Negative electrode and preparation method thereof and zinc ion battery

By forming a porous structure of hydrophobic polypropionate layer on the zinc matrix surface of the zinc ion battery, the problems of zinc negative electrode corrosion and zinc dendrites are solved, the cycle life and rate performance of zinc ion battery are improved, and more stable battery use is achieved.

CN115132970BActive Publication Date: 2024-11-22SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210807131.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-11-22
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

The contact between the zinc negative electrode in the zinc ion battery and the electrolyte leads to corrosion and the formation of zinc dendrites, which pierces the separator and causes a short circuit, limiting the service life of the zinc ion battery.

Method used

A hydrophobic zinc polypropionate layer is formed on the surface of the zinc matrix, with a porous structure, which acts as a protective layer to block contact of electrolyte and improve the desolvation ability of zinc ions, and inhibit the generation and growth of zinc dendrites.

Benefits of technology

It effectively improves the cycle life and rate performance of zinc ion batteries, avoids the occurrence of short circuits, and enhances the corrosion resistance of the negative electrode and uniform electric field distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115132970B_ABST
    Figure CN115132970B_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode, comprising a zinc substrate and a hydrophobic zinc polypropionate layer arranged on the surface of the zinc substrate, wherein the hydrophobic zinc polypropionate layer has a porous structure. The hydrophobic zinc polypropionate layer can protect the zinc substrate and prevent the electrolyte in the zinc ion battery from directly contacting the zinc substrate. At the same time, the setting of the hydrophobic zinc polypropionate layer effectively inhibits the generation and growth of zinc dendrites, thereby avoiding the occurrence of short circuits and improving the cycle life of the zinc ion battery; the zinc ions in the hydrophobic zinc polypropionate layer can move freely under an electric field, thereby improving the rate performance of the zinc ion battery. The present application also provides a method for preparing a negative electrode and a zinc ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode and a preparation method thereof, and a zinc ion battery. Background Art

[0002] Zinc-ion batteries are considered as one of the important directions to replace lithium batteries due to their advantages such as high safety, low price, stable chemical properties, and high theoretical specific capacity. However, the zinc negative electrode contacts and reacts with the electrolyte, causing corrosion and passivation of the zinc negative electrode, thereby forming zinc dendrites. The continuous growth of zinc dendrites will pierce the diaphragm, causing the battery to short-circuit, thus limiting the use of zinc-ion batteries. Summary of the invention

[0003] In view of this, the present application provides a negative electrode and a preparation method thereof and a zinc ion battery, wherein the negative electrode can inhibit the formation and growth of zinc dendrites, thereby improving the cycle life of the zinc ion battery and promoting the use of the zinc ion battery.

[0004] In a first aspect, the present application provides a negative electrode, comprising a zinc substrate and a hydrophobic zinc polypropionate layer disposed on the surface of the zinc substrate, wherein the hydrophobic zinc polypropionate layer has a porous structure.

[0005] Optionally, the pore size of the porous structure is 0.05 μm-0.3 μm.

[0006] Optionally, the thickness of the hydrophobic polyzinc propionate layer is 3 μm-10 μm.

[0007] Optionally, the thickness ratio of the zinc substrate to the hydrophobic zinc polypropionate layer is 70-120.

[0008] Optionally, the material of the zinc matrix includes zinc element or zinc alloy.

[0009] In a second aspect, the present application provides a method for preparing a negative electrode, comprising: forming a hydrophobic zinc polypropionate layer on the surface of a zinc substrate to obtain a negative electrode, wherein the hydrophobic zinc polypropionate layer has a porous structure.

[0010] Optionally, the forming of a hydrophobic zinc polypropionate layer on the surface of the zinc substrate includes: dissolving zinc acrylate and a photoinitiator in an organic solvent to obtain a mixed solution; coating the mixed solution on the surface of the zinc substrate, and forming the hydrophobic zinc polypropionate layer after photoinitiated polymerization.

[0011] Furthermore, the mass ratio of the zinc acrylate to the photoinitiator is 33-100.

[0012] Furthermore, the concentration of the zinc acrylate in the mixed solution is 2 mg / mL-5 mg / mL.

[0013] Furthermore, the photo-initiated polymerization time is 1h-4h.

[0014] In a third aspect, the present application provides a zinc ion battery, comprising the negative electrode described in the first aspect or the negative electrode prepared by the preparation method described in the second aspect.

[0015] Optionally, the zinc ion battery also includes a positive electrode, an electrolyte and a separator.

[0016] Furthermore, the positive electrode includes a positive electrode active material, and the positive electrode active material includes at least one of manganese dioxide, sodium vanadate and vanadium pentoxide.

[0017] Furthermore, the electrolyte is an aqueous solution of an electrolyte, and the electrolyte includes a water-soluble zinc salt.

[0018] Furthermore, the material of the diaphragm includes at least one of glass fiber, cellulose, polyethylene and polypropylene.

[0019] The hydrophobic zinc polypropionate layer in the negative electrode provided in the present application can protect the zinc matrix and prevent the electrolyte in the zinc ion battery from directly contacting the zinc matrix. At the same time, the provision of the hydrophobic zinc polypropionate layer improves the desolvation ability of zinc ions in the electrolyte, improves the uniform distribution of the electric field and the corrosion resistance of the negative electrode during the charge and discharge process, effectively inhibits the generation and growth of zinc dendrites, thereby avoiding the occurrence of short circuits and improving the cycle life of the zinc ion battery; and the zinc ions in the hydrophobic zinc polypropionate layer can move freely under the electric field, thereby improving the rate performance of the zinc ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the embodiments or the prior art description. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0021] Figure 1 A schematic diagram of the structure of a negative electrode provided in one embodiment of the present application.

[0022] Figure 2 A flow chart of a method for preparing a negative electrode provided in one embodiment of the present application.

[0023] Figure 3 This is a cross-sectional electron microscope image of the negative electrode prepared in Example 1.

[0024] Figure 4 This is an electron microscope image of the hydrophobic polyzinc propionate layer in the negative electrode prepared in Example 1.

[0025] Figure 5 This is a diagram of the curling experiment process of the negative electrode prepared in Example 1.

[0026] Figure 6This is an in-situ optical microscope image of the negative electrode.

[0027] Figure 7 The constant current charge and discharge curves of the battery at different current densities.

[0028] Figure 8 This is the rate performance diagram of the battery. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0030] See also Figure 1 , is a schematic diagram of the structure of the negative electrode provided in one embodiment of the present application, wherein the negative electrode 100 includes a zinc substrate 10 and a hydrophobic zinc polypropionate layer 20 disposed on the surface of the zinc substrate 10, and the hydrophobic zinc polypropionate layer 20 has a porous structure. During the charge and discharge cycle of a zinc ion battery, factors such as uneven electric field on the surface of the zinc negative electrode, the generation of a tip effect, and difficulty in desolvation of zinc ions will lead to the formation of zinc dendrites; the dendrites continue to grow and eventually pierce the diaphragm, causing a short circuit in the battery; at the same time, the electrolyte continuously erodes the surface of the zinc negative electrode, and a large amount of byproducts will be generated, affecting the use of the battery. The hydrophobic zinc polypropionate layer 20 in the negative electrode 100 provided in the present application can be used as a protective layer to protect the zinc substrate 10, thereby avoiding direct contact between the electrolyte and the zinc substrate 10, especially avoiding direct contact between the aqueous electrolyte and the zinc substrate 10. At the same time, due to the hydrophobicity of the hydrophobic zinc polypropionate layer 20 and the anions on the polymer chain, the desolvation ability of zinc ions in the electrolyte is enhanced, and the electric field distribution and corrosion resistance of the negative electrode 100 of the zinc ion battery are improved during the charging and discharging process, effectively inhibiting the generation and growth of zinc dendrites and the occurrence of hydrogen evolution and corrosion side reactions, thereby avoiding the occurrence of short circuits and improving the cycle life of the zinc ion battery. In addition, the zinc ions in the hydrophobic zinc polypropionate layer 20 can move freely under the action of the electric field, thereby replenishing the zinc ion supply and improving the battery's rate performance.

[0031] In the embodiment of the present application, the hydrophobic zinc polypropionate layer 20 is a mesh structure, so that the hydrophobic zinc polypropionate layer 20 has a porous structure. Further, the hydrophobic zinc polypropionate layer 20 is a cross-linked mesh structure. In other words, the hydrophobic zinc polypropionate layer 20 is a mesh structure formed by a cross-linking reaction. The distribution of the porous structure in the hydrophobic zinc polypropionate layer 20 of the cross-linked mesh structure is more uniform, which is conducive to the uniform deposition of zinc ions on the surface of the negative electrode 100.

[0032] In the embodiment of the present application, the hydrophobic polypropionic acid zinc layer 20 has a plurality of porous structures, and at least 80% of the porous structures have a pore size of 0.05 μm-0.3 μm (such as 0.05 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm or 0.3 μm, etc.), which is beneficial to blocking the electrolyte and also beneficial to the transmission of ions. Further, at least 90% of the porous structures have a pore size of 0.05 μm-0.3 μm.

[0033] In the embodiment of the present application, the pore size of the porous structure is 0.05μm-0.3μm. That is, the pore size of all porous structures is within the range of 0.05μm-0.3μm, which is more conducive to blocking the electrolyte. Specifically, the pore size of the porous structure can be but is not limited to 0.05μm, 0.1μm, 0.15μm, 0.2μm, 025μm or 0.3μm, etc. Further, the pore size of the porous structure is 0.05μm-0.15μm, 0.15μm-0.2μm or 0.2μm-0.3μm, etc.

[0034] In the embodiment of the present application, the thickness of the hydrophobic zinc polypropionate layer 20 is 3μm-10μm. In this way, the hydrophobic zinc polypropionate layer 20 can protect the zinc substrate 10 without affecting the transmission of ions. Specifically, the thickness of the hydrophobic zinc polypropionate layer 20 can be, but is not limited to, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm, etc. Further, the thickness of the hydrophobic zinc polypropionate layer 20 is 3μm-5μm, 5μm-8μm or 7μm-10μm, etc.

[0035] In the embodiment of the present application, the thickness ratio of the zinc substrate 10 and the hydrophobic zinc polypropionate layer 20 is 70-120. In this way, the hydrophobic zinc polypropionate layer 20 can not only provide better protection for the zinc substrate 10, but also ensure the electrochemical performance of the battery. Specifically, the thickness ratio of the zinc substrate 10 and the hydrophobic zinc polypropionate layer 20 can be, but not limited to, 75, 80, 85, 90, 95, 100, 110, 115 or 120, etc. Further, the thickness ratio of the zinc substrate 10 and the hydrophobic zinc polypropionate layer 20 is 70-90, 85-105 or 95-120, etc.

[0036] In the embodiment of the present application, the thickness of the zinc substrate 10 is 400 μm-600 μm. Specifically, the thickness of the zinc substrate 10 may be, but is not limited to, 400 μm, 450 μm, 500 μm, 550 μm or 600 μm, etc. Further, the thickness of the zinc substrate 10 is 400 μm-500 μm or 500 μm-600 μm.

[0037] In the embodiment of the present application, the material of the zinc substrate 10 includes zinc or zinc alloy. The zinc substrate 10 can be, but is not limited to, zinc foil, zinc sheet, zinc powder, zinc alloy foil, zinc alloy sheet, and the like.

[0038] In the embodiment of the present application, 10 mA / cm 2 Under the charge and discharge conditions of , the cycle life of the negative electrode 100 reaches more than 280h, which has excellent cycle life and stability, and is conducive to use in zinc ion batteries.

[0039] The present application also provides a method for preparing a negative electrode 100, which can prepare the negative electrode 100 in any of the above embodiments, comprising: forming a hydrophobic zinc polypropionate layer 20 on the surface of a zinc substrate 10, wherein the hydrophobic zinc polypropionate layer 20 has a porous structure, to obtain the negative electrode 100. By forming the hydrophobic zinc polypropionate layer 20 on the surface of the zinc substrate 10, the zinc substrate 10 is protected, and the uniform precipitation of zinc ions during the charge and discharge process is facilitated, thereby obtaining a safe and highly reversible negative electrode 100, and improving the electrochemical performance of a zinc ion battery having the negative electrode 100.

[0040] See also Figure 2 , is a flow chart of a method for preparing a negative electrode provided in one embodiment of the present application, comprising:

[0041] S101: dissolving zinc acrylate and a photoinitiator in an organic solvent to obtain a mixed solution.

[0042] S102: coating the mixed solution on the surface of the zinc substrate to form a hydrophobic polyzinc propionate layer after photoinitiated polymerization, wherein the hydrophobic polyzinc propionate layer has a porous structure, thereby obtaining a negative electrode.

[0043] In the present application, the hydrophobic polypropionate zinc layer 20 is directly formed on the surface of the zinc substrate 10 by photoinitiated polymerization, thereby improving the bonding force between the zinc substrate 10 and the hydrophobic polypropionate zinc layer 20 and ensuring the reliability of the negative electrode 100 structure.

[0044] In S101, zinc acrylate and a photoinitiator are mixed to obtain a mixed solution, so that the zinc acrylate can be polymerized and cross-linked to form a hydrophobic zinc polypropionate layer 20 under the action of the photoinitiator. In the embodiment of the present application, the mass ratio of zinc acrylate to the photoinitiator is 33-100, so that zinc acrylate can be fully polymerized and cross-linked, and the formation of a porous structure in the hydrophobic zinc polypropionate layer 20 can be ensured. Specifically, the mass ratio of zinc acrylate to the photoinitiator can be, but is not limited to, 33, 45, 50, 60, 75, 90 or 100, etc. Further, the mass ratio of zinc acrylate to the photoinitiator can be 33-50, 45-60, 50-75 or 75-100, etc.

[0045] In the embodiment of the present application, the concentration of zinc acrylate in the mixed solution is 2 mg / mL-5 mg / mL, which is conducive to the formation of the hydrophobic polypropionate zinc layer 20. Specifically, the concentration of zinc acrylate in the mixed solution can be, but is not limited to, 2 mg / mL, 3 mg / mL, 4 mg / mL or 5 mg / mL. Further, the concentration of zinc acrylate in the mixed solution can be 2 mg / mL-3 mg / mL, 3 mg / mL-4 mg / mL or 4 mg / mL-5 mg / mL.

[0046] In the present application, the photoinitiator absorbs energy of a certain wavelength to generate free radicals and cations, thereby initiating the polymerization and cross-linking of zinc acrylate to form polyzinc propionate. In the embodiment of the present application, the photoinitiator may include an ultraviolet light initiator. Specifically, the ultraviolet light initiator may include, but is not limited to, at least one of 2,2-dimethoxy-phenylacetophenone, α,α'-ethoxyacetophenone, 2,4,6-trimethylbenzoyl ethyl phosphate, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone and methyl benzoylformate.

[0047] In the present application, the organic solvent is selected from solvents capable of dissolving zinc acrylate and a photoinitiator. Specifically, the organic solvent may include, but is not limited to, 2-methoxyethanol.

[0048] In S102, the mixed solution on the surface of the zinc substrate 10 undergoes photoinitiated polymerization to obtain a hydrophobic zinc polypropionate layer 20, and since the hydrophobic zinc polypropionate layer 20 is directly formed on the surface of the zinc substrate 10, the hydrophobic zinc polypropionate layer 20 has a high bonding strength with the zinc substrate 10, thereby ensuring the structural reliability of the negative electrode 100. In the present application, zinc acrylate is cross-linked to form a network structure under the promotion of the generation of a photoinitiator, thereby obtaining a hydrophobic zinc polypropionate layer 20 having a porous structure.

[0049] In the present application, when a UV light initiator is selected, photopolymerization can be carried out by UV light irradiation; the wavelength of the UV light can be selected according to the performance of the photoinitiator. For example, when the photoinitiator includes 2,2-dimethoxy-phenylacetophenone, a UV light with a wavelength of 365nm can be selected to irradiate the mixed solution on the surface of the zinc substrate 10, and 2,2-dimethoxy-phenylacetophenone can absorb the UV light with a wavelength of 365nm, thereby generating free radicals and cations, inducing free radical polymerization and crosslinking of zinc acrylate to photopolymerize. In the embodiment of the present application, the time of photopolymerization is 1h-4h. In this way, crosslinking and polymerization can be ensured to be complete, and the bonding force between the hydrophobic polypropionate zinc layer 20 and the zinc substrate 10 can be promoted. Specifically, the time of photopolymerization can be, but is not limited to, 1h, 1.5h, 1h, 2.5h, 3h, 3.5h or 4h, etc. Further, the time of photopolymerization can be 1h-2h, 2h-3h or 3h-4h, etc. In the embodiment of the present application, the intensity of the photo-induced polymerization is 0.5 W / cm 2 -2W / cm 2 , which helps cross-linking and polymerization to be complete, and promotes the formation of the hydrophobic polypropionate zinc layer 20. Specifically, the intensity of the light-induced polymerization can be, but is not limited to, 0.5 W / cm 2 , 1W / cm 2 , 1.5W / cm 2 or 2W / cm 2 In the embodiment of the present application, the ultraviolet light source irradiates the mixed solution, and the distance from the zinc substrate 10 is 2cm-5cm. Further, the distance from the ultraviolet light source to the zinc substrate 10 is 2cm-3cm. Specifically, an ultraviolet lamp can be used for photoinitiated polymerization.

[0050] It is understandable that the hydrophobic polypropionate zinc layer 20 may also be directly attached to the surface of the zinc substrate 10 to form the negative electrode 100 .

[0051] The preparation method of the negative electrode 100 provided in the present application is simple, easy to operate, has low preparation cost, can be industrially produced, and the hydrophobic polypropionate zinc layer 20 is tightly combined with the zinc substrate 10 and is not easy to fall off, thereby improving the stability and reliability of the negative electrode 100 and facilitating the use of the negative electrode 100.

[0052] The present application also provides a zinc ion battery, comprising the negative electrode 100 in any of the above embodiments. The zinc ion battery having the above negative electrode 100 has excellent cycle life and rate performance, which is conducive to the wide use of the battery.

[0053] In the embodiment of the present application, the zinc ion battery may further include a positive electrode. In the embodiment of the present application, the positive electrode includes a positive electrode active material, and the positive electrode active material may include at least one of manganese dioxide, sodium vanadate and vanadium pentoxide.

[0054] In the embodiment of the present application, the zinc ion battery may further include a diaphragm. In the embodiment of the present application, the diaphragm may be disposed between the positive electrode and the negative electrode 100. In the embodiment of the present application, the material of the diaphragm includes at least one of glass fiber, cellulose, polyethylene and polypropylene.

[0055] In one embodiment of the present application, the zinc ion battery may further include an electrolyte, the electrolyte being an aqueous solution of an electrolyte, and the electrolyte including a water-soluble zinc salt. That is, the zinc ion battery is an aqueous zinc ion battery. In one embodiment of the present application, the water-soluble zinc salt includes at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc bistrifluoromethylsulfonyl imide, zinc trifluoromethanesulfonate, zinc phenolsulfonate, zinc gluconate and zinc acetate. In another embodiment of the present application, a soluble vanadium salt or a soluble manganese salt is also added to the aqueous electrolyte. In this way, the rate performance of the battery can be further improved. Specifically, the vanadium salt may include but is not limited to at least one of vanadium oxalate, vanadium chloride, vanadium acetate, vanadium sulfate, triisopropyl vanadium, vanadium trichloride, vanadium acetylacetonate and vanadium acetylacetonate; the manganese salt may include but is not limited to at least one of manganese sulfate, manganese acetate, manganese chloride, manganese nitrate and manganese acetylacetonate. In another embodiment of the present application, the zinc ion battery may further include a solid electrolyte. That is, the zinc ion battery is a solid-state zinc ion battery.

[0056] The effects of the negative electrode provided in the present application are further illustrated below through specific examples.

[0057] Example 1

[0058] 0.01g of zinc acrylate and 0.0002g of 2,2-dimethoxy-phenylacetophenone were dissolved in 2mL of 2-methoxyethanol solvent to form a mixed solution. The mixed solution was poured on the surface of zinc foil (4cm wide × 10cm long × 500μm thick), and the surface of the zinc foil was adhered with silicone strips to prevent the mixed solution from flowing away. Then the zinc foil was placed under ultraviolet light (wavelength 365nm) for 2h to form a hydrophobic polyacrylic acid zinc layer (5μm thick) on the surface of the zinc foil to obtain the negative electrode.

[0059] See also Figure 3 and Figure 4 ,in Figure 3 This is a cross-sectional electron microscope image of the negative electrode obtained in Example 1. Figure 4 This is an electron microscope image of the hydrophobic polypropionate zinc layer in the negative electrode prepared in Example 1, where the dotted line range is the hydrophobic polypropionate zinc layer. It can be seen that the hydrophobic polypropionate zinc layer in the negative electrode has a porous structure. Figure 5, which is a diagram of the curling experiment process of the negative electrode prepared in Example 1. By curling the negative electrode prepared in Example 1, the hydrophobic zinc polypropionate layer and the zinc foil in the negative electrode are still tightly bonded after volatilization, indicating that the bonding force between the hydrophobic zinc polypropionate layer and the zinc foil is excellent.

[0060] Example 2

[0061] The method is substantially the same as Example 1, except that the thickness of the hydrophobic polyzinc propionate layer is 3 μm.

[0062] Example 3

[0063] The method is substantially the same as Example 1, except that the thickness of the hydrophobic polyzinc propionate layer is 10 μm.

[0064] Example 4

[0065] It is substantially the same as Example 1, except that the thickness of the hydrophobic polyzinc propionate layer is 20 μm.

[0066] Example 5

[0067] It is substantially the same as Example 1, except that the thickness of the hydrophobic polyzinc propionate layer is 1 μm.

[0068] Effect Example

[0069] The negative electrode prepared in Example 1 was used as the working electrode and the counter electrode, the electrolyte was 2M zinc sulfate, and the glass fiber membrane was used as the separator to assemble a transparent battery as the experimental group; the control group used zinc foil as the working electrode and the counter electrode, and the other conditions were the same. The negative electrode surface of the battery in the experimental group and the control group during the working process was observed by in-situ optical microscope. The results are as follows Figure 6 As shown. It can be seen that the surface of the negative electrode in the experimental group did not change within 0min-20min, and no dendrites were generated, while the zinc foil of the control group was light-colored at 0min. As the working time increased, dark substances were generated on the light-colored surface, that is, obvious dendrites were generated on the surface of the zinc foil in the control group. Therefore, the setting of the hydrophobic polypropionic acid zinc layer in the present application effectively inhibits the generation and growth of zinc dendrites.

[0070] The negative electrode prepared in Example 1 was used as the working electrode and the counter electrode, the electrolyte was 2M zinc sulfate, and the glass fiber membrane was used as the separator to assemble a 2032 button-type battery as the experimental group; the control group used zinc foil as the working electrode and the counter electrode, and the other conditions were the same. 2 The constant current charge and discharge were performed at a current density of 0.2 h each, and the cycle was repeated alternately. The results were as follows: Figure 7As shown, the constant current charge and discharge curves of the battery at different current densities show that the cycle life of the battery in the experimental group reaches more than 280 hours, which is significantly better than that in the control group. At the same time, the negative electrodes prepared in Examples 2-5 are subjected to the same experiment as above, and it is found that the cycle life of the prepared battery can reach more than 280 hours, and the cycle life of the battery prepared by the negative electrodes of Examples 1-3 is even higher.

[0071] The negative electrode prepared in Example 1 was used as the negative electrode, manganese dioxide was used as the positive electrode, a mixture of 2M zinc sulfate and 0.1M manganese sulfate was used as the electrolyte, and a glass fiber membrane was used as a separator to assemble a 2032 button-type battery as the experimental group; the control group used zinc foil directly as the negative electrode, and the other conditions were the same. The battery was charged and discharged 10 times at current densities of 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 1.5A / g, 2A / g, and 3A / g, and the rate performance diagram of the battery was obtained, as shown in FIG. Figure 8 As shown, it can be seen that the rate performance of the experimental group battery is significantly better than that of the control group. At the same time, the negative electrodes prepared in Examples 2-5 were subjected to the same experiment as above, and it was found that the rate performance of the prepared batteries was also significantly better than that of the control group, and the rate performance of the batteries prepared by the negative electrodes of Examples 1-3 was even better. It can be seen that the battery prepared by the negative electrode provided in the present application has excellent cycle life and rate performance, which is beneficial to the use of the battery.

[0072] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A negative electrode, characterized in that: The invention comprises a zinc substrate and a hydrophobic zinc polypropionate layer arranged on the surface of the zinc substrate, wherein the hydrophobic zinc polypropionate layer has a porous structure.

2. The negative electrode according to claim 1, characterized in that The pore size of the porous structure is 0.05 μm-0.3 μm.

3. The negative electrode according to claim 1, characterized in that The thickness of the hydrophobic polyzinc propionate layer is 3 μm-10 μm.

4. The negative electrode according to claim 1, characterized in that The thickness ratio of the zinc substrate to the hydrophobic polypropionate zinc layer is 70-120.

5. The negative electrode according to claim 1, characterized in that The material of the zinc substrate includes zinc element or zinc alloy.

6. A method for preparing a negative electrode, characterized in that: The method comprises: forming a hydrophobic zinc polypropionate layer on the surface of a zinc substrate to obtain a negative electrode, wherein the hydrophobic zinc polypropionate layer has a porous structure.

7. The preparation method according to claim 6, characterized in that: The method of forming a hydrophobic polypropionate zinc layer on the surface of the zinc substrate comprises: dissolving zinc acrylate and a photoinitiator in an organic solvent to obtain a mixed solution; The mixed solution is coated on the surface of the zinc substrate, and the hydrophobic polyzinc propionate layer is formed after photoinitiated polymerization.

8. The preparation method according to claim 7, characterized in that: The mass ratio of the zinc acrylate to the photoinitiator is 33-100; The concentration of zinc acrylate in the mixed solution is 2 mg / mL-5 mg / mL; The time of the photo-initiated polymerization is 1 h to 4 h.

9. A zinc ion battery, characterized in that: The invention comprises the negative electrode according to any one of claims 1 to 5 or the negative electrode prepared by the preparation method according to any one of claims 6 to 8.

10. The zinc ion battery according to claim 9, characterized in that: The zinc ion battery also includes a positive electrode, an electrolyte and a separator; The positive electrode includes a positive electrode active material, and the positive electrode active material includes at least one of manganese dioxide, sodium vanadate and vanadium pentoxide; The electrolyte is an aqueous solution of an electrolyte, and the electrolyte includes a water-soluble zinc salt; The material of the separator includes at least one of glass fiber, cellulose, polyethylene and polypropylene.