A hot working method for simultaneously improving the surface quality and tensile strength of titanium alloy rolled bars

By heating and deforming in the β single-phase area or α+β two-phase area and rolling multiple times in the β single-phase area, the problems of surface quality and tensile strength of titanium alloy rods are solved, and the quality of titanium alloy rods is realized. Increased high temperature tensile strength and improved surface quality.

CN115178597BActive Publication Date: 2024-10-18BAOWU TEYE TITANIUM TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210811071.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-10-18
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

In the traditional thermal processing process, the primary α phase size distribution of titanium alloy rods is uneven, resulting in low room temperature and high temperature tensile strength and large dispersion of the material, and the surface layer of high-temperature titanium alloy rods is prone to cracking during low-temperature rolling. , affecting the yield rate and testing results.

Method used

Heating and deformation is carried out in the β single-phase region or the α+β two-phase region to form a bar blank, and then rolling is performed at least twice in the β single-phase region. The rolling temperature is set to 10 to 30°C above the phase transformation point, and the holding time is Calculated based on 1 min/mm, the deformation amount is 70% to 90% to obtain titanium alloy rods with high surface quality and tensile strength.

Benefits of technology

The titanium alloy rods prepared by this method form uniform and fine equiaxed α phases near the grain boundaries. There are flaky α phases in the grains, which avoids the existence of large pieces of α and significantly improves the room temperature and 600°C high temperature of the material. The tensile strength reaches more than 100MPa of conventional two-phase zone rolled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115178597B_ABST
    Figure CN115178597B_ABST
Patent Text Reader

Abstract

The present invention provides a hot working method for improving the surface quality and tensile strength of titanium alloy rolled bars at the same time, wherein the bars obtained by blanking and intermediate blank forging are heated and deformed in a β single-phase region or an α+β two-phase region to form a bar blank; the bar blank is ground to remove surface defects and then heated in a β single-phase region, and the heating temperature is set to 10 to 30°C above the phase transition point. o C, the holding time is calculated as 1min / mm, and then at least two rollings are carried out, the total rolling deformation is 70%~90%, and air cooling is carried out after deformation to obtain bars with high surface quality and tensile strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the field of metallurgy and relates to a hot processing technology for titanium alloy bars, in particular to a hot processing method for simultaneously improving the surface quality and tensile strength of titanium alloy rolled bars. Background technology:

[0002] Titanium alloys are widely used in aerospace and other fields due to their high specific strength and excellent corrosion resistance. Among them, near-α alloys have good high-temperature strength and structural stability, and are used as high-temperature titanium alloys above 500°C.

[0003] The traditional hot working process for small-sized high-temperature titanium alloy bars is to prepare the intermediate billet by forging or rolling deformation in the α+β two-phase region, and then roll it into the finished product in the two-phase region (30-50°C below the phase transition point). However, a large number of practical results show that the size distribution of the primary α phase of the bars obtained by the traditional hot working process is uneven, and large pieces of α exist in local positions, resulting in low room temperature and high temperature tensile strength of the material and large dispersion. During the tensile process of the material, cracks are easy to initiate at the interface between the large piece of α and the matrix, resulting in the phenomenon that the high temperature tensile strength often does not meet the standard.

[0004] One method to improve the tensile strength of rolled bars is to perform low-temperature rolling in the two-phase region after deformation in the single-phase region, which can obtain materials with excellent room temperature and high temperature tensile strength. However, during the low-temperature rolling process, there is a risk of cracking on the surface of high-temperature titanium alloy bars, which has a great impact on subsequent testing and yield rate. Therefore, it is a technical problem that needs to be solved to simultaneously improve the surface quality and tensile strength of high-temperature titanium alloy rolled bars. Summary of the invention:

[0005] In view of the above-mentioned technical problems in the prior art, the present invention provides a hot working method for simultaneously improving the surface quality and tensile strength of titanium alloy rolled bars. The hot working method for simultaneously improving the surface quality and tensile strength of titanium alloy rolled bars is intended to solve the technical problem that during the low-temperature rolling process of titanium alloy rolled bars in the prior art, there is a risk of cracking on the surface of the high-temperature titanium alloy bar, which has a great impact on subsequent inspection and yield rate.

[0006] The present invention provides a hot working method for simultaneously improving the surface quality and tensile strength of a titanium alloy rolled bar, comprising the following steps:

[0007] 1) The rod obtained by blanking and intermediate blank forging is heated and deformed in the β single-phase region or the α+β two-phase region to form a rod blank; in the process of heating and deforming the β single-phase region to form a rod blank, the heating temperature of the β single-phase region is set to 30-50°C above the phase transformation point, the holding time is calculated as 1 min / mm, and then rolled or radial forged, the deformation amount is 50%-70%, and air-cooled after deformation; in the process of heating and deforming the α+β two-phase region to form a rod blank, the heating temperature is set to 30-50°C below the phase transformation point, the holding time is calculated as 1 min / mm, and then rolled or radial forged, the deformation amount is 50%-70%, and air-cooled after deformation;

[0008] 2) The rod blank obtained in step 1) is ground to remove surface defects and then heated in the β single-phase region, the heating temperature is set to 10-30° C. above the phase transformation point, the holding time is calculated as 1 min / mm, and then rolled at least twice, the total rolling deformation is 70%-90%, and a rod with high surface quality and tensile strength can be obtained.

[0009] The high-temperature titanium alloy rolled rod prepared by the method of the present invention has high surface quality, and the α phase in the rolled state exists in a uniform, fine, equiaxed shape near the grain boundary, with a size of 1-3um. The intracrystalline α phase exists in a sheet shape with a thickness of about 1um, and there is no large block of α in the crystal. After double annealing heat treatment, the room temperature and 600°C high-temperature tensile strength of the material with this structure is increased by more than 100MPa compared with the conventional two-phase zone rolled material.

[0010] The preparation process of titanium alloy bars is generally: ingot smelting, blanking, intermediate billet forging, radial forging / rolling, final rolling, and heat treatment. The present invention mainly focuses on the final rolling process of titanium alloy bars.

[0011] The principle of the present invention is as follows:

[0012] The strength of titanium alloys with dual-state structure is related to the effective slip distance of dislocations, and the strength of titanium alloys with equiaxed structure is related to the size of α phase. The primary α phase spacing is small, the effective slip distance of dislocations is short, and the strength of the material is high. The size of the equiaxed α phase is small, the interface effect is obvious, and the strength of the material is high. For small-sized bars of high-temperature titanium alloys, although higher material strength can be obtained through low-temperature rolling in the two-phase region, cracks are easily generated on the surface of the material when the rolling temperature is low. Although the surface quality is high when rolling in the entire β single-phase region, the obtained structure is Widmanstatten structure, the material plasticity is low, and it cannot meet the use requirements. The "cross-phase rolling" process proposed in the present invention utilizes the coupling effect between temperature-structure-deformation, performs a certain deformation in the β region, and accumulates strain energy at the grain boundary; with the temperature drop after leaving the furnace and the temperature drop during the deformation process, the material enters the α+β two-phase region, and the α phase is preferentially precipitated at and near the β grain boundary containing a large amount of distortion energy, and is broken and spheroidized during the deformation process, and at the same time, a distorted lamellar α phase is formed in the crystal. The spheroidized α phase at the grain boundary is uniform and fine, which improves the strength of the material. At the same time, the spheroidal structure coordinates the deformation aggregation under the action of external force to a certain extent, avoiding the deficiency of lamellar Widmanstatten structure. Research and practice show that when the heating temperature of the β single-phase region is selected to be 10-30℃ above the phase transformation point, the holding time is calculated as 1min / mm, and the deformation amount is 70%-90%, the spheroidized α and intracrystalline lamellar structure existing within a certain width range of the grain boundary can be obtained. If the heating temperature of the β single-phase region is too high, the β grains will grow seriously, and the deformation amount distribution of the two-phase region will be insufficient, and the α phase that precipitates preferentially at the grain boundary cannot be effectively crushed; if the heating temperature is too low, it is easy to cause insufficient deformation above the phase transformation point, the strain energy stored in the β grain boundary is limited, and the width of the formed grain boundary α is limited, which affects the range of crushing the spheroidized α phase.

[0013] Compared with the existing technology, the technical progress of the present invention is significant. The "cross-phase rolling" process technology proposed in the present invention has a higher heating temperature than conventional two-phase rolling, a smaller material deformation resistance, easier forming, and a higher yield rate; the α phase in the prepared high-temperature titanium alloy rolled rod is present in a uniform, fine, equiaxed shape near the grain boundary with a size of 1-3um. The intracrystalline α phase exists in the form of flakes with a thickness of about 1um, and there are no large pieces of α in the crystal. After double annealing heat treatment, the grain boundaries and intracrystalline α grow slightly. The room temperature and 600°C high-temperature tensile strength of the material with this organization is more than 100MPa higher than that of conventional two-phase rolled materials. Description of the drawings:

[0014] Figure 1 This is a schematic diagram of the “cross-phase rolling” process route proposed in the present invention.

[0015] Figure 2 This is the microstructure morphology obtained by using the traditional two-phase zone rolling process in the comparative example.

[0016] Figure 3This is the microstructure morphology obtained by using the preparation process proposed by the present invention in Example 1.

[0017] Figure 4 This is the microstructure morphology obtained by using the preparation process proposed by the present invention in Example 2. Specific implementation method:

[0018] The high temperature titanium alloy in the comparative example and the embodiment is Ti-Al-Sn-Zr-Mo-Nb system, containing a small amount of Si and Ce. For other near-α high temperature titanium alloys, the preparation process proposed in the present invention can also achieve the same effect.

[0019] Comparative Example:

[0020] The φ760mm ingot is obtained by three vacuum consumable melting, and the phase transition point is 1020℃. The ingot is opened into φ220mm by a fast forging machine, and the forging temperature is 1050~1150℃; then it is forged into φ80mm bar, and the forging temperature is 950~970℃. After grinding, the bar is loaded into the electric furnace, the temperature is 990℃, and it is kept warm for 80 minutes, and then it is radially forged into a billet with a deformation of 60%. After grinding to remove surface defects, the billet is loaded into the electric furnace, the temperature is 980℃, and it is kept warm for 40 minutes, and rolled into a bar with a deformation of 75%. The rolled bar is double annealed, specifically 960℃ / 1h, air cooling + 570℃ / 2h, air cooling.

[0021] Figure 2 This is the microstructural morphology obtained by the traditional two-phase rolling process in the comparative example. It can be seen that the size distribution of the primary α phase in the rolled rod is uneven, with coarse sizes of 8-15um and fine sizes of 2-10um. There are also some large pieces of α that are left over and not fully broken. During the subsequent double annealing heat treatment, the fine α dissolves and disappears, but the large pieces of α still exist. Table 1 gives the room temperature and 600°C high-temperature tensile properties of the rolled rod. Due to the uneven size distribution of the α phase after rolling and the presence of large pieces of α, the high-temperature performance of the rolled rod fluctuates significantly, and most of the values ​​do not meet the relevant material specifications (yield strength requirements ≥550MPa, tensile strength requirements ≥650MPa).

[0022] Embodiment 1:

[0023] The φ80mm bar after blanking and forging in the comparative example was used. After grinding, the bar was loaded into an electric furnace at a temperature of 970℃, kept warm for 80 minutes, and then forged into a blank with a deformation of 60%. After grinding to remove surface defects, the blank was loaded into an electric furnace at a temperature of 1030℃, kept warm for 40 minutes, and rolled into a bar with a deformation of 85%, and air-cooled after rolling. The obtained bar has good surface quality and no obvious cracks.

[0024] Figure 3The microstructure morphology of the rolled rod obtained in Example 1. The α phase in the rolled rod exists in a uniform, fine, equiaxed shape near the grain boundary, with a size of 1-3um. The intracrystalline α phase exists in a twisted sheet with a thickness of about 1um, and there is no large piece of α in the crystal. After double annealing heat treatment, the α at the grain boundary and within the crystal grows slightly, with sizes of 5-8um and 2-4um, respectively. The room temperature and 600°C high temperature tensile strength of the material are shown in Table 1, both of which are significantly improved compared to the comparative example.

[0025] Embodiment 2:

[0026] The φ80mm bar after blanking and forging in the comparative example was used. After grinding, the bar was loaded into an electric furnace at a temperature of 1070℃, kept warm for 80 minutes, and then rolled into a blank with a deformation of 60%. After grinding to remove surface defects, the rolled blank was loaded into an electric furnace at a temperature of 1050℃, kept warm for 40 minutes, and rolled into a bar with a deformation of 70%, and air-cooled after rolling. The obtained bar has good surface quality and no obvious cracks.

[0027] Figure 4 The microstructure morphology of the rolled rod obtained in Example 2 is similar to that of Example 1. Compared with the comparative example, the room temperature and 600°C high temperature tensile strength of the material are significantly improved. Compared with Example 1, since the billet is obtained by deformation in the single-phase region before final rolling, the original β grains are large. These β grains continue to grow during the final rolling heating process, resulting in a small number of grain boundary α grains participating in spheroidization and large spacing, so the material strength is slightly reduced. The data is shown in Table 1.

[0028] Table 1 Mechanical properties of examples and comparative examples

[0029]

[0030]

[0031] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.

Claims

1. A hot working method for simultaneously improving the surface quality and tensile strength of titanium alloy rolled bars, characterized in that The steps include: 1) The bars obtained by forging the blank and the intermediate blank are heated and deformed in the β single-phase region or the α+β two-phase region to form a bar blank; in the process of heating and deforming the β single-phase region to form a bar blank, the heating temperature of the β single-phase region is set to 30~50 ℃ above the phase transformation point, the holding time is calculated as 1min / mm, and then rolled or radial forged, the deformation amount is 50%~70%, and air cooled after deformation; in the process of heating and deforming the α+β two-phase region to form a bar blank, the heating temperature is set to 30~50 ℃ below the phase transformation point, the holding time is calculated as 1min / mm, and then rolled or radial forged, the deformation amount is 50%~70%, and air cooled after deformation; 2) The bar blank obtained in step 1) is ground to remove surface defects and then heated in the β single phase region. The heating temperature is set to 10~30°C above the phase transformation point. The holding time is calculated as 1min / mm. Then, at least two rollings are performed. The total rolling deformation is 70%~90%. A bar with high surface quality and tensile strength can be obtained.

Citation Information

Patent Citations