A sulfide-coated magnesium ion storage positive electrode material, preparation method and application in magnesium metal secondary battery

By coating the surface of the olivine-type magnesium storage cathode material with a two-dimensional layered sulfide layer, the problem of slow electrochemical reaction kinetics in magnesium metal secondary batteries is solved, efficient charge transfer and cycle stability are achieved, and the battery life is improved. Magnesium ion storage capacity and battery performance.

CN115117314BActive Publication Date: 2024-10-29QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210781307.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-04
Publication Date
2024-10-29
Estimated Expiration
2042-07-04

AI Technical Summary

Technical Problem

Olivine-type magnesium storage cathode materials have the problem of slow electrochemical reaction kinetics in magnesium metal secondary batteries. Especially in ether magnesium electrolyte systems, the desolvation process at the interface is difficult, resulting in a slow charge transfer rate. The ability to deintercalate magnesium ions cannot be fully exerted.

Method used

Using a sulfide-coated magnesium ion storage cathode material, a two-dimensional layered transition metal sulfide layer, such as molybdenum disulfide or vanadium disulfide, is coated on the surface of the olivine-type cathode material to form a 2-20nm thick coating layer , improve the interface desolvation speed and structural stability.

Benefits of technology

Significantly accelerates the desolvation process of magnesium ions, improves the electrochemical performance and cycle stability of the cathode material, the first discharge specific capacity reaches 140mAh/g, the capacity retention rate reaches 85.7% after 100 cycles, and reduces the corrosion of the electrode by the electrolyte .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115117314B_ABST
    Figure CN115117314B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of magnesium metal secondary batteries, and in particular, relates to a sulfide-coated magnesium ion positive electrode material, a preparation method, and an application in a magnesium metal secondary battery. The positive electrode material is a magnesium ion positive electrode material with a sulfide coated on the surface, wherein the magnesium ion storage positive electrode material is an olivine type electrode material. The method provided by the present invention not only significantly improves the magnesium ion storage capacity of the magnesium storage positive electrode material, but also effectively improves the positive electrode cycle performance, and has the advantages of good repeatability and strong versatility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of magnesium metal secondary batteries, and in particular relates to a sulfide-coated magnesium ion storage positive electrode material, a preparation method thereof, and an application thereof in magnesium metal secondary batteries. Background Art

[0002] Magnesium metal secondary batteries are gaining increasing attention from industry, academia, and research circles due to their many advantages, such as high volumetric energy density, high safety, and abundant raw material resources. As a key component in magnesium metal secondary batteries, magnesium ion storage cathode materials play a vital role in the overall performance of batteries. However, the high charge density of magnesium ions leads to slow transmission in the cathode solid phase structure, and the desolvation process at the interface is also very difficult. Therefore, magnesium storage cathode materials generally have the problem of slow electrochemical reaction kinetics, especially embedded magnesium storage cathodes.

[0003] Among the various reported embedded magnesium storage cathode materials, olivine-type magnesium storage cathodes show outstanding advantages such as high voltage platform, high specific capacity, easy batch synthesis and low cost, and have important development potential. However, in the ether magnesium electrolyte system compatible with magnesium metal anode, the high desolvation energy barrier at the interface causes the charge transfer rate at the interface of the olivine-type cathode to be very slow, the desolvation process is difficult, and the excellent ability to deintercalate magnesium ions cannot be exerted. Therefore, the currently reported olivine-type magnesium storage cathode is generally matched with acetonitrile magnesium electrolytes that are easier to desolvate. However, there are serious side reactions between acetonitrile and magnesium metal anodes, and it cannot be used in magnesium metal secondary battery systems.

[0004] Based on the above background, in order to achieve the matching of olivine-type cathode with ether magnesium electrolyte system and exert excellent performance in magnesium metal secondary batteries, it is necessary to effectively reduce the desolvation energy of the olivine-type cathode interface and accelerate the charge transfer process at the interface. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a sulfide-coated magnesium ion storage positive electrode material, a preparation method and an application in a magnesium metal secondary battery.

[0006] To achieve the above purpose, the present invention adopts the following technical solution:

[0007] A sulfide-coated magnesium ion storage positive electrode material, wherein the positive electrode material is a magnesium ion storage positive electrode material with a sulfide coated on the surface, wherein the magnesium ion storage positive electrode material is an olivine-type positive electrode material.

[0008] On the one hand, the sulfide coating layer can accelerate the desolvation process of solvated magnesium ions at the interface, and on the other hand, it can also improve the structural stability of the positive electrode itself during the charge and discharge process, thereby greatly improving the electrochemical performance of the positive electrode material.

[0009] The thickness of the sulfide coating layer is 2-20 nm, such as 2 nm, 5 nm, 10 nm, 15 nm, 20 nm, etc., but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. In the present invention, if the thickness of the sulfide coating layer is too thin, the coating effect will be poor and the effect of improving the cycle stability will not be achieved; if the thickness of the sulfide coating layer is too thick, the transmission of magnesium ions will be hindered, increasing the interface impedance.

[0010] The sulfide is a transition metal sulfide with a two-dimensional layered structure, which is easy to form a coating layer on the surface of spherical particles, and the interlayer allows smaller ions to pass through, which can effectively improve the electrochemical performance of the magnesium ion storage positive electrode material; such substances include one or more of molybdenum disulfide, vanadium tetrasulfide, vanadium disulfide or cobalt disulfide. The use of the coating layer can effectively improve the magnesium ion storage capacity and long-cycle stability of the positive electrode material.

[0011] A method for preparing a sulfide-coated magnesium ion storage positive electrode material,

[0012] (1) dispersing the sulfide in an organic solvent to obtain a sulfide dispersion;

[0013] (2) adding the magnesium ion storage positive electrode material to the sulfide dispersion obtained in step (1) and mixing evenly, and heating and reacting under sealing conditions after mixing evenly to obtain a mixed precursor; the mass ratio of the magnesium ion storage positive electrode material to the sulfide in the sulfide dispersion is 20 to 100:1;

[0014] (3) heat treating the mixed precursor obtained in step (2) in an inert or reducing atmosphere, and grinding it after cooling to obtain a sulfide-coated magnesium ion storage positive electrode material.

[0015] In the step (1), after the sulfide is dispersed in the organic solvent, the concentration of the metal cation in the dispersion is controlled to be 1 to 200 mmol / L (preferably 5 to 100 mmol / L, more preferably 10 to 50 mmol / L); the organic solvent is one or more of methanol, ethanol, n-propanol, N,N-dimethylformamide or N,N-dimethylacetamide.

[0016] The transition metal ion concentration in the above organic solvent is relatively lower than that in the aqueous solution. If the transition metal ion concentration is too high, agglomeration will easily occur, affecting the coating effect. However, it cannot be too low, which will cause waste of organic solvent.

[0017] The dispersion is formed by ultrasonic dispersion, the frequency of which is 30 to 200 kHz, the temperature of which is 20 to 70° C., and the time of which is 1 to 20 hours (more preferably 3 to 8 hours). Ultrasonic dispersion can make the transition metal sulfide dispersed evenly in the organic solvent, but the ultrasonic dispersion time should not be too short, otherwise it will lead to uneven dispersion and thus induce agglomeration.

[0018] In the step (2), the magnesium ion storage positive electrode material is one or more of the olivine structure MgMXO4, wherein M represents one or more of the elements iron, manganese, cobalt, and nickel, and X represents phosphorus or silicon.

[0019] The average particle size of the olivine-type positive electrode material is 50 to 500 nm, for example, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] The mass ratio of the magnesium ion storage positive electrode material to the sulfide in the sulfide dispersion is preferably 30 to 50: 1. If the amount of sulfide relative to the positive electrode material is too low, the sulfide is insufficient to coat the positive electrode material particles, and it is difficult to achieve a good coating effect; if the amount of sulfide relative to the positive electrode material is too high, the coating layer is too thick, which limits the insertion and extraction rate of magnesium ions, resulting in poor rate performance of the positive electrode material.

[0021] In step (2), the magnesium ion storage positive electrode material is added to the sulfide dispersion obtained in step (1) and stirred for 1 to 6 hours to make it uniform; then the heating reaction time is 2 to 24 hours (more preferably 8 to 10 hours) at 80 to 300° C. (more preferably 140 to 200° C.). By heating the reaction in the sealed reactor to create a high temperature and high pressure atmosphere, the sulfide is uniformly coated on the surface of the positive electrode particles.

[0022] After the reaction in step (2), the mixture is naturally cooled, washed, filtered and dried to obtain a mixed precursor; the organic solvent used to disperse the sulfide in step (1) is used in the washing and filtering process.

[0023] In the step (3), the heat treatment temperature is 150-800°C, and the heat treatment time is 2-10 hours; the inert atmosphere is helium, nitrogen, argon or argon / hydrogen mixture, wherein the volume fraction of hydrogen in the argon / hydrogen mixture is 1-10% (more preferably 3-7%).

[0024] After the heating reaction in the above step (2), the sulfide is relatively loosely coated on the surface of the positive electrode. By heat treating at the temperature and time described in step (3), the sulfide coating layer can be made tighter to obtain sulfide-coated positive electrode particles with good crystallization performance and a tight coating layer. Therefore, the heat treatment temperature cannot be too high.

[0025] An application of the sulfide-coated magnesium ion storage positive electrode material, and an application of the sulfide-coated magnesium ion storage positive electrode material in the preparation of a magnesium storage positive electrode sheet.

[0026] A magnesium storage positive electrode plate, wherein the positive electrode material in the positive electrode plate comprises the above-mentioned sulfide-coated magnesium ion storage positive electrode material, wherein the content of the sulfide-coated magnesium ion storage positive electrode material in the positive electrode material is 40wt% to 98wt%.

[0027] A magnesium metal secondary battery comprises a magnesium metal negative electrode, a separator, an electrolyte and the positive electrode plate.

[0028] The beneficial effects of the present invention are as follows:

[0029] (1) The surface of the sulfide-coated magnesium ion storage positive electrode material of the present invention has a uniform sulfide coating layer, which can prevent the corrosion of the electrolyte to the electrode and accelerate the charge transfer process at the interface; the battery made of the material of the present invention is subjected to a charge and discharge test. Under the conditions of 0.5C charge / 1C discharge, the first discharge specific capacity can reach up to 140mAh / g, the discharge platform is around ~2.5V, and the capacity can reach up to 120mAh / g after 100 cycles. The capacity retention rate can reach up to 85.7%, indicating that the material of the present invention has excellent rate performance and cycle performance;

[0030] (2) The preparation process of the present invention is simple, and the cost of transition metal sulfide and olivine-type positive electrode raw materials and processes is low, and it is easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a SEM image of the molybdenum disulfide coated MgFePO4 positive electrode material obtained in Example 1 of the present invention;

[0032] Figure 2 This is a SEM image of the vanadium disulfide coated MgFePO4 positive electrode material obtained in Example 2 of the present invention;

[0033] Figure 3 This is a SEM image of the molybdenum disulfide coated MgFeSiO4 positive electrode material obtained in Example 3 of the present invention;

[0034] Figure 4 This is a SEM image of the vanadium disulfide coated MgFeSiO4 positive electrode material obtained in Example 4 of the present invention;

[0035] Figure 5 This is a SEM image of the molybdenum disulfide coated MgMnSiO4 positive electrode material obtained in Example 5 of the present invention;

[0036] Figure 6This is a SEM image of the vanadium disulfide coated MgMnSiO4 positive electrode material obtained in Example 6 of the present invention;

[0037] Figure 7 This is a SEM image of the uncoated MgFePO4 positive electrode material obtained in Comparative Example 1 of the present invention;

[0038] Figure 8 This is a SEM image of the uncoated MgFeSiO4 positive electrode material obtained in Comparative Example 2 of the present invention;

[0039] Fig. 9 This is a SEM image of the uncoated MgMnSiO4 positive electrode material obtained in Comparative Example 3 of the present invention; DETAILED DESCRIPTION

[0040] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0041] The sulfide layer coated on the surface of the magnesium ion storage positive electrode material of the present invention has good structural stability and protective effect. It is not only structurally stable in the electrolyte, but also can well isolate moisture, carbon dioxide and corrosion of the electrolyte in the air, inhibit the occurrence of side reactions, and stabilize the olivine structure of the positive electrode material. In addition, the coating layer can accelerate the charge transfer process at the interface, and is conducive to the passage of magnesium ions, thereby improving the magnesium ion storage capacity of the magnesium ion storage positive electrode material, and ensuring the long-cycle stability of the material itself, and has the advantages of good repeatability and strong versatility.

[0042] Example 1

[0043] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0044] (1) accurately weighing 0.2 g of molybdenum disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a molybdenum disulfide dispersion;

[0045] (2) 10 g of olivine-type positive electrode material MgFePO4 was added to the molybdenum disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixed solution was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, it was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0046] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a molybdenum disulfide-coated MgFePO4 positive electrode material (see Figure 1 ).

[0047] The average particle size of the positive electrode material MgFePO4 is 80-120nm.

[0048] like Figure 1 As shown, the surface of the molybdenum disulfide-coated MgFePO4 positive electrode material is uniformly coated with a rough-surfaced molybdenum disulfide coating, and the thickness of the molybdenum disulfide coating is about 5 nm.

[0049] The performance test results of the molybdenum disulfide coated MgFePO4 positive electrode material provided in this embodiment are shown in Table 1.

[0050] Example 2

[0051] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0052] (1) accurately weighing 0.2 g of vanadium disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a vanadium disulfide dispersion;

[0053] (2) 10 g of olivine-type positive electrode material MgFePO4 was added to the vanadium disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixed solution was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, the mixture was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0054] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a vanadium disulfide-coated MgFePO4 positive electrode material (see Figure 2 ).

[0055] The average particle size of the positive electrode material MgFePO4 is 80-120nm. Figure 2 As shown, the surface of the vanadium disulfide-coated MgFePO4 positive electrode material is uniformly coated with a layer of rough vanadium disulfide coating, and the thickness of the vanadium disulfide coating layer is about 10 nm.

[0056] The performance test results of the vanadium disulfide coated MgFePO4 positive electrode material provided in this embodiment are shown in Table 1.

[0057] Example 3

[0058] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0059] (1) accurately weighing 0.2 g of molybdenum disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a vanadium disulfide dispersion;

[0060] (2) 10 g of olivine-type positive electrode material MgFeSiO4 was added to the molybdenum disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixed solution was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, it was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0061] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a molybdenum disulfide-coated MgFeSiO4 positive electrode material (see Figure 3 ).

[0062] The average particle size of the positive electrode material MgFeSiO4 is 80-120nm. Figure 3 As shown, the surface of the molybdenum disulfide-coated MgFeSiO4 positive electrode material is uniformly coated with a rough-surfaced molybdenum disulfide coating, and the thickness of the molybdenum disulfide coating is about 10 nm.

[0063] The performance test results of the molybdenum disulfide coated MgFeSiO4 positive electrode material provided in this embodiment are shown in Table 1.

[0064] Example 4

[0065] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0066] (1) accurately weighing 0.2 g of vanadium disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a vanadium disulfide dispersion;

[0067] (2) 10 g of olivine-type positive electrode material MgFeSiO4 was added to the vanadium disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixed solution was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, it was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0068] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a vanadium disulfide-coated MgFeSiO4 positive electrode material (see Figure 4 ).

[0069] The average particle size of the positive electrode material MgFeSiO4 is 80-120nm. Figure 4 As shown, the surface of the vanadium disulfide-coated MgFeSiO4 positive electrode material is uniformly coated with a layer of rough vanadium disulfide coating, and the thickness of the vanadium disulfide coating layer is about 10 nm.

[0070] The performance test results of the vanadium disulfide coated MgMnSiO4 positive electrode material provided in this embodiment are shown in Table 1.

[0071] Example 5

[0072] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0073] (1) accurately weighing 0.2 g of molybdenum disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a vanadium disulfide dispersion;

[0074] (2) 10 g of olivine-type positive electrode material MgMnSiO4 was added to the molybdenum disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixture was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, it was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0075] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a molybdenum disulfide-coated MgMnSiO4 positive electrode material (see Figure 5 ).

[0076] The average particle size of the positive electrode material MgMnSiO4 is 80-120nm. Figure 5 As shown, the surface of the molybdenum disulfide-coated MgMnSiO4 positive electrode material is uniformly coated with a rough-surfaced molybdenum disulfide coating, and the thickness of the molybdenum disulfide coating is about 10 nm.

[0077] The performance test results of the molybdenum disulfide coated MgMnSiO4 positive electrode material provided in this embodiment are shown in Table 1.

[0078] Example 6

[0079] The method for preparing the sulfide-coated positive electrode material is specifically as follows:

[0080] (1) accurately weighing 0.2 g of vanadium disulfide, dispersing it in 100 mL of anhydrous ethanol, and ultrasonically dispersing it at 80 kHz and 20° C. for 10 h to obtain a vanadium disulfide dispersion;

[0081] (2) 10 g of olivine-type positive electrode material MgMnSiO4 was added to the vanadium disulfide dispersion obtained in step (1), and after magnetic stirring for 6 h, the mixed solution was added to a polytetrafluoroethylene reactor, sealed, and placed in a 200° C. oven for reaction for 10 h. After being taken out and naturally cooled, the mixture was washed with anhydrous ethanol, filtered 3 times, and dried to obtain a mixed precursor;

[0082] (3) The mixed precursor obtained in step (2) was placed in a tubular resistance furnace, calcined at 300° C. in an argon atmosphere for 8 h, and ground after cooling to obtain a vanadium disulfide-coated MgMnSiO4 positive electrode material (see Figure 6 ).

[0083] The average particle size of the positive electrode material MgMnSiO4 is 80-120nm. Figure 6 As shown, the surface of the vanadium disulfide-coated MgMnSiO4 positive electrode material is uniformly coated with a layer of rough vanadium disulfide coating, and the thickness of the vanadium disulfide coating layer is about 10 nm.

[0084] The performance test results of the vanadium disulfide coated MgMnSiO4 positive electrode material provided in this embodiment are shown in Table 1.

[0085] Comparative Example 1

[0086] The positive electrode material of this comparative example directly uses the magnesium-containing positive electrode material MgFePO4 in Example 1 without being coated with any sulfide.

[0087] like Figure 7 As shown, the surface of the MgFePO4 positive electrode material is not coated, and the surface is smooth and complete. The performance test results of the positive electrode material of this comparative example are shown in Table 1.

[0088] Comparative Example 2

[0089] The positive electrode material of this comparative example directly uses the magnesium-containing positive electrode material MgFeSiO4 in Example 3 without being coated with any sulfide.

[0090] like Figure 8 As shown, the surface of the uncoated MgFeSiO4 positive electrode material is smooth and complete.

[0091] The performance test results of the positive electrode material of this comparative example are shown in Table 1.

[0092] Comparative Example 3

[0093] The positive electrode material of this comparative example directly uses the magnesium-containing positive electrode material MgMnSiO4 in Example 5 without being coated with any sulfide.

[0094] like Fig. 9 As shown, the surface of the uncoated MgMnSiO4 positive electrode material is smooth and complete.

[0095] The performance test results of the positive electrode material of this comparative example are shown in Table 1.

[0096] Test Method

[0097] The positive electrode material products provided in the above embodiments and comparative examples are used as positive electrode active materials to prepare magnesium metal secondary batteries. The preparation method is as follows: the positive electrode active material, the binder polyvinylidene fluoride, and the conductive agent (SP conductive agent) are mixed in NMP in a ratio of 8:1:1 to form a slurry, the solid content of which is controlled to be 70%, and the slurry is coated on a stainless steel foil as a positive electrode, and then dried in a blast drying oven at 80°C for 12 hours, and the positive electrode sheet is punched into The discs were dried under vacuum for 24 h; magnesium metal sheets ( The CR2032 button cell was prepared in an argon-filled glove box with a thickness of 200 μm) as the negative electrode, the materials in the above embodiments and comparative examples as the positive electrode, the electrolyte solute was magnesium tetrakis(hexafluoroisopropyl)borate with a concentration of 0.3 M, the electrolyte solvent was a mixed solvent of ethylene glycol dimethyl ether and diethylene glycol dimethyl ether (volume ratio of 1:1), Whatman GF / D as the diaphragm, and the CR2032 button cell was prepared in an argon-filled glove box. The cell was used for electrochemical testing.

[0098] The capacity retention rate after 100 charge and discharge cycles was tested using a Blue Power Battery Test System (CT 2001A) in the potential range of 1.5 to 3.5 V at rates of 0.1C and 0.5C (1C = 150 mAh / g).

[0099] The results of the above tests are shown in Table 1 below:

[0100]

[0101] It can be seen from the above embodiments and comparative examples that the sulfide coating layer is crucial to the capacity of the olivine-type positive electrode material. The presence of the sulfide coating layer greatly improves the positive electrode magnesium storage capacity.

[0102] By comparing the data of Examples 1-6, it can be found that among the three olivine-type positive electrode materials, the coated MgFeSiO4 and MgMnSiO4 have higher magnesium ion storage capacity, and the performance of the positive electrode material coated with molybdenum disulfide is generally better than that of the vanadium disulfide coating.

[0103] In Comparative Examples 1-3, since there is no sulfide coating layer, the desolvation process at the interface is very difficult, so it is difficult for magnesium ions to be embedded in the positive electrode material, making it difficult for these materials to perform the magnesium storage performance.

[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A sulfide-coated magnesium ion storage positive electrode material, characterized in that: The positive electrode material is a magnesium ion storage positive electrode material with a sulfide coated on its surface, wherein the magnesium ion storage positive electrode material is an olivine type positive electrode material; The magnesium ion storage positive electrode material is one or more of olivine structure MgMXO4, wherein M represents one or more of iron, manganese, cobalt, and nickel elements, and X represents phosphorus or silicon elements; The sulfide is a transition metal sulfide; The thickness of the sulfide coating layer is 2-20 nm.

2. A method for preparing the sulfide-coated magnesium ion storage positive electrode material according to claim 1, characterized in that: (1) dispersing the sulfide in an organic solvent to obtain a sulfide dispersion; (2) adding the magnesium ion storage positive electrode material to the sulfide dispersion obtained in step (1) and mixing evenly, and heating and reacting under sealing conditions after mixing evenly to obtain a mixed precursor; the mass ratio of the magnesium ion storage positive electrode material to the sulfide in the sulfide dispersion is 20 to 100:1; (3) The mixed precursor obtained in step (2) is heat treated in an inert or reducing atmosphere, and then ground after cooling to obtain a sulfide-coated magnesium ion storage positive electrode material.

3. The method for preparing the sulfide-coated magnesium ion storage positive electrode material according to claim 2, characterized in that: In the step (1), after the sulfide is dispersed in the organic solvent, the concentration of the metal cation in the dispersion is controlled to be 1 to 200 mmol / L; the organic solvent is one or more of methanol, ethanol, n-propanol, N,N-dimethylformamide or N,N-dimethylacetamide.

4. The method for preparing the sulfide-coated magnesium ion storage positive electrode material according to claim 2, characterized in that: In the step (2), the magnesium ion storage positive electrode material is added to the sulfide dispersion obtained in the step (1) and stirred for 1 to 6 hours to make it uniformly mixed; and then the heating reaction time is 80 to 300° C. and 2 to 24 hours.

5. The method for preparing the sulfide-coated magnesium ion storage positive electrode material according to claim 2, characterized in that: In the step (3), the heat treatment temperature is 150 to 800°C, and the heat treatment time is 2 to 10 hours; the inert atmosphere is helium, nitrogen, argon or an argon / hydrogen mixture, wherein the volume fraction of hydrogen in the argon / hydrogen mixture is 1 to 10%.

6. An application of the sulfide-coated magnesium ion storage positive electrode material according to claim 1, characterized in that: The use of the sulfide-coated magnesium ion storage positive electrode material in the preparation of magnesium storage positive electrode sheets.

7. A magnesium storage positive electrode plate, characterized in that: The positive electrode material in the positive electrode plate includes the sulfide-coated magnesium ion storage positive electrode material according to claim 1, wherein the content of the sulfide-coated magnesium ion storage positive electrode material in the positive electrode material is 40 wt% to 98 wt%.

8. A magnesium metal secondary battery, characterized in that: The magnesium metal secondary battery comprises a magnesium metal negative electrode, a separator, an electrolyte and the positive electrode sheet according to claim 7.

Citation Information

Patent Citations

  • Magnesium-transition metal phosphoric acid compound positive electrode material of rechargeable battery and preparation method

    CN106848307A

  • Ternary cathode material coated with vanadium sulfide of lithium ion battery and preparation method of ternary cathode material

    CN106960955A

  • Sodium vanadate / molybdenum disulfide nanobelt composite material, preparation method thereof and application of sodium vanadate / molybdenum disulfide nanobelt composite material in magnesium ion battery