Method for producing stretched film

By using variable spacing type clamps to extend diagonally and form a temperature gradient area during the manufacturing process of circular polarizers, the problems of relaxation and wrinkles in the stretched film are solved, the stability and quality of the film are improved, and it is suitable for image display devices Manufacturing of optical laminates.

CN115139501BActive Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210312544.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2024-10-29
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

When manufacturing circular polarizers, problems such as relaxation and wrinkles often occur in diagonally stretched films, which affects the quality and use of the film.

Method used

The longitudinally variable spacing type left and right clamps are used to extend the long strip of film diagonally, and a temperature gradient area is formed during the heat fixing process, so that the temperature of the end side of the leading clamp is higher than that of the other end side, and a 0.3 is formed by hot air heating ℃ ~ 25 ℃ temperature difference to reduce stress unevenness caused by extension.

Benefits of technology

It effectively reduces the slack and wrinkles in the obliquely stretched film, improves the stability and quality of the film, and is suitable for the manufacture of optical laminates for liquid crystal display devices and organic electroluminescent display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115139501B_ABST
    Figure CN115139501B_ABST
Patent Text Reader

Abstract

The present invention reduces the slack and / or wrinkles generated in the film stretched obliquely. The method for manufacturing the stretched film of the present invention comprises: holding the left and right ends of the long film in the width direction by using left and right clamps of variable spacing type with varying clamp spacing in the longitudinal direction; moving the left and right clamps in a manner of drawing a left-right symmetrical track while changing the clamp spacing of at least one clamp to stretch the film obliquely; and thermally fixing the film; in the oblique stretching, one of the left and right clamps is moved ahead of the other clamp, and in the fixing, a temperature gradient region is formed in which the temperature of the end side of the film held by the first clamp is higher than the temperature of the other end side.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a stretched film and a method for producing an optical layered body. Background Art

[0002] In image display devices such as liquid crystal display devices (LCDs) and organic electroluminescent display devices (OLEDs), circular polarizers are used to improve display characteristics or prevent reflection. Circular polarizers typically stack polarizers and phase difference films (typically λ / 4 plates) in a manner such that the absorption axis of the polarizer forms a 45° angle with the slow axis of the phase difference film. Phase difference films have been typically made by uniaxial stretching or biaxial stretching in the longitudinal and / or transverse directions, so their slow axes are mostly presented in the transverse direction (width direction) or longitudinal direction (length direction) of the long strip of film raw material. As a result, when making a circular polarizer, it is necessary to cut the phase difference film at a 45° angle relative to the width direction or the length direction and stick them together one by one.

[0003] In addition, in order to ensure the wide bandwidth of the circular polarizer, there is also a case where two phase difference films of a λ / 4 plate and a λ / 2 plate are stacked. In this case, it is necessary to stack the λ / 2 plate at an angle of 75° relative to the absorption axis of the polarizer, and to stack the λ / 4 plate at an angle of 15° relative to the absorption axis of the polarizer. In this case, when making a circular polarizer, it is necessary to cut the phase difference film at an angle of 15° and 75° relative to the width direction or the length direction, and stick them one by one.

[0004] Furthermore, in other embodiments, in order to prevent the light from the laptop from being reflected into the keyboard, etc., a λ / 2 plate is sometimes used on the visible side of the polarizer for the purpose of rotating the direction of the linear polarized light from the polarizer by 90°. In this case, it is necessary to cut the phase difference film at an angle of 45° with respect to the width direction or the length direction and laminate them one by one.

[0005] In order to solve this problem, a technique has been proposed in which the left and right ends of the long strip film in the width direction are held by using left and right clamps of variable spacing type with varying clamp spacing in the longitudinal direction, the clamp spacing of at least one of the left and right clamps is varied, and the slow axis of the phase difference film is presented in the oblique direction by stretching the film in the oblique direction relative to the longitudinal direction (hereinafter also referred to as "oblique stretching") (e.g. Patent Document 1). However, the obliquely stretched film obtained by this technique sometimes sags (droops) or wrinkles.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 4845619 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The present invention has been made to solve the above-mentioned technical problems, and its main object is to reduce the sag and / or wrinkles generated in the obliquely stretched film.

[0011] Means for solving technical problems

[0012] According to one aspect of the present invention, there is provided a method for manufacturing a stretched film, comprising: gripping the left and right ends of a long strip of film in the width direction using left and right clamps of a variable spacing type in which the clamp spacing in the longitudinal direction changes; moving the left and right clamps in a manner that draws a left-right symmetrical track while changing the clamp spacing of at least one clamp, thereby obliquely stretching the film; and thermally fixing the film; in the oblique stretching, one of the left and right clamps is moved ahead of the other clamp, and in the fixing, a temperature gradient region is formed in which the temperature of the end side of the film gripped by the leading clamp is higher than the temperature of the other end side.

[0013] In one embodiment, the maximum value of the temperature difference between both ends in the width direction of the temperature gradient region is 0.3°C to 25°C.

[0014] In one embodiment, the temperature gradient region is formed such that the isothermal line extends in an oblique direction with respect to the width direction of the film.

[0015] In one embodiment, the temperature gradient region is formed by supplying hot air to the film.

[0016] In one embodiment, the wind speed of the hot air is 3 m / min to 45 m / min.

[0017] In one embodiment, the oblique extension includes: (i) increasing the clamp spacing of one of the clamps from P1 to P2, while reducing the clamp spacing of the other clamp from P1 to P3; and (ii) changing the clamp spacing of each clamp in such a manner that the reduced clamp spacing and the increased clamp spacing become a specified equal spacing.

[0018] In one embodiment, P2 / P1 is 1.25 to 1.75, and P3 / P1 is 0.50 or more and less than 1.

[0019] According to another aspect of the present invention, there is provided a method for producing an optical laminate, comprising: obtaining a long-shaped stretched film by the above-mentioned production method; and continuously bonding the long-shaped optical film and the long-shaped stretched film while conveying them in the same longitudinal direction.

[0020] In one embodiment, the optical film is a polarizing plate, and the stretched film is a λ / 4 plate or a λ / 2 plate.

[0021] Effects of the Invention

[0022] In the method for manufacturing a stretched film of the present invention, heat fixing is performed in a heat fixing region having a temperature gradient region where the temperature of the end side held by the first clamp during oblique stretching is higher than the temperature of the other end side. Thus, the non-uniformity of residual stress caused by oblique stretching can be reduced, and as a result, a long oblique stretched film with reduced sag and / or wrinkles can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic plan view for explaining the overall structure of an example of a stretching device that can be used in the method for producing a stretched film of the present invention.

[0024] Figure 2 To illustrate the Figure 1 A schematic top view of the main parts of the linkage mechanism for changing the distance between the clamps in the extension device.

[0025] Figure 3 To illustrate the Figure 1 A schematic top view of the main parts of the linkage mechanism for changing the distance between the clamps in the extension device.

[0026] Figure 4A It is a schematic diagram showing the outline of the clamp spacing in one embodiment of the oblique extension.

[0027] Figure 4B It is a schematic diagram showing the outline of the clamp spacing in one embodiment of the oblique extension.

[0028] Figure 5 This is a schematic plan view for explaining an example of the temperature gradient that the thermal fixation region D has.

[0029] Fig. 6A A schematic diagram for explaining a hot air heating device that can be used to form a temperature gradient region.

[0030] Figure 6B A schematic plan view illustrating an example of the arrangement of a hot air type heating device that can be used to form a temperature gradient region.

[0031] Figure 7 This is a schematic cross-sectional view of a circularly polarizing plate using a retardation film obtained by the production method of the present invention.

[0032] Figure 8 This is a schematic diagram for explaining the method of measuring the relaxation amount.

[0033] Explanation of symbols

[0034] 1. Stretch film

[0035] 10L Endless Ring

[0036] 10R Endless Ring

[0037] 20 Clamp

[0038] 100 Extension device

[0039] 200 Hot air heating device

[0040] 300 Transport roller

[0041] 400 Ultrasonic displacement sensor

[0042] 500 Circular Polarizer DETAILED DESCRIPTION

[0043] The preferred embodiments of the present invention are described below, but the present invention is not limited to these embodiments. In addition, in this specification, "the clamp spacing in the longitudinal direction" refers to the distance between the centers of adjacent clamps in the longitudinal direction in the travel direction. In addition, the left-right relationship in the width direction of the long film refers to the left-right relationship facing the conveying direction of the film unless otherwise specified.

[0044] A. Method for producing stretched film

[0045] The method for manufacturing a stretched film according to an embodiment of the present invention comprises: holding left and right ends of a long film in a width direction with left and right clamps of a variable pitch type in which the clamp pitch in the longitudinal direction varies (holding step);

[0046] The film is obliquely stretched by moving the left and right clamps in a manner that draws a left-right symmetrical track while changing the clamp interval of at least one clamp (oblique stretching step);

[0047] and heat-fixing the film (heat-fixing step).

[0048] In the manufacturing method of this embodiment, during the oblique stretching, one of the left and right clamps is moved ahead of the other clamp, and during the thermal fixation, a temperature gradient region is formed in which the temperature of the end side of the film held by the first clamp is higher than the temperature of the other end side. Typically, the manufacturing method of this embodiment further includes a preheating step. Specifically, the film held by the left and right clamps is preheated and then supplied to the oblique stretching.

[0049] The above-mentioned oblique stretching can be performed, for example, using a spread-type simultaneous biaxial stretching device having left and right clamps that can hold the left and right ends of the long strip film in the width direction while moving in a manner that describes a left-right symmetrical track at different speeds. With this spread-type simultaneous biaxial stretching device, the left and right ends of the film can be stretched at different stretching ratios. Therefore, in a pair of left and right clamps when holding the film, by making the moving speed of one clamp faster than the moving speed of the other clamp (stretching at a stretching ratio of one end of the film higher than that of the other end), one clamp can be moved ahead of the other clamp, and the film can be stretched in an oblique direction between the leading clamp and the trailing clamp. At this time, the side held by the clamp that reaches the terminal of the stretching area ahead of the other is the side held by the leading clamp (the side with a higher stretching ratio).

[0050] Figure 1 The schematic top view of the overall structure of an example of a stretching device that can be used in the manufacturing method of the present invention is used to illustrate the present invention. In the stretching device 100, from the inlet side to the outlet side of the film, a holding area A, a preheating area B, a stretching area C, a heat fixing area D, and a release area E are sequentially arranged. These areas refer to the areas where the film to be stretched is actually held, preheated, obliquely stretched, heat fixed, and released, and do not refer to mechanically or structurally independent partitions. In addition, it should be noted that Figure 1 The length ratio of each region in the extension device is different from the actual length ratio.

[0051] Figure 1 Although not shown in the figure, an area for performing any appropriate treatment may be provided between the stretching area C and the heat fixing area D as required. Such treatment may include a lateral shrinking treatment. In addition, although not shown in the figure, the stretching device typically includes a heating device (e.g., various ovens such as hot air type, near infrared type, and far infrared type) for making the preheating area B to the release area E a heating environment.

[0052] The stretching device 100 has an endless ring 10L and an endless ring 10R with a plurality of clamps 20 for holding the film symmetrically on the left and right sides in a top view. In addition, in this specification, the endless ring on the left side is referred to as the endless ring 10L on the left side, and the endless ring on the right side is referred to as the endless ring 10R on the right side when viewed from the inlet side of the film. The clamps 20 of the endless rings 10L and 10R on the left and right are respectively guided to the standard track 70 and move in a circular manner. The clamps 20 of the endless ring 10L on the left side move in a counterclockwise direction, and the clamps 20 of the endless ring 10R on the right side move in a clockwise direction. At this time, as described above, since the endless loop 10L and the endless loop 10R are constructed to be symmetrical in a plan view, the clamp 20 of the left endless loop 10L and the clamp 20 of the right endless loop 10R move from the holding area A toward the release area E in a manner that describes a symmetrical trajectory.

[0053] In the holding area A and preheating area B of the stretching device 100, the left and right endless loops 10L and 10R are configured to be approximately parallel to each other at a distance corresponding to the initial width of the film to be stretched. The stretching area C is configured such that the distance between the left and right endless loops 10L and 10R gradually expands to a width corresponding to the stretched width of the film from one side of the preheating area B toward the heat fixing area D. In the heat fixing area D and the release area E, the left and right endless loops 10L and 10R are configured to be approximately parallel to each other at a distance corresponding to the width of the film after stretching. However, the configuration of the left and right endless loops 10L and 10R is not limited to the above-mentioned illustrated example. For example, the left and right endless loops 10L and 10R can also be configured to be approximately parallel to each other at a distance corresponding to the initial width of the film to be stretched from the holding area A to the release area E.

[0054] The clamp (clamp on the left side) 20 of the endless ring 10L on the left side and the clamp (clamp on the right side) 20 of the endless ring 10R on the right side can be moved in a circular motion independently. For example, the driving sprockets 11 and 12 of the endless ring 10L on the left side are driven to rotate in the counterclockwise direction by the motors 13 and 14, and the driving sprockets 11 and 12 of the endless ring 10R on the right side are driven to rotate in the clockwise direction by the motors 13 and 14. As a result, the clamp holding member of the driving roller (not shown) meshed with these driving sprockets 11 and 12 is given a walking force. As a result, the endless ring 10L on the left side is moved in a circular motion in the counterclockwise direction, and the endless ring 10R on the right side is moved in a circular motion in the clockwise direction. By driving the left motor and the right motor independently, the endless ring 10L on the left side and the endless ring 10R on the right side can be moved in a circular motion independently.

[0055] Furthermore, the clamp 20 of the left endless ring 10L (the clamp on the left) and the clamp 20 of the right endless ring 10R (the clamp on the right) are both of variable pitch type. That is, the left and right clamps 20, 20 are independent of each other, and the clamp pitch in the longitudinal direction can be changed as they move. The variable pitch type structure can be realized by adopting a driving method such as a pantograph method, a linear motor method, a motor chain method, etc. The following is an example of a link mechanism (pantograph mechanism).

[0056] Figure 2 and Figure 3 For illustration Figure 1 A schematic top view of the main part of the link mechanism for changing the distance between the clamps in the extension device. Figure 2 Indicates that the distance between the fixtures is the smallest. Figure 3 Indicates the state where the distance between the fixtures is at the maximum.

[0057] like Figure 2 and Figure 3 As shown in the figure, a slender rectangular clamp holding member 30 is provided in the horizontal direction of each holding clamp 20 when viewed from above. Although not shown in the figure, the clamp holding member 30 is closed by an upper beam, a lower beam, a front wall (the wall on the clamp side) and a rear wall (the wall on the opposite side of the clamp), forming a frame structure with a strong cross section. The clamp holding member 30 is arranged in such a way that it rotates on the running surfaces 81 and 82 using the running wheels 38 at both ends. In addition, Figure 2 and Figure 3 In the figure, the running wheels on the front wall side (the running wheels on the rotating running surface 81) are not shown. The running surfaces 81 and 82 are parallel to the standard track 70 in the entire area. On the rear side of the upper beam and the lower beam of the clamp holding member 30 (the opposite side of the clamp side (hereinafter referred to as the anti-clamp side)), a long hole 31 is formed along the length direction of the clamp holding member, and the slider 32 can be slidably engaged in the length direction of the long hole 31. Near the end of the clamp 20 side of the clamp holding member 30, a first shaft member 33 is vertically provided through the upper beam and the lower beam. On the other hand, a second shaft member 34 is vertically provided on the slider 32 of the clamp holding member 30. One end of the main connecting rod member 35 is pivotally connected to the first shaft member 33 of each clamp holding member 30. The main connecting rod member 35 is pivotally connected to the second shaft member 34 of the clamp holding member 30 at the other adjacent end. In addition to the main link member 35, one end of a secondary link member 36 is also pivotally connected to the first shaft member 33 of each clamp holding member 30. The other end of the secondary link member 36 is pivotally connected to the middle part of the main link member 35 through a pivot 37. The link mechanism obtained by the main link member 35 and the secondary link member 36 is as follows: Figure 2 As shown in FIG. 1 , the slider 32 moves toward the rear side (anti-clamp side) of the clamp holding member 30, and the longitudinal distance between the clamp holding members 30 (resulting in the clamp distance) becomes smaller, as shown in FIG. Figure 3 As shown in FIG. 1 , the more the slider 32 moves toward the front side (the clamp side) of the clamp holding member 30, the larger the longitudinal distance between the clamp holding members 30 (resulting in the clamp distance). The slider 32 is positioned by the distance setting rail 90. Figure 2 and Figure 3 As shown, the smaller the spacing distance between the standard rail 70 and the spacing setting rail 90 is, the larger the clamp spacing becomes.

[0058] By using the stretching device to stretch the film obliquely, an oblique stretched film, for example, a phase difference film having a slow axis in an oblique direction can be produced. In addition, the specific implementation of the stretching device is described in, for example, Japanese Patent Application Laid-Open No. 2008-44339, which is incorporated herein by reference in its entirety. The following is a detailed description of each step of the method for producing the stretched film.

[0059] A-1. Holding process

[0060] In the holding area A (film receiving entrance of the stretching device 100a), the two ends of the film to be stretched are held by the clamps 20 of the left and right endless loops 10L and 10R at a constant clamp pitch equal to each other or at different clamp pitches. The film is sent to the preheating area B by the movement of the clamps 20 of the left and right endless loops 10L and 10R (substantially, the movement of each clamp holding member guided to the standard track).

[0061] A-2. Preheating process

[0062] In the preheating area B, the left and right endless rings 10L and 10R are configured as described above to be approximately parallel to each other at a distance corresponding to the initial width of the film to be stretched, so that the film is heated without basically stretching it horizontally or vertically. However, since the preheating may cause the film to warp, in order to avoid contact with the nozzle in the oven, etc., the distance between the left and right clamps (the distance in the width direction) may be slightly widened.

[0063] In the preheating step, the film is heated to a temperature T1 (°C). The temperature T1 is preferably above the glass transition temperature (Tg) of the film, more preferably above Tg+2°C, and further preferably above Tg+5°C. On the other hand, the heating temperature T1 is preferably below Tg+40°C, and more preferably below Tg+30°C. The temperature T1 varies depending on the film used, and is, for example, 70°C to 190°C, and preferably 80°C to 180°C.

[0064] The heating time to reach the temperature T1 and the holding time at the temperature T1 can be appropriately set according to the constituent material of the film or the manufacturing conditions (e.g., the conveying speed of the film). The heating time and the holding time can be controlled by adjusting the moving speed of the clamp 20, the length of the preheating zone, the temperature of the preheating zone, etc.

[0065] A-3. Oblique stretching process

[0066] In the extension area C, the film is extended obliquely by changing the longitudinal clamp spacing of at least one of them and moving the left and right clamps 20 in a manner that depicts a left-right symmetrical track. For example, the clamp spacing of the left and right clamps can be increased or decreased at different positions, and the clamp spacing of the left and right clamps can be changed (increased and / or decreased) at different change speeds. The result of moving the left and right clamps while changing the clamp spacing in this way is that in a pair of left and right clamps that move to the extension area at the same time, one clamp moves ahead of the other clamp, and the one clamp reaches the terminal of the extension area ahead of the other clamp. Through this oblique extension, the film is extended in an oblique direction between the leading clamp and the trailing clamp, and as a result, a slow axis can be presented in a desired direction of the long film (for example, a direction of 45° relative to the longitudinal direction).

[0067] The oblique extension may also include lateral extension. In this case, the oblique extension may be performed while expanding the distance between the left and right clamps (the distance in the width direction), as shown in the example in the figure. Alternatively, the oblique extension may not include lateral extension, and may be performed while maintaining the distance between the left and right clamps, as is different from the example in the figure.

[0068] When the oblique stretching includes the transverse stretching, the stretching ratio in the transverse direction (TD) (the width W of the film after the oblique stretching) final The initial width W of the film initial The ratio (W final / W initial )) is preferably 1.05 to 6.00, more preferably 1.10 to 5.00.

[0069] In one embodiment, the oblique extension can be performed by increasing or decreasing the clamp spacing of each clamp to a predetermined spacing while making the position where the clamp spacing of one of the left and right clamps starts to increase or decrease different from the position where the clamp spacing of the other clamp starts to increase or decrease in the longitudinal direction. For the oblique extension of this embodiment, for example, the description of Patent Document 1, Japanese Patent Application Publication No. 2014-238524, etc. can be referred to.

[0070] In other embodiments, the oblique extension can be performed by increasing or decreasing the clamp spacing of the other clamp to a predetermined spacing while fixing the clamp spacing of one of the left and right clamps, and then returning to the initial clamp spacing. For the oblique extension of this embodiment, for example, reference can be made to the records of Japanese Patent Publication No. 2013-54338, Japanese Patent Publication No. 2014-194482, etc.

[0071] In other embodiments, the oblique extension can be performed by: (i) increasing the clamp spacing of one of the left and right clamps from P1 to P2, while reducing the clamp spacing of the other clamp from P1 to P3; and (ii) changing the clamp spacing of each clamp in such a way that the reduced clamp spacing and the increased clamp spacing become a predetermined equal spacing. For the oblique extension of this embodiment, for example, reference can be made to the records of Japanese Patent Publication No. 2014-194484. The oblique extension of this embodiment may also include: extending the distance between the left and right clamps while increasing the clamp spacing of one clamp from P1 to P2 and reducing the clamp spacing of the other clamp from P1 to P3, thereby extending the film obliquely (first oblique extension); and extending the distance between the left and right clamps while maintaining the clamp spacing of one clamp at P2 or reducing it to P4 in a manner that the clamp spacings of the left and right clamps become equal, and increasing the clamp spacing of the other clamp to P2 or P4, thereby extending the film obliquely (second oblique extension).

[0072] In the first oblique stretching, by stretching one end of the film in the longitudinal direction and shrinking the other end in the longitudinal direction while performing oblique stretching, a slow axis can be presented in a desired direction (for example, a direction at 45° relative to the longitudinal direction) with high uniaxiality and in-plane orientation. In addition, in the second oblique stretching, by narrowing the difference in the gap between the left and right clamps while performing oblique stretching, it is possible to fully stretch in the oblique direction while relieving excess stress.

[0073] In the oblique stretching of the above three embodiments, since the film can be released from the clamps while the moving speeds of the left and right clamps become equal, it is difficult for unevenness in the film conveying speed to occur when the left and right clamps are released, and the subsequent film winding can also be carried out appropriately.

[0074] Figure 4A and Figure 4B 1 and 2 are schematic diagrams showing an example of the outline of the clamp spacing in the oblique extension including the first oblique extension and the second oblique extension. The first oblique extension will be described in detail below with reference to these diagrams. Figure 4A and Figure 4BIn the figure, the horizontal axis corresponds to the travel distance of the clamp. At the beginning of the first oblique extension, the clamp spacing on the left and right is P1. P1 is representatively the clamp spacing when holding the film. At the beginning of the first oblique extension, the clamp spacing of one clamp (hereinafter sometimes referred to as the first clamp) begins to increase and the clamp spacing of another clamp (hereinafter sometimes referred to as the second clamp) begins to decrease. In the first oblique extension, the clamp spacing of the first clamp is increased to P2 and the clamp spacing of the second clamp is reduced to P3. Therefore, at the end of the first oblique extension (when the second oblique extension begins), the second clamp moves with a clamp spacing of P3 and the first clamp moves with a clamp spacing of P2. In addition, the ratio of the clamp spacings can roughly correspond to the ratio of the moving speeds of the clamps. Therefore, the ratio of the clamp spacings of the left and right clamps can roughly correspond to the ratio of the stretching ratios in the MD direction of the right end and the left end of the film.

[0075] Figure 4A and Figure 4B In the embodiment, the timing of starting to increase the clamp spacing of the first clamp and the timing of starting to reduce the clamp spacing of the second clamp are both at the beginning of the first oblique extension. Unlike the illustrated example, the clamp spacing of the second clamp can be reduced after the clamp spacing of the first clamp is increased, and the clamp spacing of the first clamp can be increased after the clamp spacing of the second clamp is reduced. In a preferred embodiment, the clamp spacing of the second clamp can be reduced after the clamp spacing of the first clamp is increased. According to this embodiment, since the film has been extended to a certain extent (preferably about 1.2 times to 2.0 times) in the width direction, wrinkles are difficult to occur even if the clamp spacing of the second clamp is greatly reduced. Therefore, a more acute oblique extension can be performed, and a phase difference film with high uniaxiality and in-plane orientation can be preferably obtained.

[0076] Likewise, in Figure 4A and Figure 4B In the figure, the increase in the clamp spacing of the first clamp and the decrease in the clamp spacing of the second clamp continue until the end of the first oblique extension (the beginning of the second oblique extension), but unlike the illustrated example, either the increase or the decrease in the clamp spacing may end earlier than the other, and the clamp spacing may remain the same until the other ends (until the end of the first oblique extension).

[0077] The rate of change of the clamp spacing of the first clamp (P2 / P1) is preferably 1.25 to 1.75, more preferably 1.30 to 1.70, and further preferably 1.35 to 1.65. In addition, the rate of change of the clamp spacing of the second clamp (P3 / P1) is, for example, greater than 0.50 and less than 1, preferably 0.50 to 0.95, more preferably 0.55 to 0.90, and further preferably 0.55 to 0.85. When the rate of change of the clamp spacing is within this range, a slow axis can be presented with high uniaxiality and in-plane orientation in a direction of approximately 45 degrees relative to the length direction of the film.

[0078] As described above, the distance between the fixtures can be adjusted by adjusting the spacing between the extension device, setting the distance between the track and the standard track, and positioning the slider.

[0079] The stretch ratio in the width direction of the film in the first oblique stretching (film width at the end of the first oblique stretching / film width before the first oblique stretching) is preferably 1.1 times to 3.0 times, more preferably 1.2 times to 2.5 times, and further preferably 1.25 times to 2.0 times. When the stretch ratio is less than 1.1 times, tinplate-like wrinkles sometimes occur at the end of the contracted side. In addition, when the stretch ratio exceeds 3.0 times, the biaxiality of the obtained phase difference film becomes high, and when it is applied to a circular polarizer, the viewing angle characteristics are sometimes reduced.

[0080] In one embodiment, the first oblique stretching is performed in such a manner that the product of the change rate of the first fixture's inter-clamp spacing and the change rate of the second fixture's inter-clamp spacing is preferably 0.7 to 1.5, more preferably 0.8 to 1.45, and even more preferably 0.85 to 1.40. When the product of the change rates is within this range, a retardation film with high uniaxiality and in-plane orientation can be obtained.

[0081] Next, refer to Figure 4A One embodiment of the second oblique extension is specifically described. In the second oblique extension of this embodiment, the clamp spacing of the second clamp is increased from P3 to P2. On the other hand, the clamp spacing of the first clamp is maintained at P2 during the second oblique extension. Therefore, at the end of the second oblique extension, both left and right clamps move at the clamp spacing P2.

[0082] Figure 4A The change rate (P2 / P3) of the second clip pitch in the second oblique extension of the embodiment shown is not limited unless the effect of the present invention is impaired. The change rate (P2 / P3) is, for example, 1.3 to 4.0, preferably 1.5 to 3.0.

[0083] One side reference Figure 4BNext, other embodiments of the second diagonal extension will be specifically described. In the second diagonal extension of this embodiment, while reducing the clamp pitch of the first clamp, the clamp pitch of the second clamp is increased. Specifically, the clamp pitch of the first clamp is reduced from P2 to P4, and the clamp pitch of the second clamp is increased from P3 to P4. Therefore, at the end of the second diagonal extension, both the left and right clamps move with a clamp pitch of P4. In addition, in the illustrated example, the reduction of the clamp pitch of the first clamp and the increase of the clamp pitch of the second clamp start simultaneously with the start of the second diagonal extension, but these can start at different timings. Similarly, the reduction of the clamp pitch of the first clamp and the increase of the clamp pitch of the second clamp can also end at different timings.

[0084] Figure 4B The change rate (P4 / P2) of the clamp pitch of the first clamp and the change rate (P4 / P3) of the clamp pitch of the second clamp in the second diagonal extension of the illustrated embodiment are not limited as long as the effects of the present invention are not impaired. The change rate (P4 / P2) is, for example, 0.4 or more and less than 1.0, preferably 0.6 to 0.95. In addition, the change rate (P4 / P3) is, for example, more than 1.0 and 2.0 or less, preferably 1.2 to 1.8. It is preferred that P4 is equal to or greater than P1. When P4 < P1, problems such as wrinkles at the ends and increased biaxiality may occur.

[0085] The extension ratio in the width direction of the film during the second diagonal extension (film width at the end of the second diagonal extension / film width at the end of the first diagonal extension) is preferably 1.1 times to 3.0 times, more preferably 1.2 times to 2.5 times, and further preferably 1.25 times to 2.0 times. When this extension ratio is less than 1.1 times, wrinkles like those of galvanized iron may sometimes occur at the ends on the shrinking side. In addition, when this extension ratio exceeds 3.0 times, the biaxiality of the obtained retardation film becomes high, and when applied to a circular polarizing plate or the like, the viewing angle characteristics may deteriorate. In addition, from the same viewpoint as above, the extension ratio in the width direction during the first diagonal extension and the second diagonal extension (film width at the end of the second diagonal extension / film width before the first diagonal extension) is preferably 1.2 times to 4.0 times, more preferably 1.4 times to 3.0 times.

[0086] The diagonal extension can typically be carried out at a temperature T2. The temperature T2 is preferably Tg - 20°C to Tg + 30°C, more preferably Tg - 10°C to Tg + 20°C, and particularly preferably around Tg with respect to the glass transition temperature (Tg) of the film. Although it varies depending on the film used, the temperature T2 is, for example, 70°C to 180°C, preferably 80°C to 170°C. The difference (T1 - T2) between the above temperature T1 and temperature T2 is preferably ±2°C or more, more preferably ±5°C or more. In one embodiment, T1 > T2, so the film heated to temperature T1 in the preheating zone can be cooled to temperature T2.

[0087] As described above, the lateral shrinkage treatment may be performed after the oblique stretching. For this treatment after the oblique stretching, reference may be made to paragraphs 0029 to 0032 of Japanese Patent Application Laid-Open No. 2014-194483.

[0088] A-4. Heat fixing process

[0089] In the heat fixation zone D, the obliquely stretched film is heat treated. If necessary, the clamp spacing in the longitudinal direction is reduced during the heat treatment, thereby also relieving stress. The stretched state is fixed by the heat treatment and any stress relaxation.

[0090] In the embodiment of the present invention, in the thermal fixing region D, the end portion side (S H side) is higher than the other end side (S L side) temperature gradient area. Figure 5 This is a schematic top view illustrating an example of a temperature gradient formed in the thermal fixation region D, and the dotted line represents an isotherm (a°C>b°C>c°C>d°C). Figure 5 As shown, the heat fixation region D has regions D1 and D3 with uniform temperature distribution on the side of the extension region C and the side of the release region E, respectively, and has a region (temperature gradient region) D2 with the above-mentioned specified temperature gradient therebetween. In addition, unlike the example shown in the figure, the heat fixation region D can also omit either or both of the regions D1 and D3. In addition, the above-mentioned temperature gradient region is formed in the heat fixation region as the ambient temperature of the film (for example, the temperature of the region 250 mm away from the film surface), and the temperature of the temperature gradient region can substantially correspond to the film temperature.

[0091] In the region D2, it is preferred that the isotherms extend in an oblique direction relative to the width direction of the temperature gradient region (substantially the width direction of the film). H Side and S LThe extension direction of the isotherm (the direction of extension of the straight line on the side) can change sequentially from upstream to downstream in the conveying direction of the temperature gradient area, or it can be constant in the entire area of ​​the temperature gradient area. In addition, in the temperature gradient area of ​​the example shown in the figure, the isotherms are formed in a curved shape, but the isotherms can also be straight lines. When the extension direction of the isotherm changes sequentially from upstream to downstream in the conveying direction of the temperature gradient area, the angle formed by the extension direction of the isotherm and the width direction can increase sequentially from the upstream side to the downstream side in the conveying direction. The angle (the maximum value of the angle when the extension direction of the isotherm changes) is preferably 10° to 80° or 100° to 170°, more preferably 20° to 70° or 110° to 160°, and further preferably 30° to 60° or 120° to 150°. In one embodiment, the extension direction of the isotherm (the direction in which the isotherm with the largest angle relative to the width direction is extended when the extension direction of the isotherm changes (in the example shown in the figure, the angle connecting S L3 With S H3 A straight line or connection S L4 With S H4 The straight line is the stretching direction)) relative to the oblique stretching direction (when the film 1 is a resin film with positive birefringence, it is the slow axis direction) X is preferably 0° to 60° or 120° to 180°, more preferably 0° to 50° or 130° to 180°, further preferably 0° to 45° or 135° to 180°, further preferably 0° to 30° or 150° to 180°, further more preferably 0° to 20° or 160° to 180°, further more preferably 0° to 10° or 170° to 180°. The stretching direction of the isotherm is preferably inclined to the same side as the oblique stretching direction X based on the length direction of the film (in other words, the slope has the same sign). Through this temperature gradient region D2, the non-uniformity of the residual stress caused by the oblique stretching can be reduced, and as a result, the relaxation and / or wrinkles can be preferably reduced. Furthermore, when the extending direction of the isothermal line changes sequentially from upstream to downstream in the conveying direction of the temperature gradient region, the minimum value of the angle between the extending direction of the isothermal line and the width direction exceeds 0°, and may be 1°, for example.

[0092] In region D2, as long as the temperature is parallel to the width direction, L Side S H The side may be simply raised, and the pattern may be linear or curved. In addition, in the downstream region of the region D2, as the temperature gradient is eliminated, there may be a portion with a constant temperature in the width direction.

[0093] The maximum temperature difference between the two ends of the width direction in the region D2 (for example, the S H Side and S LThe maximum value of the temperature difference above 250 mm at the end of the film 1 on the side is, for example, 0.3°C to 25°C. H Side and S L When the temperature difference between the two sides is within this range, the effect of reducing sag and / or wrinkles can be preferably obtained.

[0094] In one embodiment, the maximum value of the temperature difference is preferably 1°C to 20°C, more preferably 3°C to 17°C. H Side and S L When the temperature difference on the side is within this range, the effect of reducing sag can be more preferably obtained.

[0095] In one embodiment, the maximum value of the temperature difference is preferably 0.5°C to 25°C, more preferably 5°C to 20°C. H Side and S L When the temperature difference on the side is within this range, the wrinkle reduction effect can be more preferably obtained.

[0096] In one embodiment, the maximum value of the temperature difference is preferably 5°C to 17°C, more preferably 7°C to 15°C. H Side and S L When the temperature difference on both sides is within this range, the effect of reducing sag and wrinkles can be more preferably obtained.

[0097] In the conveying direction (length direction of the film) of region D2, the temperature gradually decreases from upstream to downstream. The temperature at the beginning of region D2 (the most upstream location with a temperature gradient in the width direction) and the temperature at the end of region D2 (the most downstream location with a temperature gradient in the width direction) can be appropriately set according to the type of resin forming the film. In one embodiment, the temperature at the beginning of region D2 is, for example, 80°C to 180°C, preferably 90°C to 170°C, and more preferably 100°C to 160°C. The temperature at the end of region D2 is, for example, 30°C to 150°C, preferably 40°C to 140°C, and more preferably 50°C to 130°C. The temperature difference between the beginning and the end of region D2 is, for example, 10°C to 70°C, preferably 20°C to 60°C, and more preferably 30°C to 50°C. In addition, in the downstream region of region D2, as the temperature gradient is eliminated, there may be a portion with a constant temperature in the conveying direction.

[0098] The heat treatment time in the region D2 is, for example, 10 seconds to 600 seconds, or preferably 30 seconds to 360 seconds.

[0099] The method of forming the region D2 having the temperature gradient is not particularly limited. For example, by setting a temperature gradient in the conveying direction in which the temperature decreases from the starting end side to the terminal side of the region D2 (i.e., from upstream to downstream in the conveying direction), and at the same time setting a temperature gradient from S at the starting end of the region D2 to H Side SL The temperature gradient in the width direction in which the temperature of the side is reduced can preferably form a temperature gradient area D2 in which the isotherms extend in the oblique direction. As a method for forming a temperature gradient in the conveying direction, there can be cited a method of dividing the D2 area into a plurality of partitions, and using a heater, hot air, etc. to adjust the atmosphere temperature of each partition in a manner such that the temperature decreases from the starting side to the terminal side. As a method for forming a temperature gradient in the width direction, a method of supplying hot air with a temperature gradient in the width direction to the film; a method of irradiating an infrared heater with different powers in the width direction to the film, etc. can be preferably used. Since the temperature gradient is easy to control, a method of supplying hot air to the film can be preferably used.

[0100] A method of supplying hot air having a temperature gradient in the width direction to the film is, for example, Fig. 6A The hot air type heating device 200 shown in the figure can be used to supply high temperature air from one pipe 210 and low temperature air from another pipe 220, mix them in various proportions in the main body 230, and eject the hot air of different temperatures from a plurality of nozzles 240 arranged at predetermined intervals in the width direction. The main body 230, for example, has a high temperature air distribution head (not shown) connected to the pipe 210, whose flow rate decreases toward the pipe 220 side; and a low temperature air distribution head (not shown) connected to the pipe 220, whose flow rate decreases toward the pipe 210 side. The ratio of high temperature air and low temperature air distributed from these distribution heads is adjusted, so that hot air with a desired temperature gradient can be supplied.

[0101] In one embodiment, in a heat fixing area having a temperature gradient in the conveying direction, a hot air heating device is arranged at the beginning of area D2 to supply hot air having a temperature gradient in the width direction to the film. In this case, a plurality of hot air heating devices are arranged in parallel, and the temperature gradient of the hot air supplied by each hot air heating device is controlled, so that hot air having a temperature gradient in both the conveying direction and the width direction can be supplied (as a result, hot air having a temperature gradient with isotherms extending in an oblique direction). For example, in Figure 6B In the embodiment shown, the first to fourth hot air type heating devices 200a to 200d are arranged in parallel in order from upstream to downstream in the conveying direction. The first to fourth hot air type heating devices 200a to 200d respectively supply heat having a temperature from the right end portion (S H side) to the left end (S L side) reduces the temperature gradient of the hot air, and in addition, S H Side and S LThe temperature of the hot air on the side is set in a manner that decreases from the first hot air type heating device 200a to the fourth hot air type heating device 200d (i.e., toward the downstream of the conveying direction). The supply time of the hot air can be, for example, 10 seconds to 600 seconds, preferably 30 seconds to 360 seconds. By slowly cooling the hot air having a temperature gradient in the width direction or the hot air having a temperature gradient in the conveying direction and the width direction to the regional temperature toward the downstream of the conveying direction, a temperature gradient region in which the isotherm extends in the oblique direction can be formed.

[0102] The wind speed of the hot air supplied to the film from the hot air heating device 200 is, for example, 3 m / min to 45 m / min. If the wind speed of the hot air is within this range, the film having the temperature gradient region extending to the film end can be temperature-controlled as desired, and as a result, the effect of reducing sag and / or wrinkles can be preferably obtained.

[0103] In one embodiment, the wind speed of the hot air is preferably 5 m / min to 30 m / min, more preferably 10 m / min to 25 m / min. When the wind speed of the hot air is within this range, the effect of reducing sag can be more preferably obtained.

[0104] In one embodiment, the wind speed of the hot air is preferably 15 m / min to 40 m / min, more preferably 20 m / min to 35 m / min. When the wind speed of the hot air is within this range, the wrinkle reduction effect can be more preferably obtained.

[0105] In one embodiment, the wind speed of the hot air is preferably 15 m / min to 30 m / min, more preferably 20 m / min to 25 m / min. When the wind speed of the hot air is within this range, the effect of reducing sag and wrinkles can be more preferably obtained.

[0106] As long as the temperature gradient region is formed, the angle at which the hot air is blown is not limited. In one embodiment, the hot air is blown at an angle of 90° relative to the membrane surface.

[0107] The temperature of the region D1 is typically the same as the temperature at the start of the region D2. The heat treatment time in the region D1 is, for example, 3 seconds to 120 seconds.

[0108] The temperature of the region D3 is typically the same as the temperature at the end of the region D2. The heat treatment time in the region D3 is, for example, 3 seconds to 120 seconds.

[0109] A-5. Release process

[0110] The film is released from the clamp at any position in the release region E. In the release region E, the heat-fixed film is usually neither stretched horizontally nor stretched vertically, and the film is released from the clamp after cooling to a desired temperature. Typically, the release region has a uniform temperature distribution.

[0111] The film temperature when released from the jig is, for example, 150°C or lower, preferably 70°C to 140°C, and more preferably 80°C to 130°C.

[0112] The stretched film released from the clamp is sent out from the outlet of the stretching device and is inspected for slack and / or the presence of wrinkles.

[0113] B. Extending the membrane of an object

[0114] In the manufacturing method of the present invention, any appropriate film can be used. For example, a resin film that can be used as a phase difference film can be cited. As the material constituting this film, for example, polycarbonate resins, polyvinyl acetal resins, cycloolefin resins, acrylic resins, cellulose ester resins, cellulose resins, polyester resins, polyester carbonate resins, olefin resins, polyurethane resins, etc. can be cited. Preferred are polycarbonate resins, cellulose ester resins, polyester resins, polyester carbonate resins, and cycloolefin resins. The reason is that if these resins are used, a so-called wavelength-dependent phase difference film showing reverse dispersion can be obtained. These resins can be used alone or in combination with the desired properties.

[0115] As the polycarbonate resin, any appropriate polycarbonate resin may be used, and for example, a polycarbonate resin including a structural unit derived from a dihydroxy compound is preferred. Specific examples of the dihydroxy compound include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-propylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-sec-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropyloxy)phenyl)fluorene, etc. In addition to the structural units derived from the above-mentioned dihydroxy compounds, the polycarbonate resin may also contain structural units derived from dihydroxy compounds such as isosorbide, isomannide, isoidide, spiroethylene glycol, dioxane glycol, diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), cyclohexanedimethanol (CHDM), tricyclodecanedimethanol (TCDDM), and bisphenols.

[0116] The details of the polycarbonate resin are described in, for example, Japanese Patent Application Laid-Open No. 2012-67300 and Japanese Patent No. 3325560. The descriptions of these patent documents are incorporated herein by reference.

[0117] The glass transition temperature of the polycarbonate resin is preferably 110°C to 250°C, more preferably 120°C to 230°C. When the glass transition temperature is too low, the heat resistance tends to deteriorate, and dimensional changes may occur after film molding. When the glass transition temperature is too high, the molding stability during film molding may deteriorate, and the transparency of the film may be impaired. In addition, the glass transition temperature is obtained according to JIS K 7121 (1987).

[0118] As the above-mentioned polyvinyl acetal resin, any appropriate polyvinyl acetal resin can be used. Representatively, the polyvinyl acetal resin can be obtained by condensing at least two aldehyde compounds and / or ketone compounds with a polyvinyl alcohol resin. Specific examples of polyvinyl acetal resins and detailed production methods are described in, for example, Japanese Patent Publication No. 2007-161994. This description is cited in this specification as a reference.

[0119] The stretched film (phase difference film) obtained by stretching the film of the above-mentioned stretching object preferably shows a refractive index characteristic of nx>ny. In one embodiment, the phase difference film can preferably function as a λ / 4 plate. In the present embodiment, the in-plane phase difference Re(550) of the phase difference film (λ / 4 plate) is preferably 100nm~180nm, more preferably 135nm~155nm. In other embodiments, the phase difference film can preferably function as a λ / 2 plate. In the present embodiment, the in-plane phase difference Re(550) of the phase difference film (λ / 2 plate) is preferably 230nm~310nm, more preferably 250nm~290nm. In addition, in this specification, nx is the refractive index in the direction where the in-plane refractive index reaches the maximum (ie, the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis (ie, the fast axis direction), and nz is the refractive index in the thickness direction. In addition, Re(λ) is the in-plane phase difference of the film measured at 23°C with light of a wavelength of λnm. Therefore, Re(550) is the in-plane retardation of the film measured with light of a wavelength of 550 nm at 23° C. Re(λ) is a value obtained by the formula: Re(λ)=(nx-ny)×d when the thickness of the film is d (nm).

[0120] The in-plane phase difference Re (550) of the phase difference film can be set to a desired range by appropriately setting the oblique stretching conditions. For example, the method of manufacturing a phase difference film having an in-plane phase difference Re (550) of 100 nm to 180 nm by oblique stretching is disclosed in detail in Japanese Patent Publication No. 2013-54338, Japanese Patent Publication No. 2014-194482, Japanese Patent Publication No. 2014-238524, Japanese Patent Publication No. 2014-194484, etc. Therefore, those skilled in the art can set appropriate oblique stretching conditions according to the disclosure.

[0121] When a circular polarizing plate is prepared using a single retardation film, or when the direction of linear polarized light is rotated 90° using a single retardation film, the slow axis direction of the retardation film used is preferably 30° to 60° or 120° to 150° relative to the length direction of the film, more preferably 38° to 52° or 128° to 142°, further preferably 43° to 47° or 133° to 137°, and particularly preferably about 45° or 135°.

[0122] In addition, when producing a circular polarizer using two retardation films (specifically, a λ / 2 plate and a λ / 4 plate), the slow axis direction of the retardation film (λ / 2 plate) used is preferably 60° to 90°, more preferably 65° to 85°, and particularly preferably about 75° with respect to the length direction of the film. In addition, the slow axis direction of the retardation film (λ / 4 plate) is preferably 0° to 30°, more preferably 5° to 25°, and particularly preferably about 15° with respect to the length direction of the film.

[0123] The retardation film preferably exhibits a so-called inverse dispersion wavelength dependence. Specifically, the in-plane retardation satisfies the relationship Re(450) < Re(550) < Re(650). Re(450) / Re(550) is preferably 0.8 or more and less than 1.0, more preferably 0.8 to 0.95. Re(550) / Re(650) is preferably 0.8 or more and less than 1.0, more preferably 0.8 to 0.97.

[0124] The absolute value of the photoelastic modulus of the retardation film is preferably 2×10 -12 (m 2 / N) to 100×10 -12 (m 2 / N), more preferably 5×10 -12 (m 2 / N) to 50×10 -12 (m 2 / N).

[0125] C. Optical laminate and manufacturing method of the optical laminate

[0126] The stretched film obtained by the manufacturing method of the present invention can be laminated with other optical films and used as an optical laminate. For example, the retardation film obtained by the manufacturing method of the present invention can be laminated with a polarizer and preferably used as a circular polarizer.

[0127] Figure 7 is a schematic cross-sectional view of an example of such a circular polarizer. The illustrated circular polarizer 500 has a polarizer 510, a first protective film 520 disposed on one side of the polarizer 510, a second protective film 530 disposed on the other side of the polarizer 510, and a retardation film 540 disposed outside the second protective film 530. The retardation film 540 is a stretched film (e.g., a λ / 4 plate) obtained by the manufacturing method described in item A. The second protective film 530 can also be omitted. In this case, the retardation film 540 can function as a protective film for the polarizer. The angle formed by the absorption axis of the polarizer 510 and the slow axis of the retardation film 540 is preferably 30° to 60°, more preferably 38° to 52°, further preferably 43° to 47°, and particularly preferably about 45°.

[0128] The phase difference film obtained by the manufacturing method of the present invention is long and has a slow axis in an oblique direction (for example, a direction of 45° relative to the length direction). In addition, in most cases, the long polarizer has an absorption axis in the length direction or the width direction. Therefore, if the phase difference film obtained by the manufacturing method of the present invention is used, the circular polarizer can be made with extremely excellent manufacturing efficiency using the so-called roll-to-roll method. In addition, roll-to-roll refers to a method in which long strips of film are rolled and transported to each other while their length directions are uniformly and continuously bonded.

[0129] In one embodiment, the method for producing an optical layered body of the present invention comprises: obtaining a long stretched film by the method for producing a stretched film described in Section A; and continuously laminating the long optical film and the long stretched film together in a uniform longitudinal direction while conveying the long optical film and the long stretched film.

[0130] [Example]

[0131] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. In addition, the measurement and evaluation methods of the examples are as follows.

[0132] (1) Thickness

[0133] The measurement was performed using a micrometer (manufactured by PEACOCK, product name: "DG-205 type pds-2").

[0134] (2) Phase difference

[0135] The in-plane retardation Re (550) was measured using Axoscan manufactured by Axometrics.

[0136] (3) Orientation angle (direction of the slow axis)

[0137] The central portion of the film to be measured was cut into a square shape of 50 mm in width and 50 mm in length so that one side was parallel to the width direction of the film to prepare a sample. The sample was measured using Axoscan manufactured by Axometrics to measure the orientation angle θ at a wavelength of 590 nm.

[0138] (4) Glass transition temperature (Tg)

[0139] Measured according to JIS K7121.

[0140] (5) Relaxation

[0141] like Figure 8As shown in FIG. 1 , an ultrasonic displacement sensor 400 is arranged below the conveying path of the film 1 at the midpoint between the conveying rollers 300a and 300b (distance between rollers: 912 mm). The distance from the ultrasonic displacement sensor to the stretched film is measured at the center and end portions in the width direction when conveying at a conveying tension of 150 N / m, and the maximum distance (L MAX ) and the minimum distance (L MIN ) difference (L MAX -L MIN ) as the slack amount (mm). In addition, the above-mentioned slack amount was measured by cutting off the tension applied to correct the slack using a suction roll or the like, and then conveying the roll at a conveying tension of 150 N / m.

[0142] <Example 1>

[0143] (Production of polyester carbonate resin film)

[0144] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux cooler controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of ISB, 42.28 parts by mass (0.139 mol) of SPG, 63.77 parts by mass (0.298 mol) of DPC and 1.19×10 mol of calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5 mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. After 40 minutes from the start of heating, the internal temperature reached 220°C, and the temperature was kept under control while the pressure was reduced. After reaching 220°C, it reached 13.3 kPa in 90 minutes. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux cooler, and a certain amount of monomer components contained in the phenol vapor was returned to the reactor. The uncondensed phenol vapor was introduced into a 45°C condenser for recovery. Nitrogen was introduced into the first reactor, and after temporarily restoring the pressure to atmospheric pressure, the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature and pressure reduction in the second reactor were started, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. After that, polymerization was carried out until the specified stirring power was reached. When the specified power was reached, nitrogen was introduced into the reactor for restoring the pressure, the generated polyester carbonate was extruded into water, and the strands were cut to obtain pellets. The Tg of the obtained polyester carbonate resin was 140°C.

[0145] After the obtained polyester carbonate resin was vacuum dried at 80°C for 5 hours, a resin film with a thickness of 135 μm was prepared using a film-making device having a uniaxial extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chilled roll (setting temperature: 120-130°C) and a winder.

[0146] (Production of stretched film)

[0147] use Figures 1 to 3 The stretching device shown in the figure obliquely stretches the polyester carbonate resin film obtained as above to obtain a phase difference film.

[0148] Specifically, the left and right ends of the polyester carbonate resin film were gripped by left and right clamps at the entrance of the stretching device and preheated to 145° C. in the preheating zone B. In the preheating zone, the clamp pitch ( P1 ) between the left and right clamps was 125 mm.

[0149] Next, as the film enters the stretching region C, the clamp spacing of the right clamp begins to increase and the clamp spacing of the left clamp begins to decrease. While the clamp spacing of the right clamp is increased to P2, the clamp spacing of the left clamp is reduced to P3 (first oblique extension). At this time, the clamp spacing change rate (P2 / P1) of the right clamp is 1.42, the clamp spacing change rate (P3 / P1) of the left clamp is 0.78, and the lateral stretch ratio relative to the original width of the film is 1.45 times. Next, while maintaining the clamp spacing of the right clamp at P2, the clamp spacing of the left clamp begins to increase from P3 to P2 (second oblique extension). During this period, the rate of change (P2 / P3) of the clamp spacing of the left clamp is 1.82, and the lateral stretch ratio relative to the original width of the film is 1.9 times. In addition, the stretching region C is set to Tg+3.2°C (143.2°C).

[0150] Next, at the beginning of the heat fixation area D (the terminal of the extension area C) where the atmosphere temperature is set to 140°C, a hot air heating device is used to blow hot air with a temperature gradient decreasing from the right end side to the left end side of the film from upstream to downstream in the conveying direction, in a manner that the right end side decreases from 140°C to 125°C and the left end side decreases from 140°C to 115°C, while adjusting the film to be blown for 180 seconds, and the film is heat treated (heat fixation time 210 seconds). At this time, the wind speed of the hot air (the wind speed when ejected from the hot air heating device) is 20m / min, and it is blown from 200mm below the film at an angle of 90° relative to the film surface. In addition, the temperature of the terminal of the heat fixation area D is reduced to the atmosphere temperature (115°C), and the temperature gradient in the width direction is eliminated.

[0151] Next, in the release region E whose temperature was set at 100° C., the film was cooled to 100° C., and then the left and right clamps were released.

[0152] Thus, a stretched film was obtained. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0153] In addition, when the temperature of the heat fixation area (the temperature at 250 mm above the film) was measured using a non-contact zone thermometer, a temperature gradient area was formed from the beginning to the end of the heat fixation area, in which the temperature on the right side was higher than the temperature on the left side relative to the center of the width direction of the film. The maximum value of the temperature difference at both ends of the width direction in the temperature gradient area was 10°C, and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film). In addition, the temperatures of the preheating area, the oblique stretching area, and the release area were uniform in the width direction, and no temperature gradient area was formed.

[0154] Before the above-mentioned stretched film is produced, hot air at 140°C is evenly blown in the width direction at a wind speed of 7 m / min at the starting end of the heat fixing area D, and then heat fixing following the atmosphere temperature is performed (as a result, no temperature gradient is formed in the oblique direction). Apart from this, when the stretched film is obtained in the same manner as in Example 1, relaxation occurs at the left end in the width direction, and the relaxation amount is 18 mm.

[0155] <Example 2>

[0156] At the beginning of the heat fixing area D, hot air at 140°C was blown uniformly in the width direction at a wind speed of 25 m / min for 180 seconds, and then a temperature gradient was formed by the same method as in Example 1 (specifically, hot air (wind speed 25 m / min) with a temperature gradient decreasing from the right end side to the left end side of the film was blown to the film for 180 seconds while being adjusted from upstream to downstream in the conveying direction in such a manner that the right end side was reduced from 140°C to 125°C and the left end side was reduced from 140°C to 111°C). A stretched film was obtained in the same manner as in Example 1. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0157] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 14° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0158] <Example 3>

[0159] At the beginning of the heat fixing area D, hot air at 140°C was blown uniformly in the width direction at a wind speed of 23 m / min for 180 seconds, and then a temperature gradient was formed by the same method as in Example 1 (specifically, hot air (wind speed 23 m / min) with a temperature gradient decreasing from the right end side to the left end side of the film was blown to the film for 180 seconds while being adjusted from upstream to downstream in the conveying direction in such a manner that the right end side was reduced from 140°C to 125°C and the left end side was reduced from 140°C to 118°C). A stretched film was obtained in the same manner as in Example 1. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0160] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 7° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0161] <Example 4>

[0162] At the beginning of the heat fixing area D, hot air at 140°C was blown uniformly in the width direction at a wind speed of 20 m / min for 180 seconds, and then a temperature gradient was formed by the same method as in Example 1 (specifically, hot air (wind speed 20 m / min) with a temperature gradient decreasing from the right end side to the left end side of the film was blown to the film for 180 seconds while being adjusted from upstream to downstream in the conveying direction in such a manner that the right end side was reduced from 140°C to 130°C and the left end side was reduced from 140°C to 115°C). A stretched film was obtained in the same manner as in Example 1. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0163] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 15° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0164] <Example 5>

[0165] At the beginning of the heat fixing area D, hot air at 140°C was blown uniformly in the width direction at a wind speed of 25 m / min for 180 seconds, and then a temperature gradient was formed by the same method as in Example 1 (specifically, hot air (wind speed 25 m / min) having a temperature gradient decreasing from the right end side to the left end side of the film was blown to the film for 180 seconds while being adjusted from upstream to downstream in the conveying direction in such a manner that the temperature decreases from 140°C to 115.5°C on the right end side and from 140°C to 115°C on the left end side). A stretched film was obtained in the same manner as in Example 1 except that the phase difference Re(550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0166] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in the temperature gradient area was 0.5°C, and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0167] <Example 6>

[0168] A stretched film was obtained in the same manner as in Example 2 except that the wind speed of the hot air was 20 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0169] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 14° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0170] <Example 7>

[0171] A stretched film was obtained in the same manner as in Example 4 except that the wind speed of the hot air was 25 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0172] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 15° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0173] <Example 8>

[0174] A stretched film was obtained in the same manner as in Example 4 except that the wind speed of the hot air was 10 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0175] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 7° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0176] <Example 9>

[0177] A stretched film was obtained in the same manner as in Example 2 except that the wind speed of the hot air was 30 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0178] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 14° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0179] <Example 10>

[0180] A stretched film was obtained in the same manner as in Example 2 except that the wind speed of the hot air was 35 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0181] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side was higher than the temperature on the left side relative to the center in the width direction of the film. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 14° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0182] <Example 11>

[0183] A stretched film was obtained in the same manner as in Example 1 except that the wind speed of the hot air was 23 m / min. The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0184] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, a temperature gradient area was formed in which the temperature on the right side relative to the center of the width direction of the film was higher than the temperature on the left side. The maximum value of the temperature difference between the two ends in the width direction in this temperature gradient area was 10° C., and the direction in which the isotherm with the largest angle relative to the width direction was extended was the oblique direction (the direction with an angle of 3° relative to the slow axis direction of the obtained stretched film).

[0185] <Comparative Example 1>

[0186] A stretched film was obtained in the same manner as in Example 1 except that hot air at 140°C was blown uniformly in the width direction at a wind speed of 20 m / min at the beginning of the heat setting region D, and then heat setting was performed following the ambient temperature (as a result, a temperature gradient in the oblique direction was not formed). The phase difference Re (550) of the obtained stretched film was 147 nm, and the angle between the slow axis direction and the longitudinal direction was 45°.

[0187] In addition, when the temperature of the heat fixing area was measured in the same manner as in Example 1, the temperature was uniform in the width direction and no oblique temperature gradient area was formed (more specifically, the isotherms were parallel to the width direction and a temperature gradient was formed in which the temperature decreased toward the conveying direction).

[0188] [Appearance and handling evaluation]

[0189] The stretched films obtained in the above-mentioned examples and comparative examples were laminated to a long strip of masking film (manufactured by Toray Film Processing Co., Ltd., product name "Toretec 7832C-30") in a roll-to-roll manner to obtain a film laminate. Next, the masking film was peeled off from the film laminate, an adhesive was applied using a gravure coater, and the film laminate was laminated to a polarizer and irradiated with UV to obtain an optical laminate. The appearance (visual) of the optical laminate and the handling properties of the stretched film were evaluated according to the following criteria.

[0190] ○: After laminating the masking film (laminating tension 150 N / m), no wrinkles were observed, and the adhesive could be applied to the entire surface of the film.

[0191] △: When laminating the masking film, the laminating tension was increased to 300 N / m, so that the masking film could be laminarized without wrinkles. However, when applying the adhesive, the adhesive could not be applied to the slackened portion.

[0192] ×: After the masking film was attached, there were wrinkles and the appearance was deteriorated.

[0193] [Wrinkle evaluation]

[0194] The wrinkles of the obtained stretched film were evaluated according to the following criteria.

[0195] ○: No wrinkles were observed even when irradiated with a Purulite lamp (manufactured by Purulite, product number "NP-1").

[0196] △: Even when illuminated by fluorescent light, wrinkles are not visible, but when illuminated by Purui light, wrinkles are visible.

[0197] ×: Wrinkles are visible when illuminated with fluorescent light.

[0198] [Evaluation of transportability]

[0199] The obtained stretched film was visually checked for deformation or folds caused by sag and / or wrinkles, and evaluated based on the following criteria.

[0200] ○: No deformation or crease occurred in the film.

[0201] ×: Deformation and / or creases occurred in the film.

[0202] [Visibility Evaluation]

[0203] The optical laminate prepared in the above appearance and handling evaluation was bonded to the visible side of a reflector or an organic EL panel via an adhesive layer. The obtained optical laminate was visually checked for uneven shape or light leakage due to sag or wrinkles, and evaluated according to the following criteria.

[0204] ○: No unevenness or light leakage was observed in both the reflector and the panel installation.

[0205] △: Unevenness and / or light leakage is visible in the reflector, but not in the panel installation.

[0206] ×: Unevenness and / or light leakage were observed in both the reflector and the panel.

[0207] Table 1 shows the sag amounts and the evaluation results of the stretched films obtained in the above Examples and Comparative Examples.

[0208]

[0209] <Evaluation>

[0210] As shown in Table 1, it is known that sag and / or wrinkles can be reduced by performing heat fixing in a heat fixing region having a temperature gradient region where the temperature of the end side held by the leading jig during oblique stretching is higher than the temperature of the other end side.

[0211] Industrial Applicability

[0212] The method for producing a stretched film of the present invention is preferably used for producing a phase difference film, and as a result, can contribute to the production of image display devices such as liquid crystal display devices (LCD) and organic electroluminescent display devices (OLED).

Claims

1. A method for producing a stretched film, comprising: The left and right ends of the long film in the width direction are held by using left and right clamps of a variable spacing type in which the clamp spacing in the longitudinal direction changes. The film is extended obliquely by moving the left and right clamps in a manner that describes a left-right symmetrical track while changing the clamp interval of at least one clamp; and The film is heat fixed. During the oblique extension, one of the left and right clamps is moved ahead of the other clamp. In the thermal fixation, a temperature gradient region is formed in which the temperature of the end portion of the film held by the preceding jig is higher than the temperature of the other end portion. In the temperature gradient region, the isothermal line extends obliquely toward the same side as the oblique extending direction with respect to the longitudinal direction of the film.

2. The method for producing a stretched film according to claim 1, wherein: The maximum value of the temperature difference between both ends in the width direction of the temperature gradient region is 0.3°C to 25°C.

3. The method for producing a stretched film according to claim 1 or 2, wherein: The temperature gradient region is formed by supplying hot air to the film.

4. The method for producing a stretched film according to claim 3, wherein: The wind speed of the hot air is 3m / min to 45m / min.

5. The method for producing a stretched film according to claim 1 or 2, wherein: The oblique extension includes: (i) increasing the clamp spacing of one clamp from P1 to P2, while reducing the clamp spacing of the other clamp from P1 to P3; and (ii) changing the clamp spacing of each clamp in such a way that the reduced clamp spacing and the increased clamp spacing become a specified equal spacing.

6. The method for producing a stretched film according to claim 5, wherein: P2 / P1 is 1.25 to 1.75, and P3 / P1 is 0.50 or more and less than 1.

7. A method for producing an optical layered body, comprising: obtaining a long-strip stretched film by the production method according to any one of claims 1 to 6; and While conveying the long optical film and the long stretched film, their length directions are aligned and they are continuously bonded together.

8. The method for producing an optical layered body according to claim 7, wherein: The optical film is a polarizing plate, and the stretched film is a λ / 4 plate or a λ / 2 plate.

Citation Information

Patent Citations

  • JP1973045619A

  • Automatic switching system for data transferring speed for common channel signaling device

    JP1988290032A

  • Optical film containing polymer having naphthyl group

    JP2007161994A

  • Clip type sheet and film extension device

    JP2008044339A

  • Polycarbonate resin and transparent film comprising the same

    JP2012067300A