among them, the use of pyrometallurgy to smelt copper usually requires roasting, smelting, blowing, and pyrometallurgical refining of copper ore to obtain metallic copper. During the smelting process, it can be divided into top-blowing smelting, side-blowing smelting, and bottom-blowing smelting according to the position of the oxygen gun. In addition, due to the influence of factors such as the smelting method and the structure of the furnace, flue nodules often occur in this process, which seriously affects the normal smelting process of the copper ore.

[0003] In response to the above problems, the following methods are commonly used to deal with them: Method 1 is to install an automated mechanical vibrating device in the middle and upper part of the flue, that is, to use the vibrating device to beat the outer wall of the flue at a certain frequency, so that the flue vibrates and causes the nodules to fall off. This method has the problems of insufficient nodule removal and workers are easily burned by the slag that falls off. The second method is to melt it with oil, and use hot oil to make the nodules slide off the flue, but this method will seriously affect the copper smelting production process. The third method is to stop the furnace for cleaning, that is, to stop the work of the furnace regularly, and remove the nodules in the flue by shoveling and other methods before resuming production. Obviously, it will seriously affect the production efficiency, and in the process of removing nodules and cleaning slag, there are safety hazards such as burns by the residual heat of the furnace.

[0004] Therefore, we are in urgent need of a more efficient and safer method for removing nodules from the flue of a pyrometallurgical furnace. Summary of the invention

[0005] The technical problems to be solved by the present invention are:

[0006] In the work of removing nodules from the flue of smelting furnaces in fire metallurgy, the various removal methods currently used all have problems such as nodules being difficult to completely remove, easy to cause burns and scalds, low safety, or serious impact on production efficiency due to nodule removal.

[0007] The technical solution adopted by the present invention is:

[0008] The present invention provides a method for eliminating iron nodules in a flue of a pyrometallurgical furnace. During the smelting process, a slag remover is added from a discharge port, and the discharge port is located at an end of the iron nodule away from the flue discharge port; the slag remover includes one or more of SiO2, Cu2O, and CuO.

[0009] Preferably, the deslagging agent comprises SiO2, Cu2O, and CuO; in terms of weight ratio, SiO2:Cu2O:CuO=1-4:8-11:4-7.

[0010] Preferably, in terms of weight ratio, the input amount of the slag remover: the weight of the iron nodule = 0.16-0.56:1.

[0011] Preferably, the deslagging agent is in powder form, and the particle size of the deslagging agent is 0.1 to 0.2 mm.

[0012] Preferably, the slag remover is added in multiple times, and the time interval between two adjacent additions is 0 to 12 minutes.

[0013] The present invention also provides a smoke exhaust device for a pyrometallurgical furnace as described above, comprising a material conveyor belt, a furnace lining and a flue connected in sequence, a slag remover discharge port being provided on the top of the furnace lining, and the slag remover discharge port being located between the feed port and the discharge port.

[0014] Preferably, a feed opening and a discharge opening are respectively provided on the top of the furnace lining, the feed opening end of the material conveyor belt is arranged close to the feed opening, and the smoke inlet end of the flue is connected to the discharge opening.

[0015] Preferably, the slag removal agent discharge port is connected to a feeding pipe, and the discharge end of the feeding pipe is inclined toward the direction close to the flue.

[0016] Preferably, the flue is arranged in a vertical direction.

[0017] Preferably, the feed end of the feed pipeline is provided with a hopper and a delivery pump.

[0018] The technical mechanism adopted by the present invention is:

[0019] By sampling and analyzing the composition of flue nodules in copper smelting for many times, it was found that the main component was Fe3O4, and the mass of Fe3O4 accounted for more than 50% of the total mass of nodules. After research, it was found that the formation of flue nodules mainly composed of Fe3O4 in copper smelting flues is due to the following reasons: the ore source obtained by mining usually contains not only copper, but also a large amount of iron and a small amount of other metals. The pyrometallurgical process usually adopts a high oxygen content to strengthen the smelting process. In an oxygen-rich environment, the iron element contained in the ore source is inevitably oxidized to Fe3O4, and some of the Fe3O4 that participates in the redox reaction and slag formation will enter the flue with the rising air flow; in addition, due to the excessively high Fe3O4 content in the smelting slag, the slag viscosity is high, and the gas cannot escape in time, causing the melt to splash, which further causes Fe3O4 to adhere and agglomerate in the flue, and finally forms an iron nodule.

[0020] In order to reduce the adhesion between the iron nodule and the inner wall of the flue, it is necessary to modify the main component of the iron nodule, Fe3O4. Based on this, without introducing more impurities, SiO2, Cu2O, and CuO with redox effects are used as slag removers to react with Fe3O4 (the specific reaction process is as follows) to obtain products such as Fe2SiO4, CuFe2O4, and CuFe2O4 with loose structure and low adhesion, so that they can fall off naturally from the inner wall of the flue.

[0021] 2Fe3O4+2C+3SiO2=3Fe2SiO4+2CO

[0022] 6Cu2O+8Fe3O4+5O2=12CuFe2O4

[0023] 6CuO+4Fe3O4+O2=6CuFe2O4

[0024] In addition, in order to make the addition of slag remover simpler and more convenient, we use the large amount of high-temperature rising air flow in the flue itself to make the slag remover into powder or directly use powdered slag remover, and put the slag remover into the lining of the smelting furnace close to the flue, so that it can move into the flue with the rising air flow and fully contact and react with the flue nodules.

[0025] The beneficial effects of the present invention are as follows:

[0026] (1) A slag remover discharge port is arranged on the top of the furnace lining. After the powdered slag remover is put into the furnace lining, the slag remover enters the flue with the rising flue gas and contacts the flue nodules. It reacts with Fe3O4, the main substance in the flue nodules, and converts the high-melting-point Fe3O4 into low-melting-point substances such as CuFe2O4 and Fe2SiO4, thereby reducing the viscosity of the flue nodules and making the contact surface between the flue and the flue loose and easy to fall off. The nodules can fall off naturally under the action of gravity.

[0027] (2) The slag remover is added separately from the slag remover discharge port and rises into the flue with the rising flue gas, that is, the metal smelting is not affected during the removal process, and continuous and uninterrupted copper smelting can be ensured.

[0028] (3) The method for removing iron nodules in the flue of the present invention is simple to operate, and the slag remover can be directly made from raw and auxiliary materials in the pyrometallurgical production process, and the removal cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a structural schematic diagram of the flue of the pyrometallurgical furnace in Example 1;

[0030] Figure symbols: 1- material conveyor belt, 2- material discharge port, 3- slag removal agent discharge port, 4- flue, 5- nodule, 6- furnace lining. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] First, the present invention provides a method for eliminating iron nodules in the flue of a pyrometallurgical furnace. During the smelting process, a slag remover is added from a discharge port, and the discharge port is located at one end of the iron nodule away from the flue discharge port; the slag remover includes one or more of SiO2, Cu2O, and CuO.

[0033] In the present invention, the weight ratio of the deslagging agent is 0.16-0.56:1 for the weight of the iron nodule. The deslagging agent is in powder form, and the particle size of the deslagging agent is 0.1-0.2 mm. The deslagging agent is added in multiple times, and the time interval between each two adjacent additions is 0-12 minutes.

[0034] In the present invention, the flue nodules in copper smelting are sampled multiple times and the composition analysis and other studies are conducted. The study found that: the ore source used for copper smelting usually contains other metal impurities such as iron. In the process of pyrometallurgy, a large amount of oxygen needs to be introduced. In an oxygen-rich environment, part of the oxygen reacts with iron at high temperature to generate a large amount of Fe3O4. Due to the strong adhesion of Fe3O4, it is very easy to adhere to metal pipes such as iron, so that after entering the flue with the rising airflow, it adheres to the inner wall of the flue. By introducing a slag remover, it is combined with Fe3O4 and reacted to obtain products such as Fe2SiO4, CuFe2O4, CuFe2O4, etc. with loose structure and strong adhesion, so that it can fall off naturally from the inner wall of the flue.

[0035] Second, the present invention provides a smoke exhaust device for a pyrometallurgical furnace as described above, comprising a material conveyor belt 1, a furnace lining 6 and a flue 4 connected in sequence, a feed port 2 and a discharge port are respectively provided on the top of the furnace lining 6, the feed end of the material conveyor belt 1 is arranged close to the feed port 2, and the smoke inlet end of the flue 4 is connected to the discharge port; a slag remover discharge port 3 is also provided on the top of the furnace lining 6, and the slag remover discharge port 3 is located between the feed port 2 and the discharge port.

[0036] In the present invention, the slag remover discharge port 3 is connected to a feeding pipe, and the discharge end of the feeding pipe is inclined toward the flue 4, so that the slag remover can move to the nodules 5 with the rising airflow in the flue 4 and react, so that the nodules 5 fall off the inner wall of the flue 4; the flue 4 is arranged in a vertical direction. The feed end of the feeding pipe is equipped with a hopper and a delivery pump for feeding the slag remover into the furnace lining 6.

[0037] In the present invention, the deslagging agent is put into the hopper, and then the delivery pump is started. After the powdered deslagging agent is put into the furnace lining 6, the deslagging agent enters the flue 4 with the rising flue gas and contacts the nodules 5 of the flue 4, and reacts with the main substances Fe3O4 and the like in the nodules 5 of the flue 4, converting the high melting point Fe3O4 into low melting point substances such as CuFe2O4 and Fe2SiO4, reducing the viscosity of the nodules 5 of the flue 4, making the contact surface of the nodules 5 with the flue 4 loose and easy to fall off, and can fall off naturally under the action of gravity and the like.

[0038] <Example>

[0039] Example 1

[0040] The present embodiment provides a method for removing iron nodules in the flue of a pyrometallurgical furnace. During the smelting process, a slag remover is added from a discharge port, and the discharge port is located at the end of the iron nodule away from the flue discharge port. In terms of weight ratio, the slag remover is a mixed powder including SiO2, Cu2O, and CuO.

[0041] In this embodiment, by weight ratio, SiO2:Cu2O:CuO=1:10:6, the amount of slag remover added: the weight of the iron nodule = 0.3:1; the slag remover is in powder form, and the particle size of the slag remover is 0.15 mm; the slag remover is added in multiple times, and the time interval between each two adjacent additions is 8 minutes.

[0042] like Figure 1 As shown, the present embodiment also provides a smoke exhaust device for a pyrometallurgical furnace as described above, comprising a material conveyor belt 1, a furnace lining 6 and a flue 4 connected in sequence, a feed port 2 and a discharge port are respectively provided on the top of the furnace lining 6, the feed end of the material conveyor belt 1 is arranged close to the feed port 2, and the smoke inlet end of the flue 4 is connected to the discharge port; a slag remover discharge port 3 is also provided on the top of the furnace lining 6, and the slag remover discharge port 3 is located between the feed port 2 and the discharge port.

[0043] In this embodiment, the slag remover discharge port 3 is connected to a feeding pipe, and the discharge end of the feeding pipe is inclined toward the flue 4, so that the slag remover can move to the nodules 5 with the rising airflow in the flue and react, so that the nodules 5 fall off the inner wall of the flue 4; the flue 4 is arranged in a vertical direction. The feeding end of the feeding pipe is equipped with a hopper and a delivery pump for feeding the slag remover into the furnace lining.

[0044] In this embodiment, the above-mentioned smoke exhaust device for pyrometallurgical furnace and the method for eliminating iron nodules in the flue of the above-mentioned pyrometallurgical furnace are used to produce 80,000 tons of copper annually, and the amount of copper smelting raw materials put into the smelting furnace is 65t / h: after the furnace is opened and operated for one week, obvious nodules appear at the entrance of the flue. After repeated sampling and analysis, it is found that its main phases include Fe3O4, etc., which causes the flue to be blocked, the flue gas flow is not smooth, the system exhaust is affected, and the production is seriously affected. After that, the slag remover powder is added at a rate of 20kg / h. From the beginning of adding the slag remover, a large number of nodules began to fall off in the furnace, and the nodule removal effect in the flue was significant and efficient.

[0045] Example 2

[0046] The difference between this embodiment and embodiment 1 is that the slag remover is a mixed powder including SiO2 and Cu2O. The annual output of copper is 100,000 tons, and the amount of copper smelting raw materials put into the smelting furnace is 95t / h: after running for a period of time, the nodules at the flue entrance grow rapidly. After sampling and analysis, it is found that the nodule components are mainly Fe3O4, which causes most of the flue to be blocked. When obvious nodules appear at the flue mouth, 6kg of mixed powder with a weight ratio of SiO2:Cu2O=1.2:1 is added every 10 minutes while feeding. After the mixed powder is added, nodules begin to fall off frequently in the furnace, and the flue nodules are basically dropped within a week.

[0047] Example 3

[0048] The difference between this embodiment and embodiment 1 is that the slag remover is SiO2 powder. The annual output of copper is 80,000 tons, and the amount of copper smelting raw materials put into the smelting furnace is 65t / h: after the furnace was opened and operated for one week, obvious nodules appeared at the flue entrance. After repeated sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which brought serious impact on production. After that, SiO2 powder was added at a rate of 20kg / h. From the beginning of adding SiO2 powder, nodules began to fall off frequently in the furnace, and the nodule removal effect in the flue was significant.

[0049] Example 4

[0050] The difference between this embodiment and embodiment 1 is that the slag remover is Cu2O powder. The annual copper production is 100,000 tons, and the amount of copper smelting raw materials put into the smelting furnace is 95t / h. When obvious nodules appear at the flue outlet, Cu2O powder is added continuously in batches while feeding, and the addition rate of Cu2O powder is 30kg / h. From the beginning of adding Cu2O powder, nodules begin to fall off frequently in the furnace, and the flue nodules are basically removed within a week.

[0051] Example 5

[0052] The difference between this embodiment and embodiment 1 is that the amount of slag remover added is: the weight of the iron nodule

[0053] =0.16:1. The annual output of copper is 80,000 tons, and the amount of copper raw materials put into the smelting furnace is 65t / h: After the furnace was opened and operated for a week, obvious nodules appeared at the flue entrance. After multiple sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which had a serious impact on production. After that, slag remover powder was added at a rate of 20kg / h. From the beginning of adding slag remover powder, nodules began to fall off frequently in the furnace, and the nodule removal effect in the flue was obvious.

[0054] Example 6

[0055] The difference between this embodiment and embodiment 1 is that the amount of slag remover input: the weight of the iron nodule = 0.56:1. The annual output of copper is 100,000 tons, and the amount of copper smelting raw materials input into the smelting furnace is 65t / h: after the furnace was opened and operated for a week, obvious nodules appeared at the flue entrance. After multiple sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which brought serious impact on production. After that, slag remover powder was added at a rate of 20kg / h. Since the addition of the slag remover powder, nodules began to fall off frequently in the furnace, and the nodule removal effect in the flue was obvious.

[0056] <Comparative Example>

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is that the amount of slag remover input: the weight of the iron nodule = 0.1:1. The annual output of copper is 80,000 tons, and the amount of copper smelting raw materials input into the smelting furnace is 65t / h: after the furnace was opened and operated for a week, obvious nodules appeared at the flue entrance. After repeated sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which brought serious impact on production. After that, slag remover powder was added at a rate of 20kg / h. After a period of time after the slag remover powder was added, nodules began to fall off frequently in the furnace, and the nodules in the flue were basically removed.

[0059] Comparative Example 2

[0060] The difference between this comparative example and Example 1 is that the amount of slag remover input: the weight of the iron nodule = 1:1. The annual output of copper is 100,000 tons, and the amount of copper smelting raw materials input into the smelting furnace is 65t / h: after the furnace was opened and operated for a week, obvious nodules appeared at the flue entrance. After multiple sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which brought serious impact on production. After that, slag remover powder was added at a rate of 20kg / h. From the beginning of adding the slag remover powder, nodules began to fall off frequently in the furnace, but after a period of time, the nodule shedding speed slowed down, and a small amount of nodules still remained.

[0061] Comparative Example 3

[0062] The difference between this comparative example and Example 1 is that the slag remover is added in multiple times, and the time interval between each two adjacent additions is 15 minutes. The annual output of copper is 80,000 tons, and the amount of copper smelting raw materials put into the smelting furnace is 65t / h: after the furnace was opened and operated for one week, obvious nodules appeared at the flue entrance. After multiple sampling and analysis, it was found that its main phases included Fe3O4, etc., which caused the flue to be blocked, the flue gas flow was not smooth, and the system exhaust was affected, which brought serious impact on production. After that, slag remover powder was added at a rate of 20kg / h. From the beginning of adding the slag remover powder, nodules began to fall off frequently in the furnace, but after the smelting furnace was operated for two weeks, a small amount of nodules still existed in the flue.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for eliminating iron nodules in a pyrometallurgical furnace flue, characterized in that: During the smelting process, the slag remover is added from the slag remover discharge port, and the slag remover is added in multiple times, and the time interval between each two adjacent additions is 0-12 minutes. The slag remover discharge port is located at one end of the iron tumor away from the discharge port of the flue; In terms of weight ratio, the deslagging agent includes SiO2:Cu2O:CuO=1~4:8~11:4~7, and the input amount of the deslagging agent: the weight of the iron nodule=0.16~0.56:

1.

2. The method for eliminating iron nodules in the flue of a pyrometallurgical furnace according to claim 1, characterized in that: The deslagging agent is in powder form, and the particle size of the deslagging agent is 0.1-0.2 mm.

3. A smoke exhaust device for a pyrometallurgical furnace involving the method for eliminating iron nodules in a flue of a pyrometallurgical furnace according to claim 1 or 2, characterized in that: The invention comprises a material conveyor belt (1), a furnace lining (6) and a flue (4) which are connected in sequence, a slag remover discharge port (3) is provided at the top of the furnace lining (6), a feed opening (2) and a discharge port are respectively provided at the top of the furnace lining (6), and the slag remover discharge port (3) is located between the feed opening (2) and the discharge port.

4. The smoke exhaust device for a pyrometallurgical furnace according to claim 3, characterized in that: The unloading end of the material conveyor belt (1) is arranged close to the unloading port (2), and the smoke inlet end of the flue (4) is connected to the discharge port of the furnace lining (6).

5. The smoke exhaust device for a pyrometallurgical furnace according to claim 3, characterized in that: The slag removal agent discharge port (3) is connected to a feeding pipeline, and the discharge end of the feeding pipeline is inclined in a direction close to the flue (4).

6. The smoke exhaust device for a pyrometallurgical furnace according to claim 3, characterized in that: The flue (4) is arranged in a vertical direction.

7. The smoke exhaust device for a pyrometallurgical furnace according to claim 5, characterized in that: The feed end of the feed pipeline is provided with a hopper and a delivery pump.

Citation Information

Patent Citations

  • Technique for continuously smelting copper by employing oxygen bottom converter and device thereof

    CN101165196A

  • Colored metallurgical industrial furnace decoking technology method

    CN101769688A

  • Method for producing white matte by mixed smelting of scrap copper and copper concentrate

    CN101845555A

  • Modifier for clinker from oriented-silicon-steel heating furnace

    CN103343173A

  • Method for controlling slag buildup of transition section of copper smelting waste heat boiler flue