A perovskite film with two-dimensional and three-dimensional multi-level structure and its method and application
By embedding amine ligand molecules on the three-dimensional surface of perovskite solar cells and using their hydrogen bond interaction with organic ammonium salts, the growth of the domain-limited two-dimensional perovskite layer is solved. The problems of degraded photoelectric performance and poor stability have achieved efficient and stable perovskite solar cells, with an efficiency of 24.72% and maintaining working stability for 1,000 hours.
Patent Information
- Application Number
- CN202210953942.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-10
AI Technical Summary
Existing perovskite solar cells have a large number of defects on the three-dimensional surface, resulting in a decrease in photoelectric performance and poor stability under water and gas environment and light conditions. The efficiency of traditional two-dimensional three-dimensional multi-level structures is still lagging behind in the inverse structure.
The amine ligand molecules are embedded on the surface of three-dimensional perovskites. Through the strong hydrogen bond interaction between the amine ligand and the organic ammonium salt, the growth of the domain-limited two-dimensional perovskite layer is formed, forming a two-dimensional three-dimensional multi-level confined amine ligand domain-limited two-dimensional multi-level Structure, regulates the exchange of cations and the formation of two-dimensional layers, and improves the passivation effect.
The photoelectric conversion efficiency and stability of perovskite solar cells have been significantly improved, and the open circuit voltage and filling factor have been significantly improved, achieving efficient and stable inverse perovskite solar cells with an efficiency of 24.72%, and maintaining stable operation within 1,000 hours. sex.
Smart Images

Figure CN115172614B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of solar cells, and in particular relates to a perovskite film with a two-dimensional and three-dimensional multi-level structure, and a method and application thereof. Background Art
[0002] Solar cells can be used to convert solar energy into electrical energy, providing people with the energy they need, so achieving efficient conversion of solar energy into electrical energy is of great research significance. Silicon-based solar cells have mature manufacturing technology and stable product performance, and are currently the most mature system. However, expensive raw materials have become a bottleneck in their development, and the single-cell efficiency of silicon cells has also reached its limit. Therefore, developing new solar cell structures to replace silicon cells or to stack them has been a research hotspot in many fields in recent years.
[0003] Three-dimensional (3D) organic-inorganic metal halide perovskite materials have a series of excellent optoelectronic properties, such as long carrier diffusion distance, high extinction coefficient, high defect tolerance, etc., and can be prepared by a low-cost and simple solution method. All-solid-state perovskite solar cells have achieved rapid development. At present, the photoelectric conversion efficiency of positive-structure perovskite solar cells (PVSCs) has exceeded 25%. PVSCs have now become the leader of low-cost and high-efficiency solar cells and the most anticipated next-generation photovoltaic materials. At present, improving the efficiency and stability of PVSCs is an important research topic in this field. A large number of defects on the surface and grain boundaries of 3D perovskites will become non-radiative recombination centers, resulting in a decrease in the open-circuit voltage and fill factor of the device, thereby affecting the optoelectronic performance; in addition, in a water vapor environment and light conditions, ion migration and moisture will slowly penetrate through the surface / interface defects and destroy the perovskite.
[0004] In the existing technology, small molecule organic compounds containing heteroatoms can be developed to effectively passivate the surface / interface defects of three-dimensional perovskites and improve the efficiency and stability of PVSCs. Among the many passivators, the action mechanism of small molecule organic ammonium salts is relatively special. They are easy to form two-dimensional perovskites on the surface or grain boundaries of three-dimensional perovskites, that is, two-dimensional three-dimensional multi-level structures. This strategy can effectively passivate the surface / interface cation and halide vacancy defects of three-dimensional perovskites and improve the photoelectric conversion efficiency and stability of devices. However, current studies have shown that in positive-type perovskite devices, the growth of a two-dimensional perovskite layer on the surface of three-dimensional perovskites can passivate defects and help block electrons, thereby greatly improving the photoelectric conversion efficiency of the device. Although this technology can be applied to inverse-type devices with better stability and more suitable for commercialization, it can increase the open circuit voltage, but it will significantly reduce the fill factor and current, which ultimately leads to the efficiency of inverse-type devices still lagging behind that of positive-type devices. Therefore, it is very important to develop a new two-dimensional layer confined growth process based on the traditional two-dimensional three-dimensional multi-level structure system to achieve efficient and stable perovskite solar cells. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention proposes a perovskite film with a two-dimensional and three-dimensional multi-level structure, a method and application thereof, and can prepare a highly efficient and stable battery device. Using the preparation process proposed in the present invention, amine ligand molecules are first pre-embedded on the surface of the three-dimensional perovskite, and the two-dimensional layer perovskite growth is confined on the surface of the three-dimensional perovskite through the strong hydrogen bond interaction between the amine ligand and the organic ammonium salt, thereby developing a high-efficiency perovskite solar cell with a two-dimensional and three-dimensional multi-level structure confined by the amine ligand.
[0006] The specific technical solutions adopted by the present invention are as follows:
[0007] In the first aspect, the present invention provides a method for preparing a perovskite film having a two-dimensional and three-dimensional multi-level structure, as follows:
[0008] A first solution containing amine ligands is deposited on the surface of a three-dimensional perovskite, and annealing treatment is performed to complete the pre-embedding of amine molecules on the surface of the three-dimensional perovskite to obtain a preliminary film; a second solution containing an organic ammonium salt is then deposited on the preliminary film, and annealing treatment is performed to complete the growth of a confined two-dimensional perovskite layer to obtain a two-dimensional and three-dimensional multi-level structure perovskite film.
[0009] Among them, the amine molecules pre-buried in the surface of the three-dimensional perovskite can interact with ammonium salts through strong hydrogen bonds, effectively regulating the exchange of cations during the formation of the two-dimensional layer and constructing a thin and dense two-dimensional layer.
[0010] Preferably, the three-dimensional perovskite is an ABX3 type perovskite, wherein the A position is a cesium ion (Cs + ), methylamine cation (MA + ), formamidinium cation (FA + ) is a mixture of one or more of the following: the B position is lead ion (Pb 2+ ), X is a chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) or a combination of one or more thereof.
[0011] Preferably, the amine ligand is one or more of ethylenediamine, propylenediamine and butylenediamine, and the solvent of the first solution is at least one of toluene and chlorobenzene.
[0012] Preferably, the organic ammonium salt is at least one of an aromatic ring and an alkyl chain ammonium salt, and the solvent of the second solution is at least one of isopropanol and chlorobenzene.
[0013] Preferably, the annealing temperature used in preparing the preliminary film is 60-80°C, preferably 70-80°C.
[0014] Preferably, the annealing temperature used to prepare the two-dimensional and three-dimensional multi-level structure perovskite film is 100-120°C, preferably 100-110°C.
[0015] Preferably, the concentration of the amine ligand in the first solution is 0.1-0.2 mM, and the concentration of the organic ammonium salt in the second solution is 1-4 mg / mL.
[0016] In a second aspect, the present invention provides a perovskite film having a two-dimensional or three-dimensional multi-level structure obtained by any preparation method described in the first aspect.
[0017] In a third aspect, the present invention provides a perovskite solar cell device with a two-dimensional and three-dimensional multi-level structure, which is a multi-layered structure, and is stacked with a substrate, a transparent electrode layer, a hole transport layer, a photoactive layer, an electron transport layer, a work function adjustment layer and a metal electrode layer from bottom to top; wherein the photoactive layer is the perovskite film with a two-dimensional and three-dimensional multi-level structure as described in the second aspect.
[0018] Preferably, the substrate material is one of glass, quartz, flexible PET or flexible PEN; the transparent electrode layer material is indium tin oxide or fluorine-doped tin oxide; the hole transport layer material is one of nickel oxide, PTAA, PEDOT or Poly-TPD, more preferably NiO x and PTAA double-layer structure; the electron transport layer material is PCBM, C 60 or zinc dioxide; the work function adjustment layer material is BCP; the metal electrode layer material is silver, aluminum, magnesium, copper, gold, indium tin oxide or fluorine-doped tin oxide, and the thickness is 50 to 300 nm.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1) The present invention pre-buries amine ligand molecules on the surface of three-dimensional perovskite, and utilizes its strong hydrogen bond interaction with organic ammonium salt ligands to confine the growth of two-dimensional perovskite on the three-dimensional perovskite film, while retaining the passivation of the two-dimensional layer on the top of the three-dimensional perovskite, further improving the charge transfer performance of the two-dimensional and three-dimensional heterogeneous interface, greatly improving the efficiency of the two-dimensional and three-dimensional multi-level structure inversion perovskite battery device.
[0021] 2) The present invention successfully regulates the exchange of cations during the growth of two-dimensional perovskite through a "two-dimensional confined growth" processing technology, so that the concentration of organic ammonium salt can be prepared in the range of 1-4mg / mL to produce devices with an average efficiency greater than 20%. Compared with the reference device of the traditional two-dimensional three-dimensional multi-level structure perovskite (i.e., no amine ligand molecules are pre-embedded on the three-dimensional perovskite film), the open circuit voltage and fill factor of the confined two-dimensional three-dimensional multi-level structure inverted perovskite solar cell device are significantly improved. Among them, the concentration of the amine ligand molecules pre-embedded on the surface of the three-dimensional perovskite is 0.1-0.2mM. When the concentration of the pre-embedded amine ligand molecules is 0.1mM, the open circuit voltage of the prepared confined two-dimensional three-dimensional multi-level structure perovskite solar cell device is as high as 1.20V, which is one of the highest voltages of perovskite solar cells with a band gap of 1.55eV reported so far.
[0022] 3) The present invention found that pre-embedded amine ligand molecules on the surface of three-dimensional perovskite can effectively passivate the defects on the surface of perovskite, inducing the growth of a thin and dense two-dimensional layer on the three-dimensional perovskite, thereby improving the photoelectric conversion efficiency and stability of the device. Finally, based on mixed cation perovskite, the inverted solar cell device prepared using confined two-dimensional and three-dimensional multi-level structure perovskite showed an efficiency of 24.72% (V OC =1.20V,J SC =25.22mA / cm 2 ,FF=81.92) and 1000 hours of working stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the structure of a perovskite solar cell device with a two-dimensional and three-dimensional multi-level structure.
[0024] Figure 2 Based on Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 system perovskite solar cell device current-voltage curve.
[0025] Figure 3 Based on Cs 0.1 FA 0.7 MA 0.2 Pb(I 0.55 Br 0.45 )3’s current-voltage curve of the perovskite solar cell device.
[0026] Figure 4 Based on Cs 0.05 (FA 0.95 MA 0.05) 0.95 Pb(I 0.95 Br 0.05 )3 system perovskite solar cell device working stability curve.
[0027] Figure 5 Based on Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 are scanning electron microscope (SEM) plan views of the perovskite film of the system, wherein Figure (a) is the plan SEM view of the perovskite film prepared by the method of Comparative Example 1, and Figure (b) is the plan SEM view of the perovskite film prepared by the method of Example 1. DETAILED DESCRIPTION
[0028] The present invention is further described and illustrated below in conjunction with the accompanying drawings and specific embodiments. The technical features of each embodiment of the present invention can be combined accordingly without conflicting with each other.
[0029] In a preferred embodiment of the present invention, a confined two-dimensional three-dimensional multi-level structure perovskite film is first provided. The confined two-dimensional three-dimensional multi-level structure specifically refers to the strong hydrogen bond interaction between the amine molecules pre-buried on the surface of the three-dimensional perovskite and the organic ammonium salt ligand to regulate the cation exchange during the growth of the two-dimensional perovskite and then regulate the penetration depth of the organic ammonium salt cations in the three-dimensional perovskite film, so as to realize the preparation of a thin and dense two-dimensional perovskite layer on the top of the three-dimensional perovskite. The perovskite is an ABX3 type perovskite, and the A position is a cesium ion (Cs + ), methylamine cation (MA + ), formamidinium cation (FA + ) is a mixture of one or more of the following: the B position is lead ion (Pb 2+ ), X is a chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) or a combination of one or more thereof.
[0030] The above-mentioned perovskite film with two-dimensional and three-dimensional multi-level structure can be prepared by the following method:
[0031] 1) Amine molecules are pre-buried on the surface of the three-dimensional perovskite film, and the perovskite contained in the three-dimensional perovskite component is the aforementioned ABX3 type perovskite.
[0032] The solvent used in the amine molecule solution should not be able to dissolve ABX3, so as to ensure that the three-dimensional perovskite film is not damaged and the subsequent amine molecules are successfully pre-embedded on the three-dimensional perovskite surface. The solvents that can be selected in the present invention include but are not limited to toluene or chlorobenzene or any mixture of the two.
[0033] In the amine molecule solution, the concentration of the amine molecules can be optimized according to actual conditions. Preferably, the concentration of the amine in the amine molecule solution can be controlled to be 0.1-0.2 mM.
[0034] 2) Using a solution containing amine molecules to form a film on the three-dimensional perovskite dry film, the film formation method can be a spin coating method, the amine molecule solution is spin-coated onto the three-dimensional perovskite film, and annealing treatment is performed to obtain a three-dimensional perovskite film (i.e., a preparatory film) with amine molecules pre-embedded on the surface.
[0035] The solvent removal treatment method for obtaining the three-dimensional perovskite film with amine molecules pre-embedded on the surface can be an annealing process. The annealing temperature can be controlled to be 60-80°C, more preferably 70-80°C, and the higher the temperature, the shorter the time needs to be controlled.
[0036] In the present invention, since amine molecules are unstable in the air, the operation of pre-embedding amine molecules on the surface of the three-dimensional perovskite needs to be completed in a glove box.
[0037] 3) Using a solution containing an organic ammonium salt ligand to form a film on a three-dimensional perovskite film with amine molecules pre-buried on the surface, the film formation method can be a spin coating method, wherein the organic ammonium salt ligand solution is spin-coated onto the perovskite film, and annealing treatment is performed to obtain a confined two-dimensional and three-dimensional multi-level structure perovskite film.
[0038] In this step, the annealing temperature needs to be optimized according to actual conditions, and can generally be controlled between 120 and 110°C, preferably 100 to 110°C.
[0039] It can be seen that the present invention can pre-bury amine molecules on the surface of the three-dimensional perovskite film, and through the strong hydrogen bond interaction between the amine molecules and the organic ammonium salt, the penetration depth of the organic ammonium salt cations in the three-dimensional perovskite is slowed down, while retaining the passivation of the top defects of the three-dimensional perovskite, a two-dimensional perovskite passivation layer that is more conducive to charge transfer is obtained.
[0040] In the present invention, it is preferred that the above-mentioned two-dimensional perovskite layer is coated on the three-dimensional perovskite surface pre-embedded with amine ligands during the preparation process of the perovskite solar cell, and the penetration depth of the organic ammonium salt on the three-dimensional perovskite surface is regulated by the strong hydrogen bond interaction between the amine ligand and the organic ammonium salt, so as to form a confined two-dimensional and three-dimensional multi-level structure perovskite solar cell device. The specific structural form of the perovskite solar cell device is not limited, and a preferred structural form is provided below.
[0041] like Figure 1As shown, in this form, the solar cell device is a multi-layer structure, which includes, from bottom to top, a substrate 1, a transparent electrode layer 2, a hole transport layer 3, a photoactive layer 4, an electron transport layer 5, a work function adjustment layer 6, and a metal electrode layer 7. Among them, the photoactive layer 4 is the above-mentioned confined two-dimensional three-dimensional multi-level structure perovskite (i.e., a perovskite film with a two-dimensional three-dimensional multi-level structure). The remaining structural layers can be adjusted according to actual conditions without limitation.
[0042] As a preferred combination, the specific selection of materials for each layer is as follows: substrate 1 is glass; transparent electrode layer 2 is ITO; hole transport layer 3 is NiO x +PTAA double-layer structure; the electron transport layer is PCBM; the work function adjustment layer is BCP, and the cathode is silver. The preparation process of the solar cell is as follows:
[0043] The transparent conductive glass with strips of ITO (anode) etched on the surface was cleaned with detergent, deionized water, acetone and isopropanol ultrasonic oscillation for 15 minutes, dried with nitrogen flow, and then treated with ultraviolet ozone for 20 minutes; then a layer of NiO was spin-coated x The solution was annealed at 110°C for 10-15 min, and then sintered at 350°C for 1 h. The solution was then transferred to a nitrogen glove box without water or oxygen and PTAA was spin-coated on the NiO x The hole transport layer was obtained by annealing at 100°C for 10 min. The hole transport layer was then used as a substrate to prepare a three-dimensional perovskite film according to the aforementioned preparation process. EDA (ethylenediamine) molecules were pre-embedded on the dry film, and then an organic ammonium salt ligand solution was deposited to prepare a two-dimensional perovskite layer. The electron transport layer (PCBM) and the hole blocking layer (BCP) were then spin-coated at a speed of 3000 rpm. Finally, an Ag electrode with a thickness of 80-100 nm was evaporated on the BCP by an evaporator to obtain a perovskite solar cell device with a two-dimensional and three-dimensional multi-level structure.
[0044] The following will demonstrate the effect of the confined two-dimensional and three-dimensional multi-level structure perovskite of the present invention by comparing two embodiments and two ordinary perovskite solar cell devices. Wherein in Example 1, a confined two-dimensional and three-dimensional multi-level structure perovskite is constructed in a medium bandgap perovskite component, and in Example 2, a confined two-dimensional and three-dimensional multi-level structure perovskite is constructed in a wide bandgap perovskite system. It should be pointed out that the following embodiments are only the best embodiments when the device of the present invention is used as a confined two-dimensional and three-dimensional multi-level structure perovskite solar cell device, but are not intended to limit the scope of protection of the present invention. Those skilled in the art can adjust the composition of the perovskite active layer, the configuration of the battery, the temperature and time of the annealing process, etc. according to actual conditions, and further optimize as needed.
[0045] Comparative Example 1
[0046] Using FAI, MABr, PbBr, PbI2 and CsI as raw materials, Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 solution, the solvent is a mixed solvent of DMF and DMSO (4:1 / v:v), the concentration is 1.4M, 30 mol% MACl is added to obtain a perovskite precursor solution, and the precursor solution is used for subsequent spin coating.
[0047] The transparent conductive glass with strips of ITO (anode) etched on the surface was cleaned with detergent, deionized water, acetone and isopropanol ultrasonic oscillation for 15 minutes, dried with nitrogen flow, and then treated with ultraviolet ozone for 20 minutes; then a layer of NiO was spin-coated x The solution (spin coating parameters were 4000 rpm for 30 s) was annealed at 110 °C for 15 min; then it was transferred to a hot plate at 350 °C for 1 h, and then transferred to a nitrogen glove box environment without water or oxygen, and a 1.5 mg / mL PTAA toluene solution was spin coated on the NiO x The film was annealed at 100 °C for 10 min to obtain a hole transport layer.
[0048] During spin coating, 60 microliters of perovskite precursor solution was quickly dripped on the hole transport layer, and the spin coating rate was set to 4000 rpm for 40 seconds. 120 microliters of isopropanol was added 30 seconds after the start of spin coating. After the spin coating stopped, the film was placed on a hot stage at 100°C for annealing for 30 minutes. After cooling, an organic ammonium salt solution (solvent is isopropanol, concentration is 2 mg / mL) was spin-coated at a speed of 5000 rpm. The film was placed on a hot stage at 100°C for annealing for 5 minutes. After cooling, PCBM (solvent is chlorobenzene, concentration is 20 mg / mL) and BCP (solvent is ethanol, concentration is 0.5 mg / mL) were spin-coated at a speed of 3000 rpm. Finally, an Ag electrode with a thickness of 80-100 nm was evaporated on the BCP using an evaporator to obtain a Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 is a perovskite solar cell device with an active layer.
[0049] At a light intensity of 100 mW / cm 2 The current-voltage curve of the device was tested under AM1.5G simulated sunlight, and the open circuit voltage (V OC ) is 1.17V, and the short-circuit current density (Jsc) is 23.71mA / cm 2, the fill factor (FF) is 76.03, and the photoelectric conversion efficiency (PCE) is 21.10%. Figure 2 Ref in is the current-voltage curve of the device. Figure 5 Ref in is the planar SEM image of the perovskite film with this structure.
[0050] Example 1
[0051] Using FAI, MABr, PbBr, PbI2 and CsI as raw materials, Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 solution, the solvent is a mixed solvent of DMF and DMSO (4:1 / v:v), the concentration is 1.4M, 30 mol% MACl is added to obtain a perovskite precursor solution, and the precursor solution is used for subsequent spin coating.
[0052] The transparent conductive glass with strips of ITO (anode) etched on the surface was cleaned with detergent, deionized water, acetone and isopropanol ultrasonic oscillation for 15 minutes, dried with nitrogen flow, and then treated with ultraviolet ozone for 20 minutes; then a layer of NiO was spin-coated x The solution (spin coating parameters were 4000 rpm for 30 s) was annealed at 110 °C for 15 min; then it was transferred to a hot plate at 350 °C for 1 h, and then transferred to a nitrogen glove box environment without water or oxygen, and a 1.5 mg / mL PTAA toluene solution was spin coated on the NiO x The film was annealed at 100 °C for 10 min to obtain a hole transport layer.
[0053] During spin coating, 60 microliters of perovskite precursor solution was quickly dripped on the hole transport layer, and the spin coating rate was set to 4000 rpm for 40 seconds. 120 microliters of isopropanol was added 30 seconds after the start of spin coating. After the spin coating stopped, the film was placed on a hot stage at 100°C for annealing for 30 minutes. After cooling, the EDA solution was spin-coated at a speed of 4000 rpm. The film was placed on a hot stage at 70°C for annealing for 5 minutes. After cooling, the organic ammonium salt solution (solvent is isopropanol, concentration is 2 mg / mL) was spin-coated at a speed of 5000 rpm. The film was placed on a hot stage at 100°C for annealing for 5 minutes. After cooling, PCBM (solvent is chlorobenzene, concentration is 20 mg / mL) and BCP (solvent is ethanol, concentration is 0.5 mg / mL) were spin-coated at a speed of 3000 rpm. Finally, an Ag electrode with a thickness of 80-100 nm was evaporated on the BCP using an evaporator to obtain a Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I0.95 Br 0.05 )3 is a perovskite solar cell device with an active layer.
[0054] At a light intensity of 100 mW / cm 2 The current-voltage curve of the device was tested under AM1.5G simulated sunlight, and the open circuit voltage (V OC ) is 1.20V, and the short-circuit current density (Jsc) is 25.20mA / cm 2 , the fill factor (FF) is 81.19 and the photoelectric conversion efficiency (PCE) is 24.72%. Figure 2 The Target in is the current-voltage curve of the device. Figure 4 The Target in is the working stability curve of the device prepared by this example method. Figure 5 The Target in the figure is the planar SEM image of the perovskite film prepared by the method of this example.
[0055] Comparative Example 2
[0056] Using FAI, MABr, PbBr, PbI2 and CsI as raw materials, Cs 0.1 FA 0.7 MA 0.2 Pb(I 0.55 Br 0.45 )3 solution, the solvent is a mixed solvent of DMF and DMSO (3:2 / v:v), and the concentration is 1 M, thereby obtaining a perovskite precursor solution, and the precursor solution is used for subsequent spin coating.
[0057] The transparent conductive glass with strips of ITO (anode) etched on the surface was cleaned with detergent, deionized water, acetone and isopropanol ultrasonic oscillation for 15 minutes, dried with nitrogen flow, and then treated with ultraviolet ozone for 20 minutes; then a layer of NiO was spin-coated x The solution (spin coating parameters were 4000 rpm for 30 s) was annealed at 110 °C for 15 min; then it was transferred to a hot plate at 350 °C for 1 h, and then transferred to a nitrogen glove box environment without water or oxygen, and a 1.5 mg / mL PTAA toluene solution was spin coated on the NiO x The film was annealed at 100 °C for 10 min to obtain a hole transport layer.
[0058] During spin coating, 60 microliters of perovskite precursor solution was quickly dripped onto the hole transport layer, during which the temperature of the substrate was maintained at 60°C, the spin coating rate was set to 4000 rpm for 40 seconds, 70 microliters of ethyl acetate was added 30 seconds after the start of spin coating, and after the spin coating stopped, the film was placed on a hot stage at 100°C for 30 minutes, and after cooling, an organic ammonium salt solution (solvent is isopropanol, concentration is 2 mg / mL) was spin coated at a speed of 5000 rpm, and the film was placed on a hot stage at 100°C for annealing for 5 minutes. After cooling, PCBM (solvent is chlorobenzene, concentration is 20 mg / mL) and BCP (solvent is ethanol, concentration is 0.5 mg / mL) were spin coated at a speed of 3000 rpm, and finally, an Ag electrode with a thickness of 80-100 nm was evaporated on the BCP using an evaporator to obtain a Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 is a perovskite solar cell device with an active layer.
[0059] At a light intensity of 100 mW / cm 2 The current-voltage curve of the device was tested under AM1.5G simulated sunlight, and the open circuit voltage (V OC ) is 1.25V, and the short-circuit current density (Jsc) is 18.08mA / cm 2 , the fill factor (FF) is 81.36, and the photoelectric conversion efficiency (PCE) is 18.35%. Figure 3 Ref in is the current-voltage curve of the device.
[0060] Example 2
[0061] Using FAI, MABr, PbBr, PbI2 and CsI as raw materials, Cs 0.1 FA 0.7 MA 0.2 Pb(I 0.55 Br 0.45 )3 solution, the solvent is a mixed solvent of DMF and DMSO (3:2 / v:v), and the concentration is 1 M, thereby obtaining a perovskite precursor solution, and the precursor solution is used for subsequent spin coating.
[0062] The transparent conductive glass with strips of ITO (anode) etched on the surface was cleaned with detergent, deionized water, acetone and isopropanol ultrasonic oscillation for 15 minutes, dried with nitrogen flow, and then treated with ultraviolet ozone for 20 minutes; then a layer of NiO was spin-coated xThe solution (spin coating parameters were 4000 rpm for 30 s) was annealed at 110 °C for 15 min; then it was transferred to a hot plate at 350 °C for 1 h, and then transferred to a nitrogen glove box environment without water or oxygen, and a 1.5 mg / mL PTAA toluene solution was spin coated on the NiO x The film was annealed at 100 °C for 10 min to obtain a hole transport layer.
[0063] During spin coating, 60 microliters of perovskite precursor solution was quickly dripped on the hole transport layer, during which the temperature of the substrate was maintained at 60°C, the spin coating rate was set to 4000 rpm for 40 seconds, 70 microliters of ethyl acetate was added 30 seconds after the start of spin coating, and after the spin coating stopped, the film was placed on a hot stage at 100°C for annealing for 30 minutes, and after cooling, the EDA solution was spin-coated at a speed of 4000 rpm, and the film was placed on a hot stage at 70°C for annealing for 5 minutes. After cooling, the organic ammonium salt solution (solvent is isopropanol, concentration is 2 mg / mL) was spin-coated at a speed of 5000 rpm, and the film was placed on a hot stage at 100°C for annealing for 5 minutes. After cooling, PCBM (solvent is chlorobenzene, concentration is 20 mg / mL) and BCP (solvent is ethanol, concentration is 0.5 mg / mL) were spin-coated at a speed of 3000 rpm, and finally an Ag electrode with a thickness of 80-100 nm was evaporated on the BCP using an evaporator to obtain a Cs 0.05 (FA 0.95 MA 0.05 ) 0.95 Pb(I 0.95 Br 0.05 )3 is a perovskite solar cell device with an active layer.
[0064] At a light intensity of 100 mW / cm 2 The current-voltage curve of the device was tested under AM1.5G simulated sunlight, and the open circuit voltage (V OC ) is 1.25V, and the short-circuit current density (Jsc) is 18.34mA / cm 2 , the fill factor (FF) is 84.28, and the photoelectric conversion efficiency (PCE) is 19.41%. Figure 3 The Target in is the current-voltage curve of the device.
[0065] It can be seen that the present invention pre-introduces amine ligand molecules into the upper surface of three-dimensional perovskite to regulate the growth of the two-dimensional perovskite passivation layer, thereby forming a two-dimensional passivation layer with controllable dimension and thickness, thereby obtaining a two-dimensional and three-dimensional multi-level structure perovskite film with excellent photoelectric properties, which is used to realize high-performance perovskite solar cells. Based on mixed cation lead halide perovskite, an inverted solar cell device with an energy conversion efficiency of 24.72% is prepared.
[0066] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A method for preparing a perovskite film having a two-dimensional and three-dimensional multi-level structure, characterized in that: The details are as follows: Depositing a first solution containing amine ligands on the surface of a three-dimensional perovskite, and subjecting the solution to annealing to complete the pre-embedding of amine molecules on the surface of the three-dimensional perovskite to obtain a preliminary film; then depositing a second solution containing an organic ammonium salt on the preliminary film, and subjecting the solution to annealing to obtain a perovskite film having a two-dimensional and three-dimensional multi-level structure; The three-dimensional perovskite is an ABX3 type perovskite, wherein the A position is a mixture of one or more of cesium ions, methylamine cations, and formamidinium cations, the B position is a lead ion, and the X position is a mixture of one or more of chloride ions, bromide ions, and iodide ions; The solvent used in the first solution is a reagent that does not dissolve ABX3 type perovskite.
2. The method for preparing a perovskite film having a two-dimensional and three-dimensional multi-level structure according to claim 1, characterized in that: The amine ligand is one or more of ethylenediamine, propylenediamine, and butylenediamine, and the solvent of the first solution is at least one of toluene and chlorobenzene.
3. The method for preparing a perovskite film having a two-dimensional and three-dimensional multi-level structure according to claim 1, characterized in that: The organic ammonium salt is at least one of an aromatic ring and an alkyl chain ammonium salt, and the solvent of the second solution is at least one of isopropanol and chlorobenzene.
4. The method for preparing a perovskite film having a two-dimensional and three-dimensional multi-level structure according to claim 1, characterized in that: The annealing temperature used to prepare the preliminary film is 60-80°C.
5. The method for preparing a perovskite film having a two-dimensional or three-dimensional multi-level structure according to claim 1, characterized in that: The annealing temperature used to prepare the preliminary film is 70-80°C.
6. The method for preparing a perovskite film having a two-dimensional or three-dimensional multi-level structure according to claim 1, characterized in that: The annealing temperature used to prepare the two-dimensional and three-dimensional multi-level structure perovskite film is 100-120°C.
7. The method for preparing a perovskite film having a two-dimensional or three-dimensional multi-level structure according to claim 1, characterized in that: The annealing temperature used to prepare the two-dimensional and three-dimensional multi-level structure perovskite film is 100-110°C.
8. The method for preparing a perovskite film having a two-dimensional or three-dimensional multi-level structure according to claim 1, characterized in that: The concentration of the amine ligand in the first solution is 0.1-0.2 mM, and the concentration of the organic ammonium salt in the second solution is 1-4 mg / mL.
9. A perovskite film having a two-dimensional or three-dimensional multi-level structure obtained according to the preparation method of any one of claims 1 to 8.
10. A perovskite solar cell device with a two-dimensional and three-dimensional multi-level structure, characterized in that: The solar cell device is a multi-layered structure, which comprises a substrate (1), a transparent electrode layer (2), a hole transport layer (3), a photoactive layer (4), an electron transport layer (5), a work function adjustment layer (6) and a metal electrode layer (7) stacked in sequence from bottom to top; wherein the photoactive layer (4) is a perovskite film having a two-dimensional and three-dimensional multi-level structure as described in claim 9.
11. The perovskite solar cell device with a two-dimensional and three-dimensional multi-level structure according to claim 10, characterized in that: The substrate (1) is made of one of glass, quartz, flexible PET or flexible PEN; the transparent electrode layer (2) is made of indium tin oxide or fluorine-doped tin oxide; the hole transport layer (3) is made of one of nickel oxide, PTAA, PEDOT or Poly-TPD; the electron transport layer (5) is made of PCBM, C 60 or zinc dioxide; the work function adjustment layer (6) is made of BCP; the metal electrode layer (7) is made of silver, aluminum, magnesium, copper, gold, indium tin oxide or fluorine-doped tin oxide, and has a thickness of 50-300 nm.
Citation Information
Patent Citations
Perovskite film, perovskite electroluminescence device and preparation method and display device
CN110387227A
Method for improving photoelectric conversion rate of two-dimensional perovskite solar cell
CN110571336A
Preparation method and application of bifunctional ionic salt passivated tin-based perovskite thin film and perovskite solar cell of bifunctional ionic salt passivated tin-based perovskite thin film
CN114284440A
Compositions and methods for stabilizing perovskite interfaces
US20220037597A1