A method for controlling uniform cooling of hot-rolled high-strength steel along the wall thickness direction
During the rolling process of hot-rolled high-strength steel, the ultra-fast cooling system is used to dynamically adjust the water pressure and water ratio, and the problem of uneven cooling in the thickness direction of thick-walled high-strength steel is solved, and the uniformity of structure and performance is achieved, reducing the Cost and improve welding properties.
Patent Information
- Application Number
- CN202210661819.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-06-13
AI Technical Summary
The uneven cooling of thick-walled high-strength steel in the thickness direction leads to uneven structure and performance. The existing technology has high cost and poor welding properties, which cannot effectively solve the problem of cooling uniformity in the thick-walled direction.
During the rolling process of hot-rolled high-strength steel, the ultra-fast cooling system is used to perform strong cooling, dynamically adjust the water pressure and the water ratio, and segmentally adjust it according to the surface temperature and air temperature of the strip steel to ensure the uniformity of the cooling process. In the finishing process, seven-frame finishing mill and high-pressure side spraying device are used to improve cooling efficiency.
The tissue uniformity in the thickness direction is achieved, the temperature difference between the surface and the core is less than 50℃, and the cooling speed is uniform. The steel plates produced have all slat bainite tissues, the grain size difference is ≤1.0, and the surface and the core are The hardness difference of the part is ≤0.5μm, and there is no need for hardenable alloy elements, which makes the process simple and low cost.
Smart Images

Figure CN115069770B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel, and in particular to a method for controlling uniform cooling of hot-rolled high-strength steel along a wall thickness direction. Background Art
[0002] Hot-rolled high-strength steel is widely used in various fields of national economic construction, which not only improves the safety of engineering service, but also greatly extends the service life of the project, bringing significant economic benefits. Thick-gauge hot-rolled high-strength steel usually needs to be strongly cooled by the post-rolling cooling system to reach the critical point of medium and low temperature structure transformation in order to obtain the corresponding structure and performance. However, excessive cooling intensity will cause excessive differences in cooling rate along the wall thickness direction, resulting in ultra-fine structure near the surface of the steel plate and even martensitic transformation, which makes the surface hardness of the steel plate exceed the standard, and problems such as bending and cracking will occur during subsequent use. At the same time, the cooling intensity cannot be too small, otherwise the core of the thick-walled steel plate will not be able to achieve the target structure morphology due to insufficient cooling rate, resulting in the performance of the steel plate not meeting the needs of the project.
[0003] At present, in order to improve the cooling uniformity of thick-walled high-strength steel, a large amount of hardenable alloy elements such as Mo, Cr, and B are generally added to the composition system to improve the hardenability and reduce the cooling rate difference in the wall thickness direction by using low cooling rate, so as to achieve uniform cooling and obtain uniformity of the entire cross-section structure. However, this method has problems such as high cost, poor weldability, and weak market competitiveness. Therefore, it is urgent to develop a new post-rolling cooling process to solve the problems of uneven organization and performance caused by uneven cooling in the thickness direction of thick-walled high-strength steel.
[0004] The search found that Chinese invention patent CN202011171959 discloses a method for improving the cooling uniformity of TMCP steel plates, which is aimed at steel plates with a length of 45-52m and a thickness of less than 20mm. By limiting the roller speed, the grouping and interval of the water cooling zone, the shape of the nozzle on the lower surface, etc., it effectively solves the problem of cooling uniformity of TMCP type ultra-long thin steel plates in the length direction, and does not involve or solve the problem of uniform cooling in the wall thickness direction of the steel plate. Chinese invention patent CN202010034406 discloses a control system and method for ultra-fast cooling of medium and thick plates after rolling, and a method for adjusting the water flow ratio compensation value. The system includes multiple groups of cooling water headers and ultra-fast cooling control terminals. The ultra-fast cooling control terminal is configured to input a water flow ratio compensation value, which can superimpose the water flow ratio compensation value on the water flow ratio preset in the cooling model corresponding to the steel plate after the cooling of a steel plate is completed, and can control the water spray volume of multiple groups of cooling water headers according to the superimposed water flow ratio, thereby realizing real-time intervention in the water flow ratio parameters of the ultra-fast cooling control system during the operation of the ultra-fast cooling system.
[0005] For high-strength steel coiled at low temperature in thick-gauge hot rolling production lines, there are few research reports on the control process of cooling uniformity in the thickness direction. For this reason, the inventors have developed a new control process to improve the cooling uniformity of high-strength steel coiled at medium and low temperatures in thick-walled production lines. Summary of the invention
[0006] The purpose of the present invention is to solve the problem of uneven organization and performance of existing hot-rolled thick-walled high-strength steel caused by uneven cooling in the thickness direction, and to provide a method for controlling uniform cooling of hot-rolled high-strength steel along the wall thickness direction. The method comprises the following steps: continuously casting billets are heated and rolled to obtain strip steel, and the strip steel enters an ultra-fast cooling system for strong cooling. During this period, the water pressure and upper and lower water ratio of the ultra-fast cooling system are segmented and dynamically adjusted according to the surface temperature of the strip steel.
[0007] Furthermore, the rolling includes rough rolling and finish rolling, and the rough rolling is performed first and then the finish rolling.
[0008] Furthermore, the thickness of the intermediate billet obtained by rough rolling is 50-58 mm, and the thickness of the strip steel obtained by finish rolling is ≥18 mm.
[0009] Furthermore, in the finishing rolling process, the strip threading speed and acceleration are strictly controlled according to the weather temperature (i.e. air temperature): when the weather temperature T 气 ≤20℃, belt threading acceleration a: 0.003-0.005m / s 2 , belt threading speed: 1.65-1.80m / s; when the weather temperature is T 气 >20℃, belt threading acceleration a: 0.001-0.003m / s 2 , threading speed: 1.35-1.65m / s.
[0010] Furthermore, the finishing rolling equipment is specifically a seven-stand finishing rolling mill, and the purge water between the stands during the finishing rolling is all turned on.
[0011] Furthermore, in the strong cooling process, the water pressure and upper and lower water ratio of the ultra-fast cooling system are adjusted as follows: when the water temperature T 水 When the temperature is less than 25℃, the water pressure of the ultra-fast cooling system is set to 0.20-0.25MPa, and the upper and lower water ratio is set to 1:1.10-1.20; when 25≤T 水 When the temperature is less than 35℃, the water pressure of the ultra-fast cooling system is set to 0.25-0.30MPa, and the upper and lower water ratio is set to 1:1.25-1.35; when the water temperature is T 水 When the temperature is ≥35℃, the water pressure of the ultra-fast cooling system is set to 0.30-0.35MPa, and the upper and lower water ratio is set to 1:1.35-1.45. The water temperature specifically refers to the temperature of the upper and lower cooling water.
[0012] Furthermore, after the strong cooling process has been running for a period of time, when the strip surface temperature T 带钢When the temperature drops to 500℃ or below, the water pressure and upper and lower water ratio of the ultra-fast cooling system are dynamically adjusted. The specific adjustment method is as follows: When 450<T 带钢 When the temperature is ≤500℃, the water volume on the upper surface is reduced to 75% of the set water volume, and the water volume on the lower surface remains unchanged (the water pressure remains unchanged, the same below); when 400℃≤T 带钢 When the temperature is ≤450℃, the water volume on the upper surface is reduced to 50% of the set water volume, and the water volume on the lower surface remains unchanged; when T 带钢 When the temperature is less than 400℃, the water volume on the upper surface is reduced to 25% of the set water volume, and the water volume on the lower surface remains unchanged until the steel core temperature drops to the target temperature (≤500℃), then the upper and lower water of the ultra-fast cooling system are closed at the same time, and the strip is rolled into a coil.
[0013] Furthermore, the ultra-fast cooling system is composed of 4 headers in a group, with a total of 18 groups. Each group of header inlet and outlet is equipped with a group of high-pressure side spray devices with a side spray pressure of 40 bar, thereby ensuring that the cooling water of each group can only slide away from the nozzle gap on the upper surface of the hot-rolled strip without entering the adjacent cooling area.
[0014] The present invention adjusts the strip threading speed, acceleration and water opening state between racks according to the air temperature in the finishing rolling process. The main purpose is to improve the uniformity of the surface temperature of the strip before entering the water, and remove the iron oxide scale on its surface to prevent the residual iron oxide scale from affecting the uniformity of water cooling heat exchange. When the air temperature does not exceed 20°C, the radiation and convection heat exchange efficiency is high. At this time, the strip threading speed and acceleration need to be increased to reduce the temperature drop rate of the strip surface; when the weather temperature is higher than 20°C, a lower strip threading speed and acceleration can be used to ensure the temperature uniformity of the full-length finishing rolling exit of the strip.
[0015] The present invention sets the water pressure and water ratio of the ultra-fast cooling system according to the water temperature, the heat exchange capacity of the strip surface, and the water flow state of the upper and lower surfaces of the strip in the cooling process. When the water temperature is low, the heat exchange capacity is strong, the difference caused by the cooling water on the upper and lower surfaces of the strip is reduced, and the water ratio can be appropriately reduced; when the water temperature is high, the heat exchange capacity decreases, and the water ratio of the upper and lower surfaces of the strip should be appropriately increased, so as to ensure the uniformity of cooling of the upper and lower surfaces of the strip.
[0016] The setting of the water pressure in the cooling process of the present invention is also correlated to a certain extent with the temperature of the cooling water. When the water temperature is low, excessive water pressure will cause excessive bursting of bubbles on the surface of the strip, resulting in a violent exchange of heat between the water and the surface of the strip, which can easily lead to overcooling of the strip surface and insufficient heat conduction efficiency in the core, resulting in a huge difference in cooling capacity between the surface and the core, leading to the formation of a high cooling rate and low temperature transformation martensitic structure on the surface of the strip, while the core has insufficient cooling rate to form a quasi-polygonal ferrite structure. Therefore, setting the water pressure and water ratio for ultra-fast cooling according to different water temperatures is an effective means to ensure the uniformity of the thickness section structure of thick-gauge low-temperature high-strength steel.
[0017] The limiting function of the side spray arrangement and pressure of the cooling process of the present invention is to ensure that the water flow jetted to the steel plate surface for heat exchange is discharged after heat exchange according to the designed process, thereby preventing the water flows in different cooling sections from interfering with each other and causing the cooling process to be uncontrolled.
[0018] When the strip temperature is lower than 500°C, the principle and function of dynamically adjusting the upper and lower water ratio of the ultra-fast cooling system are as follows: When the strip temperature is below 500°C, the cooling enters the Leidenfrost Phenomenon. At this time, a stable boiling film cannot be formed on the strip surface, causing the droplets to flow disorderly on the strip surface, while the cooling water on the lower surface falls directly, resulting in the cooling capacity of the upper surface being significantly higher than that of the lower surface. In order to reduce the difference in heat exchange characteristics between the upper and lower surfaces, the present invention designs an upper and lower dynamic water volume increase and decrease adjustment mode in different temperature ranges.
[0019] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in the following aspects: 1) The final product has excellent performance, uniform structure in the thickness direction and is all lath bainite structure, the grain size difference is ≤1.0, the average diameter difference between the surface and the core bainite bundle is ≤0.5μm, and the thickness section hardness range HV10≤20; 2) The temperature range between the surface and the core of the product during cooling is ≤50℃, the cooling rate range is ≤10℃ / s, and the cooling in the thickness direction is more uniform and controllable; 3) There is no external hardenability alloy element, and the composition of the hot-rolled thick-walled high-strength steel is not changed. The process is simple and easy to implement, with low cost and good effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the surface metallographic structure diagram of the 22mm X80 product prepared by the present invention;
[0021] Figure 2 This is the metallographic structure diagram at 1 / 4 thickness of the 22mm X80 product prepared by the present invention;
[0022] Figure 3 The metallographic structure diagram at 1 / 2 thickness of the 22 mm X80 product prepared by the present invention. DETAILED DESCRIPTION
[0023] In order to enable ordinary technicians in the field to fully understand the technical solutions and beneficial effects of the present invention, further description is given below in conjunction with specific embodiments and drawings.
[0024] 1) The continuous casting slab is heated and then rough rolled. The thickness of the intermediate slab obtained by the rough rolling is 50-58 mm.
[0025] 2) The intermediate billet is transported to the seven-stand finishing mill for finishing rolling. 气 When the temperature is ≤20℃, the belt threading acceleration a is controlled to be 0.003-0.005m / s2 , the threading speed is 1.65-1.80m / s; when the weather temperature is T 气 When the temperature is above 20℃, the threading acceleration a is controlled to be 0.001-0.003m / s 2 The strip threading speed is 1.35-1.65m / s. The purge water between the rolling stands is fully turned on, and the thickness of the finished rolling outlet strip is ≥18mm.
[0026] 3) After finishing rolling, the obtained strip is immediately transported to the ultra-fast cooling system for strong cooling. The water pressure and upper and lower water ratio are set according to the water temperature: when the water temperature T 水 When the temperature is less than 25℃, the water pressure of the ultra-fast cooling system is set to 0.20-0.25MPa, and the upper and lower water ratio is set to 1:1.10-1.20; when the water temperature is 25≤T 水 When the temperature is less than 35℃, the water pressure of the ultra-fast cooling system is set to 0.25-0.30MPa, and the upper and lower water ratio is set to 1:1.25-1.35; when the water temperature is T 水 When the temperature is ≥35℃, the water pressure of the ultra-fast cooling system is set to 0.30-0.35MPa, and the upper and lower water ratio is set to 1:1.35-1.45.
[0027] During this period, the real-time temperature of the strip is calculated based on the incoming material temperature, cooling water temperature, strip travel speed, water pressure, etc. When the strip surface temperature T 带钢 When the temperature is less than 500℃, the upper and lower water ratios are adjusted dynamically. The specific operation is as follows: T 带钢 At 500-450℃, the water volume on the upper surface is reduced to 75% of the set water volume, and the water volume on the lower surface remains unchanged; T 带钢 At 450-400℃, the water volume on the upper surface is reduced to 50% of the set water volume, and the water volume on the lower surface remains unchanged; T 带钢 When the temperature is below 400℃, the water volume on the upper surface is reduced to 25% of the set water volume, and the water volume on the lower surface remains unchanged until the system calculates that the core temperature of the strip has reached the target temperature, and then the upper and lower water ratios are closed at the same time.
[0028] 4) Use a high-strength coiler to coil the steel to obtain a finished steel coil.
[0029] Referring to the above method, a series of experiments were carried out under different conditions, as shown in Table 1-2 below.
[0030] Table 1 Comparison table of process parameters of finishing rolling process of Examples 1-10
[0031]
[0032] Table 2 Comparison table of process parameters of cooling process in Examples 1-10
[0033]
[0034] The strip steel products obtained in Examples 1-10 were analyzed and tested, and the results are as follows: Figure 1-3 As shown in Table 3.
[0035] Table 3 Performance comparison table of strip steel products of Examples 1-10
[0036]
[0037] Depend on Figure 1-3 As can be seen from Table 3, the strip steel products obtained in Examples 1-10 have uniform structure along the thickness direction, and the metallographic structure types at the surface, 1 / 4 thickness, and 1 / 2 thickness are all lath bainite, the surface structure grain size is between 12-13 (gradient value ≤1), and the thickness section hardness extreme difference HV10≤20.
[0038] The above results show that the present invention controls the surface temperature uniformity of the strip before entering the cooling zone and the formation of secondary iron oxide scale on the surface, adopts ultra-fast cooling equipment in the cooling area, sets the water pressure and water ratio according to different water temperatures, and proposes a dynamic water ratio adjustment function to address the uneven cooling problem caused by the Leibniz effect when cooling below 500°C. Ultimately, a combination of measures is taken to achieve the effect of uniform cooling of thick-gauge hot-rolled high-strength steel in the wall thickness direction.
Claims
1. A method for controlling uniform cooling of hot-rolled high-strength steel along the wall thickness direction, characterized in that: The method comprises the following steps: the continuous casting billet is heated and rolled to obtain a strip steel, the strip steel enters an ultra-fast cooling system for strong cooling, during which the water pressure and upper and lower water ratio of the ultra-fast cooling system are adjusted segmentally and dynamically according to the surface temperature of the strip steel, as follows: when the water temperature T 水 When the temperature is less than 25℃, the water pressure of the ultra-fast cooling system is set to 0.20-0.25MPa, and the upper and lower water ratio is set to 1:1.10-1.20; when 25≤T 水 When the temperature is less than 35℃, the water pressure of the ultra-fast cooling system is set to 0.25-0.30MPa, and the upper and lower water ratio is set to 1:1.25-1.35; when T 水 ≥35℃, the water pressure of the ultra-fast cooling system is set to 0.30-0.35MPa, and the upper and lower water ratio is set to 1:1.35-1.45; after a period of strong cooling, when the strip surface temperature T 带钢 When the temperature drops to 500℃ or below, the water pressure and upper and lower water ratio of the ultra-fast cooling system are dynamically adjusted in the following manner: When 450<T 带钢 When the temperature is ≤500℃, the water volume on the upper surface is reduced to 75% of the set water volume, and the water volume on the lower surface remains unchanged; when 400℃≤T 带钢 When the temperature is ≤450℃, the water volume on the upper surface is reduced to 50% of the set water volume, and the water volume on the lower surface remains unchanged; when T 带钢 When the temperature is less than 400℃, the water volume on the upper surface is reduced to 25% of the set water volume, and the water volume on the lower surface remains unchanged until the steel core temperature drops to the target temperature, the upper and lower water of the ultra-fast cooling system are closed at the same time, and the strip is rolled into a coil.
2. The method according to claim 1, characterized in that: The rolling includes rough rolling and finish rolling, and the rough rolling is performed first and then the finish rolling.
3. The method according to claim 2, characterized in that: The thickness of the intermediate billet obtained by rough rolling is 50-58mm, and the thickness of the strip obtained by finish rolling is ≥18mm.
4. The method according to claim 2, characterized in that: In the finishing process, the threading speed and acceleration are strictly controlled according to the weather temperature: when the weather temperature T 气 When the temperature is ≤20℃, the belt threading acceleration is 0.003-0.005m / s 2 , belt threading speed 1.65-1.80m / s; when the weather temperature T 气 >20℃, belt threading acceleration 0.001-0.003m / s 2 , threading speed 1.35-1.65m / s.
5. The method according to claim 2, characterized in that: The finishing rolling equipment is specifically a seven-stand finishing rolling mill, and the purge water between the stands during the finishing rolling mill is all turned on.
6. The method according to claim 1, characterized in that: The ultra-fast cooling system is composed of 4 headers in a group, and each group of header inlet and outlet is equipped with a group of high-pressure side spray devices with a side spray pressure of 40 bar. The cooling water of each group can only slide away from the nozzle gap on the upper surface of the hot-rolled strip and cannot enter the adjacent cooling area.
7. A hot-rolled high-strength steel, characterized in that: The hot-rolled high-strength steel is prepared according to any one of the methods of claims 1-6.
Citation Information
Patent Citations
Ultrafast cooling control system and method for medium plate after rolling and method for adjusting water flow ratio compensation value
CN111229840A
Method for improving cooling uniformity of TMCP steel plate
CN112387789A
Refrigerating device of belt steel and cooling and controlling method thereof
CN101381806A
Control method for improving precision of ultra-fast cooling temperature model and self-learning efficiency
CN105032951A
Method for improving temperature control accuracy of thick-specification band steel subjected to ultra fast cooling
CN105689407A