A test method for evaluating the moisture sensitivity of road asphalt
By combining the internal water seepage patterns and surface roughness characteristics of asphalt, conducting immersion tests and spectral analysis at temperature, the problem of low efficiency of asphalt moisture sensitivity detection in existing methods is solved, a more accurate moisture sensitivity evaluation is provided, and the quality of asphalt is improved. Resistant to water damage and hydrophobic properties.
Patent Information
- Application Number
- CN202210913292.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-29
AI Technical Summary
The existing road asphalt moisture sensitivity evaluation method ignores the impact of the contact time between the asphalt film and moisture, resulting in low detection efficiency and inability to effectively improve the water damage resistance and surface hydrophobicity of asphalt.
By combining the internal water seepage laws and surface roughness characteristics of asphalt, heated asphalt samples were used to form a film, and immersion tests were conducted at different temperatures. An atomic force microscope and Fourier transform infrared spectrometer were used to measure the surface properties, and the physical water absorption index, chemical water absorption index and Average roughness, curves were drawn to evaluate the moisture sensitivity of bitumen.
It provides a more reasonable moisture sensitivity evaluation index, improves the water damage resistance and surface hydrophobicity of asphalt, and improves the accuracy of road construction and detection.
Smart Images

Figure CN115166222B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a method for evaluating the moisture sensitivity of road asphalt, and belongs to the technical field of performance detection of road engineering materials. Background Art
[0002] Asphalt pavement is widely used because of its good driving comfort, cleaning and easy maintenance. Compared with cement pavement with better durability, asphalt pavement is prone to aging. As of the end of 2020, the length of highways in Jiangsu Province that have been in operation for more than 10 years has reached 77%. Road asphalt materials undergo short-term aging and long-term aging during hot storage, construction mixing, transportation paving, and open use. The short-term aging process of asphalt is mainly the volatilization and oxygen absorption reaction of light components in a short period of time. In addition to thermal oxygen aging, the long-term aging process is also accompanied by multi-factor coupled aging such as ultraviolet light, water and driving load. The light components are further volatilized, and the unsaturated bonds are further oxygenated to generate functional groups such as carbonyl (C=O) and sulfoxide (S=O). The macroscopic characteristics are hardening and brittleness, and the viscosity increases. The aging of road asphalt is ongoing all the time, which has a great impact on the road performance of the road and seriously reduces the durability of the road surface.
[0003] In the case of rainwater, river water and groundwater infiltration, asphalt pavement will be subjected to water immersion, scouring and infiltration for a long time. At the same time, the instantaneous dynamic load of road vehicles will also produce instantaneous positive and negative high pressure, which will lead to loose asphalt pavement, pumping and asphalt mixture peeling, seriously affecting its road performance. In this environment, asphalt pavement will also face water intrusion damage when thermal oxidation aging occurs, which aggravates the aging of asphalt pavement. Some scholars also believe that when the temperature is low in winter, the water entering the pavement structure freezes into ice and expands in volume, which will destroy the adhesion of asphalt mixture; when the temperature is high in summer, water will penetrate into the asphalt along the damaged part of asphalt, causing the asphalt cohesion to weaken. However, according to research, the diffusion law of water in asphalt does not conform to Fick's diffusion law, which may be due to the aggregation of water molecules and the interaction between water molecules and asphalt functional groups. Mousavi used density functional theory to study the molecular mechanism of sensitivity between sulfur and water in asphalt. The results showed that the sensitivity of asphalt to water can be attributed to the hydrogen bond interaction between sulfoxide functional groups and water. In addition, under high temperature and high pressure, moisture will cause physical damage to the surface and interior of asphalt, accelerating the aging of asphalt by moisture and air. Other scholars have used FTIR to reveal that the concentration of polar components on the surface of asphalt increases after water infiltration, and used AFM to observe the changes in the surface morphology of asphalt when it comes into contact with water at high temperatures, and believe that the greater the surface roughness of the asphalt, the better the hydrophobic effect.
[0004] When water damage occurs on asphalt pavement, the first thing that water contacts is the asphalt film wrapped around the outer layer of aggregates. As water penetrates, the last thing that contacts is the surface of aggregates. Therefore, the sensitivity of asphalt to moisture is particularly important, which greatly affects the ability of asphalt pavement to resist water damage and water aging. However, there is currently insufficient research on the evaluation methods of asphalt's moisture sensitivity. The main evaluation method at present is to use the surface energy theory to test the contact angles of asphalt and aggregates, calculate the surface energy components of asphalt and aggregates, the cohesive work of asphalt, and the adhesion work of asphalt and aggregates to evaluate the hydrophobicity or moisture sensitivity of asphalt or aggregates. Some scholars have also conducted infrared spectroscopy tests on asphalt soaked in water, and calculated the area of the hydroxyl characteristic peak to characterize the moisture sensitivity of asphalt, but they ignore the influence of asphalt surface characteristics on moisture sensitivity.
[0005] Therefore, based on the internal water permeability law of asphalt and the surface roughness characteristics of asphalt, the present invention proposes a test method for evaluating the moisture sensitivity of road asphalt, which provides a reasonable moisture sensitivity evaluation index for road construction and road material testing, and also provides a reference for improving the asphalt's resistance to water damage and the asphalt's surface hydrophobicity. Summary of the invention
[0006] (1) Technical issues
[0007] The present invention aims to provide a test method for evaluating the moisture sensitivity of road asphalt, so as to solve the problem that the current test method for evaluating the moisture sensitivity of road asphalt ignores the effect of the contact time between the asphalt film and water on the moisture sensitivity of asphalt, and to provide a reasonable moisture sensitivity evaluation index for road construction and testing, while providing a reference for improving the water damage resistance of asphalt and the hydrophobicity of the asphalt surface.
[0008] (2) Technical solution
[0009] In view of the current unreasonable and single test methods for evaluating the moisture sensitivity of road asphalt, the present invention starts from the two aspects of the internal water permeability law of asphalt and the surface roughness characteristics, and provides a test method for evaluating the moisture sensitivity of road asphalt, so as to improve the efficiency of asphalt moisture sensitivity detection. The technical scheme of the present invention is as follows: first, the asphalt sample is heated to a flowing state, and a silicon wafer is used as a base film to prepare an asphalt film test and weigh it; then the asphalt film specimen is placed in a glass culture dish filled with distilled water, and immersed in environmental boxes at temperatures of 0°C, 30°C and 60°C to obtain a soaked asphalt film sample and weigh it; secondly, the asphalt film sample is tested by atomic force microscopy, and a three-dimensional structure diagram is drawn using NanoScope Analysis software, and the average surface roughness of the asphalt film sample is obtained at the same time, and then a Fourier infrared spectrometer is used to measure and obtain the hydroxyl index and sulfoxide index; finally, the curves of the asphalt physical water absorption index, chemical water absorption index and average roughness with respect to temperature are drawn, such as Figure 1 , in order to evaluate the sensitivity of asphalt to moisture at different temperatures.
[0010] (3) Beneficial effects
[0011] In the case of rainwater and groundwater infiltration, some asphalt pavements will be soaked, scour, and penetrated by water for a long time. The instantaneous dynamic load of road vehicles will also generate instantaneous pressure, which will lead to loose asphalt pavement, pumping and asphalt mixture peeling, which seriously affects its road performance. When water damage occurs on asphalt pavement, the first thing that water contacts is the asphalt film wrapped around the outer layer of aggregate. Therefore, the sensitivity of asphalt to moisture is particularly important. At present, the evaluation method for asphalt moisture sensitivity is to use surface energy theory to measure the contact angle of asphalt or, thereby calculating the cohesive work of asphalt and the adhesion work of asphalt and aggregate; or to perform infrared spectroscopy test on asphalt after water immersion, and calculate the area of hydroxyl characteristic peak to characterize the moisture sensitivity of asphalt. The present invention provides a road asphalt moisture sensitivity evaluation test method, which starts from the two aspects of the internal water seepage law of asphalt and the surface roughness characteristics, solves the problem of unreasonable and single road asphalt moisture sensitivity evaluation test method, provides reasonable moisture sensitivity evaluation indicators for road construction and detection, and provides a reference for improving asphalt's resistance to water damage and surface hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Change curves of physical water absorption index, chemical water absorption index and average roughness of base asphalt at different temperatures
[0013] 1- immersion temperature (℃), 2- physical water absorption index PA, 3- chemical water absorption index CA / average roughness R a , 4-PA curve, 5-CA curve, 6-R a curve. DETAILED DESCRIPTION
[0014] The present invention provides a road asphalt moisture sensitivity evaluation test method, and the specific implementation steps are as follows:
[0015] (1) Place the asphalt sample in an oven and heat it until it flows. Take 2 drops of asphalt and drop them on a clean glass slide. Place it on a 135°C constant temperature electric heating plate to keep it warm. Take a silicon wafer with a length and width of 20 mm, a thickness of 1.5 mm, and a mass of m1. Place the polished surface of the silicon wafer facing down on the asphalt. Use metal tweezers to gently press and pick up the silicon wafer so that the surface of the silicon wafer is evenly stained with asphalt. Place it in an oven at 135°C and heat it for 10 min to form a smooth and flat asphalt film on the asphalt on the silicon wafer. Prepare the asphalt film sample and weigh it as m2.
[0016] (2) Soak the asphalt film sample in a glass culture dish filled with distilled water and cover it with a glass cover. Then, place the glass culture dish in an environmental chamber at 0°C, 30°C, and 60°C for 32 hours to obtain a water-soaked asphalt film sample. Take out the asphalt film sample and place it in a drying dish at room temperature for 1 hour before taking it out and weighing it as m3;
[0017] (3) In order to evaluate the effect of water molecules on the micro-surface of the asphalt film, an atomic force microscope was used to test the asphalt film sample. The test area was a square area of 20 μm × 20 μm. The test mode was the tapping mode. The NanoScope Analysis software was used to draw the three-dimensional structure of the asphalt film surface and obtain the average surface roughness R of the asphalt film sample. a ;
[0018] (4) The asphalt film sample was tested using a Fourier transform infrared spectrometer, and the characteristic peak area A of the hydroxyl group on the infrared spectrum was obtained by integration calculation based on the Origin software. 3300 , sulfoxide characteristic peak area A 1029 and saturated carbon-hydrogen bond absorption peak area A 1374 ;
[0019] (5) Calculate the physical water absorption index PA and chemical water absorption index CA of asphalt according to formula (I) and formula (II) respectively.
[0020]
[0021]
[0022] Where, m1 is the mass of silicon wafer, m2 is the mass of asphalt film sample before immersion, m3 is the mass of asphalt film sample after immersion, A 3300 -Hydroxyl absorption peak area, A 1374 -Saturated carbon-hydrogen bond absorption peak area, A 1029 ——Sulfoxide absorption peak area;
[0023] (6) Plot PA, CA and R at three temperatures: 0℃, 30℃ and 60℃ a The change curve of the asphalt water sensitivity index K is the sum of the slopes of the three curves in the temperature range of 30-60°C and the slopes in the temperature range of 0-30°C, as shown in formula (III).
[0024]
[0025] In the formula, K P′ The slope of PA in the range of -30-60℃, K P - The slope of PA in the range of 0-30℃, K C′ -30-60℃ range CA slope, K C - The slope of CA in the range of 0-30℃, KR′ -30-60℃ range R a The slope, K R -0-30℃ range R a The slope of the K value is as follows: the larger the K value, the greater the moisture sensitivity of the asphalt, and the more hydrophilic the asphalt, thereby evaluating the moisture sensitivity of the asphalt.
Claims
1. A road asphalt moisture sensitivity evaluation test method, characterized in that The specific implementation steps of this method are as follows: (1) Place the asphalt sample in an oven and heat it until it flows. Take 2 drops of asphalt and drop them on a clean glass slide. Place it on a 135°C constant temperature electric heating plate to keep it warm. Take a silicon wafer with a length and width of 20 mm, a thickness of 1.5 mm, and a mass of m1. Place the polished surface of the silicon wafer facing down on the asphalt. Use metal tweezers to gently press and pick up the silicon wafer so that the surface of the silicon wafer is evenly stained with asphalt. Place it in an oven at 135°C and heat it for 10 min to form a smooth and flat asphalt film on the asphalt on the silicon wafer. Prepare the asphalt film sample and weigh it as m2. (2) Soak the asphalt film sample in a glass culture dish filled with distilled water and cover it with a glass cover. Then, place the glass culture dish in an environmental chamber at 0°C, 30°C, and 60°C for 32 hours to obtain a water-soaked asphalt film sample. Take out the asphalt film sample and place it in a drying dish at room temperature for 1 hour before taking it out and weighing it as m3; (3) In order to evaluate the effect of water molecules on the micro-surface of the asphalt film, an atomic force microscope was used to test the asphalt film sample. The test area was a square area of 20 μm × 20 μm. The test mode was the tapping mode. The NanoScope Analysis software was used to draw the three-dimensional structure of the asphalt film surface and obtain the average surface roughness R of the asphalt film sample. a ; (4) The asphalt film sample was tested using a Fourier transform infrared spectrometer, and the characteristic peak area A of the hydroxyl group on the infrared spectrum was obtained by integration calculation based on the Origin software. 3300 , sulfoxide characteristic peak area A 1029 and saturated carbon-hydrogen bond absorption peak area A 1374 ; (5) Calculate the physical water absorption index PA and chemical water absorption index CA of asphalt according to formula (I) and formula (II) respectively. Where, m1 is the mass of silicon wafer, m2 is the mass of asphalt film sample before immersion, m3 is the mass of asphalt film sample after immersion, A 3300 -Hydroxyl absorption peak area, A 1374 -Saturated carbon-hydrogen bond absorption peak area, A 1029 ——Sulfoxide absorption peak area; (6) Plot PA, CA and R at three temperatures: 0℃, 30℃ and 60℃ a The change curve of the asphalt water sensitivity index K is the sum of the slopes of the three curves in the temperature range of 30-60°C and the slopes in the temperature range of 0-30°C, as shown in formula (III). In the formula, K P′ The slope of PA in the range of -30-60℃, K P - The slope of PA in the range of 0-30℃, K C′ -30-60℃ range CA slope, K C - The slope of CA in the range of 0-30℃, K R′ -30-60℃ range R a The slope, K R -0-30℃ range R a The slope of the K value is as follows: the larger the K value, the greater the moisture sensitivity of the asphalt, and the more hydrophilic the asphalt, thereby evaluating the moisture sensitivity of the asphalt.
Citation Information
Patent Citations
Asphalt time-temperature sensitivity test and evaluation method based on dissipated energy change
CN114235890A
Cited By
Low-porosity composite material continuous fiber 3D printing manufacturing device and method with adjustable magnetic filler space orientation partition
CN122500946A
Magnetic filler spatially oriented zoned adjustable low porosity composite continuous fiber 3d printing manufacturing apparatus and method
CN122500946B