Positive electrode active material recycling method
Through environmentally friendly processes such as heat treatment, washing and spray drying, the problem of non-environmental acid extraction in the reuse of lithium secondary battery cathode active materials has been solved, and the effective collection of lithium elements and improvement of electrode performance have been achieved.
Patent Information
- Application Number
- CN202180014643.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-01-15
AI Technical Summary
Among the existing methods for reusing cathode active materials of lithium secondary batteries, the acid extraction process is not environmentally friendly and cannot effectively collect lithium elements, resulting in high process costs and reduced electrode performance.
The active material layer is separated by heat treatment in the air, washed with an alkaline lithium compound solution in an aqueous solution, spray dried and annealed to achieve lithium precursor supplementation and particle control, avoiding acid extraction and neutralization processes, and reducing process costs. .
It realizes the reuse of environmentally friendly lithium secondary battery cathode active materials, reduces process costs, ensures good performance of resistance and capacity characteristics, and avoids the decline of electrochemical performance.
Smart Images

Figure CN115136387B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for recycling resources in the manufacturing process of lithium secondary batteries. More specifically, the present disclosure relates to a method for collecting and recycling positive electrode waste generated in the manufacturing process of lithium secondary batteries or positive electrode active materials of lithium secondary batteries discarded after use. This application claims the benefit of Korean Patent Application No. 10-2020-0079624 filed with the Korean Intellectual Property Office on June 29, 2020, the disclosure of which is incorporated herein by reference in its entirety. Background Art
[0002] Rechargeable lithium secondary batteries are gaining attention as an alternative to fossil energy. Such lithium secondary batteries are mainly used in traditional handheld devices such as mobile phones, cameras, and power tools. Recently, the scope of application tends to be gradually expanded to vehicles driven by electricity (EV, HEV, PHEV), large-capacity energy storage systems (ESS), and uninterruptible power supply systems (UPS).
[0003] A lithium secondary battery comprises: an electrode assembly, the electrode assembly comprising a unit cell, each unit cell comprising a positive plate and a negative plate, the positive plate and the negative plate comprising a current collector and an active material coated on the current collector, a separator being interposed between the positive plate and the negative plate; and a package or battery case, in which the electrode assembly is airtightly received together with an electrolyte solution. Lithium secondary batteries mainly include lithium-based oxides as positive electrode active materials and carbon-based materials as negative electrode active materials. Lithium-based oxides contain metals such as cobalt, nickel or manganese. In particular, cobalt, nickel and manganese are very expensive precious metals. Among them, cobalt is a strategic metal, and its supply is the focus of worldwide attention. Due to the limited number of cobalt producing countries, the global supply of cobalt is unstable. When the supply and demand of strategic metals are unbalanced, the cost of raw materials is likely to rise.
[0004] Research has been conducted on collecting and recovering precious metals from lithium secondary batteries (waste batteries) discarded after expiration. In addition to waste batteries, it is more preferable to collect resources from waste materials discarded after positive plates are punched out, or from positive plates that have defects or failures in the process.
[0005] Currently, if Figure 1 As shown in FIG, a lithium secondary battery is manufactured by coating a positive electrode slurry including a positive electrode active material, a conductive material, a binder and a solvent on a long sheet type positive electrode collector 10 (such as an aluminum (Al) foil) to form a positive electrode active material layer 20, manufacturing a positive electrode sheet 30, and punching out a positive electrode plate 40 in a predetermined size. The remainder after punching is discarded as a positive electrode waste 50. If the positive electrode active material is collected and reused from the positive electrode waste 50, it will be very ideal in terms of industrial economy and environment.
[0006] Most of the existing methods for collecting positive active materials include dissolving the positive electrode with hydrochloric acid, sulfuric acid, nitric acid, etc., extracting active material elements such as cobalt, nickel, and manganese, and using them as raw materials for the synthesis of positive active materials. However, the use of acid to extract active material elements adopts a non-environmentally friendly process to collect pure raw materials, and requires a neutralization process and a wastewater treatment process, resulting in an increase in process costs. In addition, such a process is unlikely to collect lithium (one of the key positive active material elements). In order to overcome these shortcomings, a direct recycling method that does not dissolve the positive active material and does not extract the active material in elemental form is needed.
[0007] Meanwhile, the positive electrode sheet 30 is usually subjected to roller pressing. Therefore, in the case of the positive electrode waste from the electrode, the particles on the surface may crack or disintegrate when pressed by means of the roller pressing process. The unused fresh active material has no particle cracking or disintegration, but in the case of the reusable active material obtained from the roller pressed electrode, as more and more particles are cracked or disintegrated by roller pressing, the specific surface area of the active material increases, which affects the slurry properties, electrode adhesion and electrode performance during reuse. Accordingly, it is necessary to solve this problem. Summary of the invention
[0008] Technical issues
[0009] The present disclosure is directed to providing a method for collecting and reusing active materials from cathode waste.
[0010] Technical Solution
[0011] In order to solve the above problems, the method for recycling positive electrode active materials disclosed in the present invention includes: (a) heat treating positive electrode waste including a lithium composite transition metal oxide positive electrode active material layer located on a current collector in air to thermally decompose the binder and the conductive material in the active material layer so as to separate the current collector from the active material layer and collect the active material in the active material layer; (b-1) washing the collected active material with a lithium compound solution that is alkaline in aqueous solution; (b-2) mixing the washed active material with a lithium precursor solution and spray drying it to obtain an active material with particle control by adding a lithium precursor; and (c) annealing the spray-dried active material to obtain a reusable active material.
[0012] In the present disclosure, the step (b-2) includes coating the lithium precursor on the surface of the active material, and the step (c) includes annealing without adding additional lithium precursor.
[0013] In the present disclosure, the temperature of the spray drying step may be 100°C to 300°C.
[0014] In the present disclosure, the method for recycling positive electrode active materials may further include: (d) performing surface coating on the annealed active material.
[0015] The heat treatment may be performed at 300°C to 650°C.
[0016] The heat treatment may be performed at 550° C. for 30 minutes with a temperature rise rate of 5° C. / minute.
[0017] The content of the lithium compound (preferably LiOH) in the lithium compound solution is greater than 0% and less than 15%. The washing may be performed within 1 hour.
[0018] The washing may be performed by stirring the collected active material while being immersed in the lithium compound solution.
[0019] The lithium precursor may be at least one of LiOH, Li2CO3, LiNO3 and Li2O.
[0020] The amount of the lithium precursor added may be used to add lithium to the ratio between lithium and other metals in the raw active material used in the active material layer at a ratio of lost lithium.
[0021] For example, the lithium precursor may be added in an amount to add lithium at a molar ratio of 0.001 to 0.4.
[0022] Furthermore, the amount of the lithium precursor added is preferably for adding more lithium in a molar ratio of 0.0001 to 0.1 based on a molar ratio of lithium:other metals of 1:1.
[0023] The annealing may be performed at 400° C. to 1000° C. in air.
[0024] The temperature of the annealing step may exceed the melting point of the lithium precursor.
[0025] The active material in the active material layer may be collected in a powder form, and carbon generated by carbonization of the binder or the conductive material may not remain on the surface.
[0026] The surface coating step may include coating at least one of a metal, an organic metal, and a carbon material on the surface through a solid phase or liquid phase treatment, and performing a heat treatment at 100° C. to 1200° C.
[0027] The recyclable active material may be represented by the following Formula 1:
[0028] [Formula 1]
[0029] Li a Ni x Mny Co z M w O 2+δ
[0030] wherein M comprises at least one selected from the group consisting of B, W, Al, Ti and Mg, <a≤1.1,0≤x<0.95,0≤y<0.8,0≤z<1.0,0≤w≤0.1,-0.02≤δ≤0.02,x+y+z+w=1。
[0031] The reusable active material may have a fluorine (F) content of 150 ppm or less.
[0032] Beneficial Effects
[0033] According to the present disclosure, it is possible to reuse discarded positive electrode active materials (such as positive electrode waste generated in the lithium secondary battery manufacturing process) without using acid, thereby achieving environmental protection. The method according to the present disclosure does not require a neutralization process or a wastewater treatment process, thereby achieving environmental mitigation and process cost reduction.
[0034] According to the present disclosure, all metal elements of the positive electrode active material can be collected. Since the current collector is not dissolved, the current collector can be collected. The method does not use the extracted active material elements as raw materials for synthesizing the positive electrode active material, but directly uses the active material collected in powder form, thereby achieving economic benefits.
[0035] According to the present disclosure, toxic and explosive solvents such as NMP, DMC, acetone, and methanol are not used, thereby achieving safety, and since simple processes such as heat treatment, washing, and annealing are used, it is easy to manage and suitable for large-scale production.
[0036] According to the present disclosure, good resistance characteristics and capacity characteristics can be ensured without degrading the electrochemical performance of the collected active materials.
[0037] According to the present disclosure, even if the active material to be reused suffers particle cracking or disintegration due to roller pressing in the previous process, it can be re-granulated by spray drying, thereby improving the particle size and specific surface area.
[0038] Furthermore, when the washed active material is mixed with a lithium precursor solution and spray-dried, it is possible to re-granulate and replenish the lithium precursor at the same time, thereby simplifying the process and achieving a process continuous with the previous washing step. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings illustrate embodiments of the present disclosure and, together with the following detailed description, help to further understand the technical aspects of the present disclosure. Therefore, the present disclosure should not be interpreted as being limited to the drawings.
[0040] Figure 1 The figure shows the positive electrode scraps discarded after punching out the positive electrode plates in the positive electrode sheets.
[0041] Figure 2 is a flow chart of an active material recycling method according to the present disclosure.
[0042] Figure 3 It is shown Figure 2 Figure 2 shows a schematic diagram of the spray drying step in FIG.
[0043] Figure 4 is a graph of particle size distribution of sample active materials.
[0044] Figure 5 The results of battery evaluation using the sample active materials are shown.
[0045] Figure 6 and Figure 7 The results of battery evaluation using the active materials of Examples and Comparative Examples are shown. DETAILED DESCRIPTION
[0046] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. Before the description, it should be understood that the terms or words used in the specification and the appended claims should not be interpreted as being limited to the general and dictionary meanings, but are interpreted according to the meanings and concepts corresponding to the technical aspects of the present disclosure based on the principle that the inventor is allowed to appropriately define the terms to obtain the best interpretation. Therefore, the embodiments described herein and the illustrations in the drawings are only examples and do not fully describe the technical aspects of the present disclosure, so it should be understood that various other equivalents and modifications may be made to them when filing a patent application.
[0047] In the following description, reference is made to the accompanying drawings which form a part of the present disclosure. The embodiments described in the detailed description, drawings, and appended claims are not intended to be limiting. Other embodiments may be used, and modifications and changes may be made thereto, without departing from the technical aspects and scope of the subject matter disclosed herein. As generally described herein and illustrated in the accompanying drawings, aspects of the present disclosure may include arrangements, substitutions, combinations, separations, and designs of various different elements, and it will be immediately understood that all such elements are expressly contemplated.
[0048] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs (hereinafter referred to as "person skilled in the art").
[0049] The present disclosure is not limited to the specific embodiments described herein. It is obvious to those skilled in the art that many variations and changes may be made to the present disclosure without departing from the technical aspects and scope of the present disclosure. It is obvious to those skilled in the art that functionally equivalent methods within the scope of the present disclosure are apparent from the foregoing description, in addition to those methods listed herein. Such variations and changes fall within the scope of the appended claims. The scope of all equivalents to which the present disclosure and the appended claims are entitled will be defined by the appended claims. It should be understood that the present disclosure is not limited to specific variant methods. It should be further understood that the terms used herein are intended to describe specific embodiments, rather than to limit the present disclosure.
[0050] The traditional active material recycling process is mainly to extract the valuable metal (nickel, cobalt, manganese) elements in the lithium secondary battery active materials whose performance has deteriorated after use, and resynthesize the active materials. Compared with the traditional process, the feature of the present invention is to collect active materials from the positive electrode waste generated in the lithium secondary battery manufacturing process.
[0051] In addition, well-known active material recycling processes involve producing metals (direct reduction method) or resynthesizing active materials from valuable metals extracted by acid / base dissolution or melted using reducing agents / additives, which requires additional chemical methods, complicates the process, and causes additional economic expenditure. However, the present disclosure relates to a method for directly recycling positive electrode active materials without dissolving the positive electrode active materials.
[0052] In order to directly reuse the positive electrode active material, it is necessary to remove the current collector from the positive electrode. The current collector can be removed from the positive electrode by high temperature heat treatment to remove the binder, using a solvent to melt the binder, melting the current collector, and screening the active material by dry grinding and sieving.
[0053] When a solvent is used to melt the binder, the stability of the solvent is important. NMP is the most effective solvent, but its disadvantages are toxicity and high cost. Another disadvantage is that a waste solvent reprocessing or solvent collection process must be performed. The process cost required to melt the current collector is lower than that of using a solvent. However, it is difficult to remove impurities from the surface of the reusable active material, and hydrogen is produced in the process of removing the current collector, posing a risk of explosion. Dry grinding and screening cannot perfectly separate the current collector and active material. The particle size distribution of the active material changes during the grinding process, and it is difficult to remove the binder, resulting in a decrease in the characteristics of the battery including the reusable active material.
[0054] The present disclosure uses high temperature heat treatment to separate the active material from the current collector. In particular, the heat treatment is carried out in air, so the process only requires heating without any special device configuration, and is therefore relatively simple and suitable for large-scale production and commercialization. However, impurities should not remain on the surface of the reusable active material. The present disclosure proposes to remove impurities from the surface of the reusable active material.
[0055] In the following, reference will be made to Figure 2 An active material recycling method according to one embodiment of the present disclosure is described. Figure 2 is a flow chart of an active material recycling method according to the present disclosure.
[0056] refer to Figure 2 , first, discarded positive electrode waste is prepared ( S10 ).
[0057] As mentioned above Figure 1 The positive electrode waste can be what is left after manufacturing a positive electrode sheet including a lithium composite transition metal oxide positive electrode active material layer on a current collector and punching a positive electrode sheet. In addition, the positive electrode waste can be prepared by collecting positive electrodes that have defects or failures during the process. In addition, the positive electrode waste can be prepared by separating positive electrodes from lithium secondary batteries discarded after use.
[0058] For example, the positive electrode waste can be the residue after the following treatment: a slurry is coated on a sheet-type current collector of aluminum foil, and then dried in a vacuum oven at about 120°C to produce a positive electrode sheet, and a positive electrode plate is punched out in a predetermined size, the slurry being prepared by adding N-methylpyrrolidone (NMP) to a lithium cobalt oxide such as LiCoO2 (LCO) as an active material or an NCM-based active material including nickel (Ni), cobalt (Co) and manganese (Mn), carbon such as carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder and mixing.
[0059] The positive electrode active material of the lithium secondary battery includes a lithium composite transition metal oxide, in particular, a lithium cobalt oxide such as LiCoO2, lithium manganate (LiMnO2 or LiMn2O4), a lithium iron phosphate compound (LiFePO4) or lithium nickel oxide (LiNiO2). In addition, in order to improve the low thermal stability while maintaining the excellent reversible capacity of LiNiO2, a nickel-manganese-based lithium composite metal oxide is used, in which nickel (Ni) with excellent thermal stability partially replaces manganese (Mn), and NCM-based lithium composite transition metal oxide is replaced with manganese (Mn) and cobalt (Co). In particular, the present disclosure proposes to reuse NCM-based lithium composite transition metal oxide active materials.
[0060] The positive electrode waste has an active material layer on a current collector of a metal foil such as an aluminum foil. The active material layer is formed by applying a slurry including a mixture of an active material, a conductive material, a binder, and a solvent, and after the solvent is volatilized, the active material and the conductive material are combined with the binder. Therefore, when the binder is removed, the active material can be separated from the current collector.
[0061] Subsequently, the positive electrode waste is crushed to an appropriate size (S20). Crushing refers to cutting or chopping the positive electrode waste into an appropriate size for disposal. After switching or chopping, the size of the positive electrode waste is reduced to, for example, 1 cm×1 cm. Various dry milling equipment can be used for crushing, including hand mills, pin mills, disc mills, cutting mills and hammer mills, as well as high-speed cutters.
[0062] Cutting or shredding can be performed considering the characteristics required by the equipment used in the disposal and subsequent processes of the cathode waste. For example, when equipment that requires continuous processing is used to load and unload cathode waste, it is necessary to break up the oversized cathode waste to facilitate the movement of the cathode waste.
[0063] Subsequently, the cathode waste is heat-treated in air ( S30 ).
[0064] In the present disclosure, the heat treatment is performed to thermally decompose the binder in the active material layer. The heat treatment may be performed at 300°C to 650°C and may be referred to as a high temperature heat treatment. At a temperature below 300°C, it is difficult to remove the binder, making it impossible to separate the current collector, while at a temperature of 650°C or above, the current collector melts (Al melting point: 660°C), making it impossible to separate the current collector.
[0065] The heat treatment time is long enough to cause the binder to thermally decompose. For example, the heat treatment time is about 30 minutes. Preferably, the heat treatment time is more than 30 minutes. As the heat treatment time increases, the thermal decomposition time of the binder will be extended, but when the heat treatment time is equal to or longer than the predetermined time, there is no difference in the thermal decomposition effect. Preferably, the heat treatment time is more than 30 minutes and less than 5 hours.
[0066] The heat treatment equipment may include various types of furnaces. For example, the heat treatment equipment may be a box-type furnace, and in consideration of productivity, may be a rotary kiln capable of continuous treatment.
[0067] After heat treatment, the product can be cooled quickly or slowly in air.
[0068] For example, the heat treatment may be performed at 550°C for 30 minutes at a temperature rise rate of 5°C / minute. For example, the temperature rise rate is within the allowable range of the box furnace and is sufficient to heat the positive electrode waste without generating thermal shock. 550°C is set in consideration of the melting point of the aluminum current collector and for good thermal decomposition of the binder. When the heat treatment is performed at the above temperature for less than 10 minutes, the thermal decomposition is insufficient, so it is necessary to perform the heat treatment for more than 10 minutes, preferably more than 30 minutes.
[0069] Through the heat treatment in air, the CO2 and H2O are removed by thermal decomposition of the binder and the conductive material in the active material layer. Since the binder is removed, the active material can be separated from the current collector, and the active material to be collected can be screened out in the form of powder. Therefore, the current collector can be separated from the active material layer, and the active material in the active material layer can be collected by S30.
[0070] It is important to perform the heat treatment of S30 in air. When heat treated in a reducing or inert gas environment, the binder and the conductive material undergo carbonization rather than thermal decomposition. When carbonized, carbon remains on the surface of the active material and degrades the performance of the reusable active material. When heat treated in air, the carbon in the binder or conductive material is removed by generating CO, CO2 gas through a combustion reaction with oxygen, so the binder and conductive material do not remain and are almost all removed.
[0071] Therefore, according to the present disclosure, the active material is collected in a powder form, and carbon generated by carbonization of the binder or the conductive material does not remain on the surface.
[0072] Subsequently, the collected active material is washed (S40). It is important to wash with a lithium compound solution that is alkaline in aqueous solution. The lithium compound solution contains a lithium compound, preferably LiOH, in an amount of more than 0% and less than 15%. Preferably, the amount of LiOH is less than 15%. When an excess of LiOH is included, the excess LiOH may remain on the surface of the active material after washing, which may affect the subsequent annealing process. In order to make the surface of the active material as clean as possible before annealing, it is not advisable to add excess LiOH, and the amount of LiOH is limited to less than 15%.
[0073] Washing can be carried out by soaking the collected active material in a lithium compound solution. Washing can be carried out within a week (preferably one day, more preferably 1 hour) after soaking. When washing is carried out for a week or longer, the capacity will be reduced due to excessive lithium dissolution. Therefore, it is expected to perform washing within 1 hour. Washing includes soaking the active material in an alkaline lithium compound solution in an aqueous solution and stirring it under soaking. It is expected that soaking and stirring are carried out together. When the active material is soaked in a lithium compound solution without stirring, the washing process is very slow, resulting in lithium dissolution. When stirring is carried out together, the process time is minimized, therefore, it is expected to stir while soaking in a lithium compound solution.
[0074] Washing with a lithium compound solution that is alkaline in an aqueous solution is performed to remove LiF and metal fluorides that may be present on the surface of the collected active material, and surface modification is performed. In the heat treatment process of S30, the binder and the conductive material in the active material layer are removed by evaporation of CO2 and H2O. In this process, CO2 and H2O react with lithium on the surface of the active material to produce Li2CO3 and LiOH, while fluorine (F) (such as PVdF) present in the binder reacts with the metal element of the positive electrode active material to produce LiF or metal fluoride. When LiF or metal fluoride remains, the characteristics of the battery including the reusable active material will decrease. The present disclosure adds a washing step of S40 to remove reactants that may be produced on the surface of the reusable active material in the heat treatment step (S30) to prevent impurities from remaining on the surface of the reusable active material.
[0075] In S40, it is important to wash with a lithium compound solution that is alkaline in aqueous solution. When sulfuric acid or hydrochloric acid aqueous solution is used instead of a lithium compound solution that is alkaline in aqueous solution, F on the surface of the active material is washed away, but the performance of the reusable positive active material may be reduced due to the dissolution of transition metals (Co, Mg) present in the active material. The role of the lithium compound solution that is alkaline in aqueous solution used in the present disclosure is to remove trace amounts of binders that may remain after the thermal decomposition of S30, not to dissolve transition metals present in the active material, and to compensate for the amount of lithium dissolved during the washing process.
[0076] Through S40, the present disclosure can adjust the LiF content on the surface of the collected active material to less than 500ppm, thereby improving the capacity. Preferably, the F content can be 150ppm or less. More preferably, the F content can be 30ppm or less. Washing can remove LiF or metallic lithium compounds formed by decomposition of the binder, thereby improving the resistance characteristics.
[0077] Subsequently, the washed active material is directly mixed with the lithium precursor solution without being dried, and spray-dried ( S45 ).
[0078] Through the previous steps S30 and S40, lithium in the active material may be lost. S45 can compensate for the loss of lithium more simply and reliably.
[0079] The lithium precursor solution includes a lithium compound dissolved in an aqueous solution or an organic solvent. In particular, preferably, the lithium precursor in S45 may be at least one of LiOH, Li2CO3, LiNO3 and Li2O.
[0080] Preferably, the temperature in the spray drying step is 80° C. or more, and when the temperature is equal to or lower than 80° C., the solution may not be completely dried. More preferably, the temperature in the spray drying step may be 100° C. to 300° C.
[0081] When drying is performed in a furnace immediately after surface modification treatment by washing in S40, the active material particles may agglomerate. In order to mix the lithium precursor with the agglomerated particles, it may be necessary to grind the agglomerated particles. In order to mix the lithium precursor in a solid state, a powder mixing or grinding process is required. In this case, the process is complicated and a continuous process cannot be performed. In addition, in the case of NCM-based positive electrode active materials, when powder mixing or grinding is performed with the lithium precursor in a wet state, the positive electrode active material absorbs moisture, resulting in severe agglomeration. Therefore, the present disclosure proposes that after washing in S40, the active material is mixed and dispersed in a lithium precursor solution without drying, and spray drying is performed. Therefore, the agglomeration caused by drying and the difficulties involved in mixing with a solid lithium precursor can be avoided. That is, an active material in a powder state without agglomeration is produced by spray drying.
[0082] In spray drying, the lithium precursor solution is dried immediately after spraying, and the lithium precursor is coated on or in contact with the surface of the active material. In this case, the particles agglomerate under the action of capillary forces, and the lithium precursor solution as a solvent is dried, causing particle adjustment. In the case of positive electrode waste from the electrode, the particles on the surface may crack or disintegrate when pressed by the roller pressing process. In particular, compared with LCO, NCM-based active materials suffer from severe particle cracking caused by roller pressing during electrode manufacturing, and a large number of small particles are present in the collected active material compared with the raw active material used in the active material layer (i.e., unused fresh active material), resulting in uneven particles.
[0083] In particular, the NCM-based active material includes large particles or secondary particles formed by agglomeration of primary particles having a size of tens to hundreds of nanometers, and in the positive electrode manufactured using the active material, the secondary particles can be decomposed into primary particles or microparticles larger than the primary particles but smaller than the large particles during the rolling process to adjust the porosity in the electrode. As the particles cracked or disintegrated by rolling increase, the specific surface area of the active material also increases, and the reusable active material obtained from the rolled electrode may affect the slurry characteristics, electrode adhesion and electrode performance when reused.
[0084] For the reusable level of active materials, it is preferred that the particle size distribution is similar or identical to that of fresh active materials. The proposed spray drying causes smaller particles formed by cracking or disintegration during the rolling process to agglomerate into larger particles, thereby resolving the heterogeneity of the particles and making the particle size similar to the initial characteristics of the fresh active materials. In particular, the particle recovery effect of the present disclosure is outstanding in NCM-based active materials that suffer from severe particle cracking or disintegration due to rolling in the previous process. It is expected that the characteristics of batteries that reuse active materials collected according to the method of the present disclosure will be at a similar level to the characteristics of batteries using fresh active materials.
[0085] As described above, by the spray drying step (S45), the lithium precursor is coated on the surface of the active material, and the active material with particle adjustment is obtained. The lithium precursor addition, granulation and drying are performed in one step, so that the process is simplified. In addition, spray drying is not a means of simply obtaining active materials, but a means of recovering (re-granulating) particles that are cracked or disintegrated due to rolling.
[0086] In addition, since S45 is performed by mixing and dispersing the active material particles washed in S40 in a lithium precursor solution of a predetermined concentration, the washing in S40 and the spray drying in S45 can realize a continuous process. The present disclosure ensures the continuity of the process and simultaneously performs lithium precursor coating, drying and granulation (particle readjustment) in one step.
[0087] Spray drying can be carried out using common spray drying equipment. Figure 3 It is shown Figure 2 Figure 2 shows a schematic diagram of the spray drying step in FIG.
[0088] refer to Figure 3, the lithium precursor aqueous solution 100 is prepared by dissolving LiOH in distilled water, and the washed active material 110 in S40 is mixed and dispersed in the lithium precursor aqueous solution 100 to prepare a mixed solution 120 as shown. The mixed solution 120 can be kept in a stirring state by a magnetic stirrer 125. When the mixed solution 120 is sprayed into a heating container 140 maintained at 100° C. to 300° C. through a nozzle 130 of a spray drying device, agglomeration occurs in the cracked active material particles by removing moisture in droplets 120 'of the mixed solution 120, and the spray-dried active material 120" coated with a lithium precursor on the surface of the active material particles can be obtained from a collection container 150.
[0089] The particle size of the spray-dried active material 120" can be adjusted by adjusting the density of the mixed solution 120, the temperature in the heating container 140, and the size of the droplets 120'. Therefore, through the annealing process described below, the reusable active material obtained according to the present disclosure can have a particle size distribution similar to that of the fresh active material. In this specification, the volume % of particles having the same particle size with a difference within the range of ±2% is defined as a similar particle size distribution.
[0090] The amount of lithium precursor added is used to add lithium to the ratio between lithium and other metals in the raw material active material (i.e., fresh active material) used in the active material layer at the ratio of lithium loss. For example, when the ratio between lithium and other metals in the fresh active material is 1, the amount of lithium precursor added can be used to add lithium at a molar ratio of 0.001 to 0.4. It is suitable to add lithium at a molar ratio of 0.01 to 0.2. The addition of lithium precursor exceeds the lithium lost by washing, resulting in unreacted lithium precursor left on the reusable active material, so that the resistance during the active material reuse process increases, so it is necessary to supply lithium precursor in an appropriate amount.
[0091] In addition, based on a molar ratio of lithium: other metals of 1: 1, the amount of lithium precursor added is preferably used to add more lithium at a molar ratio of 0.0001 to 0.1. Excess lithium is added to form a surface protective layer on the active material by surface coating, which will be described in detail below. When a secondary battery is manufactured using an active material, side reactions can be suppressed and life characteristics can be maintained with the help of an electrolyte solution.
[0092] Subsequently, the spray-dried active material is annealed ( S50 ).
[0093] Since the lithium precursor is added to the active material in S45, annealing can be performed in this step without adding additional lithium precursor.
[0094] In S50 , the crystal structure of the active material is restored by annealing, and thus the properties of the reusable active material can be restored or improved to the level of fresh active material.
[0095] After the previous steps S30 and S40, structural transformation can be found in the surface of the active material. For example, the NCM-based lithium composite transition metal oxide as an active material may have a spinel structure, which is due to the conversion of nickel into rock salt [NiCO3·2Ni(OH)2)H20] when it is damp in S40. When the battery is manufactured in this state, the characteristics of the battery may decrease, such as a decrease in capacity. The present disclosure restores the crystal structure with the help of S50. For example, the NCM-based lithium composite transition metal oxide as an active material is restored to a hexagonal structure. Therefore, the initial characteristics can be restored or improved to a level similar to that of the fresh active material.
[0096] In addition, in the case of LCO active materials, Co3O4 may be generated on the surface by thermal decomposition. When a battery is manufactured without removing Co3O4, the characteristics of the battery may be degraded. The present disclosure can restore or improve the initial characteristics to a level similar to that of a fresh active material by restoring the crystal structure and removing Co3O4 through S50.
[0097] Annealing can be performed at 400°C to 1000°C in air. The annealing temperature can be 600°C to 900°C. The temperature varies within a limited range, depending on the type of lithium precursor. The annealing time can be at least 1 hour. Preferably, the annealing time is about 5 hours. When the annealing time is long, the crystal structure may be fully restored, but long-term annealing does not have a great effect on the performance. For example, the annealing time is about 15 hours or less. The annealing equipment can be similar to or the same as the equipment of the heat treatment step S30.
[0098] For example, when Li2CO3 is used as a lithium precursor, the annealing temperature is preferably 700°C to 900°C, more preferably 710°C to 780°C. This is because the melting point of Li2CO3 is 723°C. Most preferably, annealing is performed at 750°C. When LiOH is used as a lithium precursor, the annealing temperature is preferably 400°C to 600°C, more preferably 450°C to 480°C. This is because the melting point of LiOH is 462°C.
[0099] Preferably, the annealing temperature is higher than the melting point of the lithium precursor. However, at a temperature higher than 1000°C, the positive electrode active material will undergo thermal decomposition and the performance of the active material will be reduced, so the annealing temperature should not exceed 1000°C.
[0100] Through S50, recyclable active materials can be obtained.
[0101] Optionally, S60 may be performed. In S60, the active material annealed in S50 is surface-coated.
[0102] The surface coating step may include coating at least one of a metal, an organic metal, and a carbon material on the surface by solid phase or liquid phase treatment, and heat treating at 100° C. to 1200° C. When heat treating at a temperature higher than 1200° C., performance degradation may occur due to thermal decomposition of the positive electrode active material. In the surface coating process, coating on the surface by solid phase or liquid phase treatment may use mixing, milling, spray drying, and grinding.
[0103] By surface coating, a surface protective layer of different metals is formed. In the case where the molar ratio of lithium in the positive electrode active material: other metals is 1: 1, when the molar ratio of lithium in the positive electrode active material: other metals is reduced to less than 1: 1 due to the reaction of lithium in the active material with the surface coating material, 100% capacity cannot be exhibited. Therefore, an excess of lithium is added to compensate for the lithium loss in the previous step S45, so that the molar ratio of lithium in the positive electrode active material: other metals is 1: 1, and more lithium is included in the positive electrode active material at a molar ratio of 0.0001 to 0.1 with other metals. Therefore, a surface protective layer can be formed so that the molar ratio of lithium in the positive electrode active material: other metals in the surface coating is 1: 1.
[0104] In detail, when the active material is coated with a metal oxide such as B, W, BW and the like and subjected to heat treatment, a lithium boron oxide layer may be formed on the surface of the active material and used as a surface protective layer. The lithium additionally included at a molar ratio of 0.0001 to 0.1 in S45 reacts with the metal oxide such as B, W, BW and the like in S60, and the molar ratio of lithium: other metals in the positive electrode active material does not decrease to less than 1:1, so that the capacity does not decrease.
[0105] The recyclable active material obtained by the above method can be represented by Formula 1.
[0106] [Formula 1]
[0107] Li a Ni x Mn y Co z M w O 2+δ
[0108] wherein M comprises at least one selected from the group consisting of B, W, Al, Ti and Mg, <a≤1.1,0≤x<0.95,0≤y<0.8,0≤z<1.0,0≤w≤0.1,-0.02≤δ≤0.02,x+y+z+w=1。
[0109] The F content of the recyclable active material may be 100 ppm or less. According to the present disclosure, an active material having a reduced F content may be collected, and when reused as an active material, may provide excellent resistance characteristics and capacity characteristics.
[0110] According to the present disclosure, LiF or metal fluoride is removed in the washing step of S40. Correction of particle non-uniformity by lithium precursor addition and particle adjustment is achieved in the spray drying of S45. Co3O4 is removed in the annealing of S50. The step of washing with a lithium compound solution that is alkaline in an aqueous solution is safe and low-cost, and can remove LiF or metal fluoride without losing other elements, prevent the dissolution of transition metals, and thus compensate for the lithium loss that occurs in this process without affecting the structure of the positive electrode. Spray drying can implement a process continuous with the previous washing step, and add a lithium precursor by a simple method, and help to have a particle size similar to that of a fresh active material. The annealing step is also safe and low-cost, and can effectively remove Co3O4 and restore the crystal structure (i.e., improve crystallinity), thereby improving the battery characteristics of the reusable active material.
[0111] Since carbon generated by carbonization of the binder or conductive material does not remain on the surface, no carbon removal step is required. Figure 2 The active material obtained by the method can be used to manufacture the positive electrode without any treatment.
[0112] The recycled active material may be used 100% without composition adjustment or may be mixed with fresh active material and may be used to prepare a slurry together with a conductive material, a binder, and a solvent.
[0113] Hereinafter, experimental examples of the present disclosure will be described in detail.
[0114] <Experimental Example>
[0115] The experiments were mainly divided into two categories: the first category was experiments related to the spray drying of S45, and the second category was experiments for verifying the effect of the method according to the present disclosure on NCM-based active materials.
[0116] The following is an experiment of the first type. The evaluation was conducted after the positive electrode active material was prepared as follows.
[0117] (Sample #1) Sample #1 is fresh positive electrode active material.
[0118] (Sample #2) Sample #2 is a positive electrode active material from which a binder and a conductive material are removed by S30 according to the present disclosure. Sample #2 is obtained by applying heat at 550° C. for 30 minutes to the positive electrode scrap to thermally decompose the binder and the conductive material.
[0119] (Sample #3) Sample #3 was obtained by washing Sample #2 according to S40 of the present disclosure, drying by a common method, mixing with 0.1 mol of LiOH powder as a lithium precursor, and heat-treating at 750° C. for 5 hours in S50 of the present disclosure.
[0120] (Sample #4) Sample #4 is a reusable active material manufactured according to the present disclosure. As in Sample #2, after performing S30, S40, S45, and S50 were performed. In S45, the (washed electrode) that was not dried after washing in S40 was mixed with an aqueous solution and 0.1 mol LiOH powder (ratio of powder: aqueous solution = 1:50), and used Figure 3 Granulation was performed using the spray drying apparatus shown in . S50 was performed as in sample #3 at 750°C for 5 hours.
[0121] In S45, the mixed solution of the washed electrode and 0.1 mol LiOH is stirred to prevent electrode precipitation, and is controlled so that the atmospheric temperature (input temperature) when sprayed onto the heating container 140 using the nozzle 130 in the spray drying equipment is 180°C, and the atmospheric temperature (output temperature) when leaving the heating container 140 to the collection container 150 is 100°C or above.
[0122] Figure 4 is a particle size distribution diagram of the sample active material. The particle size distribution can be obtained using a particle size analyzer commonly used in laboratories. For example, it can be measured using a Horiba LA 950V2 particle size analyzer. There is no difference depending on the measuring device or method. Figure 4 In the graph, the horizontal axis represents the particle size (μm) and the vertical axis represents volume %.
[0123] In the case of sample #2, it was found that the active material of sample #1 was decomposed into submicron-sized (less than 1 micron) particles by the pressure applied in the electrode process. The particle size distribution of sample #2 was very different from that of sample #1.
[0124] Since Sample #3 and Sample #4 are subjected to annealing, the previously added lithium precursor melts, inducing particle agglomeration during the annealing process, and therefore it can be seen that the number of small particles is less than that of Sample #2. In particular, Sample #4 according to the present disclosure has a smaller amount of small particles and a slightly larger amount of large particles than Sample #3, but there is no big difference in particle size distribution, and from the perspective of a smaller amount of small particles, the particle size distribution of Sample #4 is closer to the particle size of Sample #1 than Sample #3.
[0125] Using the proposed spray drying (sample #4), the particle size distribution is more similar to the fresh active material (sample #1) than the mixed solid lithium precursor (sample #3), and in particular enables a process continuous with a washing step before spray drying.
[0126] The electrochemical performance was evaluated using sample active materials. 96.25wt% of the sample active material, 1.5wt% of carbon black as a conductive material and 2.25wt% of PVdF as a binder were measured and mixed with NMP to prepare a slurry, a positive electrode was made, a battery (Coin Half Cell, CHC) was manufactured and the electrochemical performance was evaluated. At different currents, the capacity as a function of the number of cycles was evaluated to determine the rate performance. The equipment used for evaluation is a charge / discharge tester commonly used in laboratories. There is no difference depending on the measuring device or method.
[0127] Figure 5 The results of battery evaluation using the sample active materials are shown, and Table 1 summarizes the result values. Figure 5 In the graph, the horizontal axis represents the cycle and the vertical axis represents the capacity. The voltage is 3 to 4.3 V, and the initial charge / discharge is performed at 0.1C / 0.1C. The electrolyte solution of the battery is a carbonate-based electrolyte solution, and includes ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3:7, and additives are added.
[0128] [Table 1]
[0129]
[0130] refer to Figure 5 As shown in Table 1, the electrodes using sample #3 and sample #4 both showed similar levels of results to the electrode using sample #1. Sample #1 showed a high initial formation capacity, and sample #3 and sample #4 showed slightly higher C rate capabilities, but they were determined to be at similar levels. According to the present disclosure (sample #4), it is possible to obtain a reusable active material at a similar level to that of fresh active material (sample #1), especially compared to adding a solid lithium precursor (sample #3), and a process continuous with the washing step before spray drying can be implemented.
[0131] Next is the second type of experiment.
[0132] As described below, electrochemical performance was evaluated using each positive electrode active material prepared by the methods of Examples and Comparative Examples.
[0133] Example 1: Reusable active materials are collected by means of the active material recycling method of the present disclosure described above. The positive electrode waste discarded after punching out the positive electrode plate with NCM-based lithium composite transition metal oxide as the active material was prepared, and the heat treatment of S30 was performed at 550°C for 30 minutes. S40 was washed with LiOH for 10 minutes. As described above, S45 was performed using spray drying equipment conditions. In particular, in this experiment, in S45, based on the molar ratio of lithium and other metals in the raw active material (inductively coupled plasma (ICP) analysis), a lithium precursor (Li2CO3) was fed into this process, and the addition amount was to add more lithium at a molar ratio of 0.09. S50 was performed by annealing at 750°C for 15 hours. Theoretically, in the case of fresh active materials, the molar ratio of lithium: other metals is 1: 1, but since the average error of the ICP equipment for measuring the molar ratio is ± 0.05 (preferably about ± 0.02), the molar ratio of lithium: other metals in the raw active material measured by ICP may be 1 ± 0.05: 1. In this experiment, the lithium precursor was added based on the analytical ratio analyzed by ICP.
[0134] Example 2: Based on Example 1, an active material surface protection layer recovery process of S60 is performed.
[0135] Comparative Example 1: Using fresh NCM-based lithium composite transition metal oxide instead of using recycled active materials.
[0136] Comparative Example 2: Only the heat treatment of S30 in the above-mentioned active material recycling method of the present invention is performed to remove the binder and the conductive material, separate the Al current collector, and collect the NCM-based lithium composite transition metal oxide active material. S30 is performed under the same conditions as Example 1. The steps after S40 in the active material recycling method of the present invention are not performed.
[0137] Comparative Example 3: On the basis of Comparative Example 2, active materials were collected by performing the active material recycling method of the present disclosure until the surface modification of S40. That is, the surface modification was performed, but the steps after S45 in the active material recycling method of the present disclosure were not performed. S40 was performed under the same conditions as in Example 1.
[0138] Comparative Example 4: Based on Comparative Example 2, the active material recycling method of the present disclosure was performed until the crystal structure of S50 was restored without performing surface modification of S45 and S40. It should be noted that annealing was performed to restore the crystal structure, but no lithium precursor was added.
[0139] Comparative Example 5: The active material recycling method was performed in the same manner as in Example 1, only up to S30, S40 and S50. It should be noted that annealing was performed to restore the crystal structure, but no lithium precursor was added. ICP analysis was performed on the positive electrode active material collected or prepared in each of the examples and comparative examples to analyze the amount of residual LiF, the ratio of lithium and other metals in the active material, and the amount of specific elements such as B or W.
[0140] Furthermore, the electrochemical performance of the battery manufactured using the positive electrode active material collected or prepared in each of the Examples and Comparative Examples was evaluated in the same manner as in the aforementioned experiments.
[0141] In order to determine the amount of LiF remaining in the active materials collected in Comparative Examples 2 and 3, F detection and analysis were performed using ICP. The results are shown in Table 2 below.
[0142] [Table 2]
[0143] Comparative Example 2 Comparative Example 3 F content (mg / kg) 1450 ND
[0144] ND means 30 ppm or less was measured. Referring to Table 2, it was found that the F content in the collected positive electrode active material was significantly reduced in Comparative Example 3 compared with Comparative Example 2. That is, it can be seen that LiF was completely dissolved in the lithium compound solution by washing, and thus was completely removed, so that it could not be detected by ICP. Therefore, it can be seen that S40 has a very good removal effect on LiF.
[0145] In order to identify whether the lithium in the positive electrode active material changes during S30 and S40 of the present disclosure, the ratio of lithium / other metals in the active material was analyzed by ICP. The results are shown in Table 3 below.
[0146] [Table 3]
[0147]
[0148] Referring to Table 3, it can be seen that, compared with Comparative Example 1, Comparative Example 2 has a lithium / other metal ratio reduced by about 0.2 to 0.5 through the heat treatment of S30, and compared with Comparative Example 2, Comparative Example 3 has a lithium / other metal ratio reduced by about 0.2 to 0.5 through the washing and drying of S40. It seems that the ratio of lithium to other metals in the NCM-based lithium composite transition metal oxide is significantly reduced due to the relatively large specific surface area of the particles and the conversion to the spinel structure. Therefore, it can be seen that it is necessary to compensate for the insufficient lithium.
[0149] Table 3 shows the values measured by ICP analysis, and as described above, the error value of ICP analysis is about ±0.02. Therefore, in Comparative Example 1 of the fresh active material, the ratio of lithium to other metals may be less than 1. Therefore, the amount of lithium precursor added to compensate for the loss of lithium is the amount of lithium reduced based on the ratio of lithium to other metals in the raw material active material (i.e., fresh active material) used in the active material layer (i.e., the molar ratio by ICP analysis).
[0150] Figure 6 and Figure 7 The results of battery evaluation using the active materials of Examples and Comparative Examples are shown.
[0151] First, refer to Figure 6 , in the case where Comparative Example 2 before surface modification and Comparative Example 3 after surface modification were subjected to a heat treatment (550°C / 30 minutes) for desorption, the surface-modified Comparative Example 3 showed a rapid decrease in electrode capacity. This is because, as mentioned above, the nickel in the NCM-based lithium composite transition metal oxide is converted into rock salt after being exposed to moisture, resulting in a decrease in capacity.
[0152] However, when annealing (750°C / 15 hours) was performed without surface modification, which corresponds to Comparative Example 4, the effect of capacity improvement was small compared with Comparative Example 2. This is due to the residual LiF on the surface of the active material when surface modification was not performed. As shown in Table 1 above, the degree of removal of LiF by washing was satisfactory.
[0153] When surface modification and annealing were performed after the primary heat treatment, the capacity increased as shown in Comparative Example 5. The reason is that, although the capacity decreased after surface modification as shown in Comparative Example 3, after LiF was removed by surface modification, Ni rock salt was reduced by annealing and its structure returned to a hexagonal shape.
[0154] Then, refer to Figure 7 , it is found that the capacity of Example 1 is improved compared with Comparative Example 5. Compared with Comparative Example 5, Example 1 realizes the addition of lithium precursor and particle adjustment by spray drying. It can be seen that the capacity is improved by adding lithium precursor to compensate for the lithium lost in the previous step. Reference Table 3 describes the lithium lost by heat treatment and washing.
[0155] Based on the results of ICP analysis (Table 3), lithium compounds were added at a ratio of lithium loss to the existing lithium content in the positive electrode active material. As can be seen from additional experiments, addition at a molar ratio of 0.09 to 0.1 showed a capacity improvement effect comparable to Comparative Example 1.
[0156] According to the present disclosure, active materials can be collected from cathode waste at a directly usable level. Since no toxic and explosive solvents such as NMP, DMC, acetone and methanol are used, and since simple and safe processes such as heat treatment, washing and drying, and annealing are adopted, it is safe and suitable for large-scale production.
[0157] The amount of specific elements was analyzed by ICP analysis of the positive electrode active material collected or prepared in each Example and Comparative Example. The results are shown in Table 4 below.
[0158] [Table 4]
[0159] B content (mg / kg) W content (mg / kg) Comparative Example 1 500 3100 Comparative Example 2 200 2700 Comparative Example 3 ND 200 Comparative Example 5 ND 200 Example 1 ND 200
[0160] As seen in Comparative Example 1, the fresh active material used in this experiment further includes B and W. In the case of Comparative Example 2, it can be seen that the contents of B and W are reduced by heat treatment, and the results of the remaining Comparative Examples reveal that B is almost completely removed in the subsequent process. In the case of W, it can be seen that a large amount of W is removed by washing in the surface modification process (as in Comparative Example 3).
[0161] Therefore, depending on the type of active material initially used, some may be susceptible to heat and moisture, so specific elements may be lost in this process, especially in the surface modification process, which may be completely removed or have a small amount of residue by washing, and in some cases, by performing the active material recycling method until annealing (as in Example 1), it may not be possible to fully restore its characteristics. In this case, it is expected that an additional surface coating step is performed as proposed. In this experimental embodiment, the surface coating step includes coating with B and W. Surface coating can serve as a surface protective layer for the positive electrode active material. Surface coating can be a process for compensating for insufficient specific elements while restoring the surface protective layer in the fresh active material. In the case of the fresh active material used in this experiment, the surface protective layer includes BW, and the loss of lithium in this process is interpreted as the ratio of (lithium in the active material itself + lithium used to form the surface protective layer): other metals, rather than the ratio of lithium in the active material itself to other metals being 1:1. Therefore, in the above experiment, the molar ratio of lithium lost in Comparative Example 3 is 0.09, which can be explained as the sum of lithium in the positive electrode active material and lithium used to form the surface protection layer. In this embodiment, the amount of lithium precursor added is to supplement lithium.
[0162] The surface coating step is subjected to a heat treatment process after a solid phase or liquid phase reaction.
[0163] When the recyclable active material is represented by the following Formula 1,
[0164] [Formula 1]
[0165] Li a Ni x Mn y Co z M w O 2+δ
[0166] wherein M comprises at least one selected from the group consisting of B, W, Al, Ti and Mg, <a≤1.1,0≤x<0.95,0≤y<0.8,0≤z<1.0,0≤w≤0.1,-0.02≤δ≤0.02,x+y+z+w=1。
[0167] It can be considered that M in Formula 1 is supplemented by surface coating.
[0168] When the surface coating layer includes B, BW, B-Ti, BW-Ti, the surface coating heat treatment can be performed at a temperature of 200°C to 500°C, and other metal materials, carbon materials and organic metal materials are used for coating at a temperature between 100°C and 1200°C.
[0169] According to the present disclosure, cathode waste can be recycled using a simple, environmentally friendly, and economical method, and a lithium secondary battery manufactured by recycling the prepared NCM-based lithium composite transition metal oxide cathode active material does not have problems with battery performance.
[0170] Although the present disclosure has been described herein with respect to limited embodiments and drawings, the present disclosure is not limited thereto, and it will be apparent to those skilled in the art that various modifications and changes may be made thereto within the technical aspects of the present disclosure and the scope of the appended claims and their equivalents.
Claims
1. A method for recycling positive electrode active materials, the method comprising the following steps: (a) heat-treating a positive electrode waste including a lithium composite transition metal oxide positive electrode active material layer on a current collector in air to thermally decompose a fluorine-containing binder and a conductive material in the active material layer, so as to separate the current collector from the active material layer, and collecting active materials in the active material layer; (b-1) washing the collected active material with a basic lithium compound solution in aqueous solution; (b-2) mixing the washed active material with a lithium precursor solution and spray drying to obtain an active material with particle control by adding a lithium precursor; as well as (c) Annealing the spray-dried active material to obtain a reusable active material.
2. The method for recycling positive electrode active materials according to claim 1, wherein: The step (b-2) includes coating the lithium precursor on the surface of the active material, and the step (c) includes annealing without adding additional lithium precursor.
3. The method for recycling positive electrode active materials according to claim 1, wherein: The spray drying temperature is 100°C to 300°C.
4. The method for recycling positive electrode active materials according to claim 1, further comprising the following steps: (d) Surface coating is performed on the annealed active material to form a surface protective layer of a different metal.
5. The method for recycling positive electrode active materials according to claim 1, wherein: The heat treatment is performed at 300°C to 650°C.
6. The method for recycling positive electrode active materials according to claim 1, wherein: The content of the lithium compound in the lithium compound solution is at most 15%, and the washing is performed within 1 hour.
7. The method for recycling positive electrode active materials according to claim 1, wherein: The washing is performed by stirring the collected active material while being immersed in the lithium compound solution.
8. The method for recycling positive electrode active materials according to claim 1, wherein: The lithium precursor is at least one of LiOH, Li2CO3, LiNO3 and Li2O.
9. The method for recycling positive electrode active materials according to claim 1, wherein: The amount of the lithium precursor added is for adding lithium to the ratio between lithium and other metals in the raw material active material used in the active material layer at a ratio of lost lithium.
10. The method for recycling positive electrode active materials according to claim 9, wherein: The lithium precursor is added in an amount for adding lithium at a molar ratio of 0.001 to 0.
4.
11. The method for recycling positive electrode active materials according to claim 9, wherein: Based on a molar ratio of lithium to other metals of 1:1, the added amount of the lithium precursor is used to add more lithium at a molar ratio of 0.0001 to 0.
1.
12. The method for recycling positive electrode active materials according to claim 1, wherein: The annealing is performed at 400° C. to 1000° C. in air.
13. The method for recycling positive electrode active materials according to claim 1, wherein: The annealing temperature exceeds the melting point of the lithium precursor.
14. The method for recycling positive electrode active materials according to claim 1, wherein: The active material in the active material layer is collected in a powder form, and carbon generated by carbonization of the binder or the conductive material does not remain on the surface.
15. The method for recycling positive electrode active materials according to claim 4, wherein: The surface coating includes coating at least one of a metal, an organic metal, and a carbon material on the surface through a solid phase or liquid phase treatment, and then performing a heat treatment at 100° C. to 1200° C.
16. The method for recycling positive electrode active materials according to claim 1, wherein: The recyclable active material is represented by the following formula 1: [Formula 1] Li a Ni x Mr y Co z M w O 2+δ wherein M comprises at least one selected from the group consisting of B, W, Al, Ti and Mg, <a≤1.1,0≤x<0.95,0≤y<0.8,0≤z<1.0,0≤w≤0.1,-0.02≤δ≤0.02,x+y+z+w=1。 17. The method for recycling positive electrode active materials according to claim 1, wherein: The reusable active material has a fluorine (F) content of 150 ppm or less.
Citation Information
Patent Citations
Apparatus for manufacturing of weak-acidic hypochlorous acid water
KR1020200079624A
Method for recycling and regenerating waste lithium ion battery electrode materials
CN105990617A
Method for recovering positive electrode active material from lithium secondary battery
CN108448193A