A single crystal nickel cobalt lithium manganese oxide positive electrode material

By using the core-shell structure of the lithium cobalt manganate positive electrode material in lithium ion batteries, and using the composite shell material of Lir(NisCotMn1-s-t)O2, metal oxides and metal metaphosphate, the lithium ion battery is solved at high voltage The problem of insufficient downcycling performance and thermal stability achieves higher battery stability and cycle life.

CN115188940BActive Publication Date: 2024-11-01JIANGSU XIANGYING NEW ENERGY TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210728850.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-30
Publication Date
2024-11-01
Estimated Expiration
2041-07-30

AI Technical Summary

Technical Problem

The existing lithium-ion batteries have poor cycling performance and thermal stability at high voltages, and the traditional secondary spherical particle structure is insufficient, resulting in an intensified electrode/solution interface reaction, affecting battery performance.

Method used

The core-shell structure of the nickel-cobalt-manganate lithium positive electrode material is adopted. The shell material consists of Lir(NisCotMn1-s-t)O2, metal oxides and metal metaphosphate. The composite material is formed through the sintering process to improve the cladding material and ternary material. compatibility and stability.

Benefits of technology

At a high voltage of 4.5V, the cycle stability and thermal stability of lithium-ion batteries are significantly improved, the side reactions of the electrolyte/material interface are suppressed, and the cycle life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115188940B_ABST
    Figure CN115188940B_ABST
Patent Text Reader

Abstract

The present invention discloses a single crystal nickel cobalt manganese oxide positive electrode material. The positive electrode material is a core-shell structure. The material of the core layer is a high-nickel nickel cobalt manganese ternary single crystal positive electrode material. The material of the shell layer includes Li r (Ni s Co t Mn 1‑s‑t )O2 (Ⅱ), metal oxides and metal metaphosphates, wherein 0.9≤r≤1.05, 0.3≤s≤0.5, 0 <t<0.4,1‑s‑t> 0; in terms of mass percentage, the material of the shell layer comprises more than 50% of the compound of formula (II), and the mass ratio of the metal oxide to the metal metaphosphate is 1:0.1-10; the positive electrode material can be suitable for working under a high voltage of 4.5V and has an ideal cycle stability performance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention is a divisional application of a Chinese invention patent application with an application date of July 30, 2021, application number 2021108693605, and name “A single crystal nickel cobalt lithium manganese oxide positive electrode material, its preparation method and application”. Technical Field

[0002] The present invention belongs to the field of lithium ion battery electrode materials, and in particular relates to a positive electrode material, and specifically relates to a single crystal nickel cobalt lithium manganese oxide positive electrode material. Background Art

[0003] Nowadays, with the increasing requirements for lithium-ion battery capacity in pure electric vehicles, hybrid vehicles and portable energy storage devices, people are looking forward to developing lithium-ion batteries with higher energy density and power density to achieve long-term endurance and energy storage. Increasing the battery operating voltage is one of the effective methods to improve the energy density of lithium-ion batteries. However, increasing the operating voltage will cause a series of problems such as the attenuation of the cycle performance of lithium-ion batteries, such as increasing the side reactions at the electrode / electrolyte interface, increasing the precipitation of oxygen, increasing the polarization and internal resistance of the battery, and causing the problem of poor cycle life. In order to improve the thermal stability and cycle performance of ternary materials at high voltage, common methods include coating and modifying the ternary positive electrode materials. However, although the current ternary materials have been coated and modified, they still cannot be well coated on the surface of the positive electrode material, and cannot effectively reduce the reaction of the electrolyte / material interface at high voltage. The cycle stability is poor and it is difficult to meet the actual needs. At the same time, the traditional secondary spherical particle structure has poor firmness. At a higher voltage, its skeleton structure is easily destroyed, resulting in an intensification of the electrode / solution interface reaction, resulting in a decrease in battery performance. Summary of the invention

[0004] The problem to be solved by the present invention is to overcome one or more deficiencies of the prior art and to provide an improved single crystal lithium nickel cobalt manganese oxide positive electrode material which can be suitable for working under a high voltage of 4.5V and has an ideal cycle stability performance.

[0005] A technical solution adopted by the present invention to solve its technical problem is: a single crystal nickel cobalt manganese lithium positive electrode material, the positive electrode material is a core-shell structure, the core-shell structure includes a core layer and a shell layer coated on the core layer, the material of the core layer is a nickel cobalt manganese ternary single crystal positive electrode material, wherein:

[0006] The nickel-cobalt-manganese ternary single crystal positive electrode material has the following structure: Li x (Ni a Co b Mn 1-a-b ) 2 (I), where 1.0≤x≤1.15, 0.5 <a≤0.9,0.05≤b≤0.35,1-a-b>0;

[0007] The material of the shell layer includes Li r (Ni s Co t Mn 1-s-t ) 2 (II), metal oxides and metal metaphosphates, wherein 0.9≤r≤1.05, 0.3≤s≤0.5, 0 <t<0.4,1-s-t> 0; wherein, in terms of mass percentage, in the material of the shell layer, the Li r (Ni s Co t Mn 1-s-t ) 2 The metal oxide accounts for more than 50%, and the mass ratio of the metal oxide to the metal metaphosphate is 1:0.1-10.

[0008] According to some preferred aspects of the present invention, the total amount of the metal oxide and the metal metaphosphate is equal to the amount of the Li r (Ni s Co t Mn 1-s-t ) 2 The mass ratio of the feed materials is 1:1-5.

[0009] According to some preferred and specific aspects of the present invention, the metal elements in the metal oxide and the metal metaphosphate are respectively selected from one or more of Al, Ti, Mg, Y, Zr, Nb, and W.

[0010] According to some preferred aspects of the present invention, the metal oxide is consistent with the metal element in the metal metaphosphate, which is beneficial to control the type of metal elements introduced into the ternary material on the one hand, and improves the compatibility of the coating material and the ternary material body on the other hand, thereby improving the cycle performance and thermal stability to a certain extent.

[0011] According to some preferred aspects of the present invention, the particle size of the metal oxide is 100-800 nm.

[0012] According to some preferred and specific aspects of the present invention, the method for preparing the shell material comprises: mixing and dispersing the precursor of formula (II) with metal oxide and metal metaphosphate, grinding, then mixing with a lithium source, and sintering in an atmosphere containing oxygen.

[0013] According to some preferred aspects of the present invention, the mass ratio of the core layer to the shell layer is 50-200:1.

[0014] According to some preferred aspects of the present invention, the particle size of the nickel-cobalt-manganese ternary single crystal positive electrode material is 2-6 μm.

[0015] According to some preferred aspects of the present invention, the shell layer has a thickness of 1-8 μm.

[0016] Another technical solution provided by the present invention is a method for preparing the above-mentioned single crystal nickel cobalt lithium manganese oxide positive electrode material, the preparation method comprising the following steps:

[0017] (1) mixing a metal oxide and a metal metaphosphate, adding the mixture to water, dispersing and stirring to form a slurry, mixing the obtained slurry with a precursor of formula (II), grinding, and then spray drying, airflow milling the dried mixture to obtain a composite material, mixing the obtained composite material with a lithium source, sintering the mixture in an atmosphere furnace, and then crushing, pulverizing, and sieving the sintered material to obtain a shell material;

[0018] (2) mixing the precursor of formula (I) with a lithium source, sintering the mixture in an atmosphere furnace, and then crushing, pulverizing, and sieving the sintered material to obtain a core layer material having a structure represented by formula (I);

[0019] (3) The shell layer material obtained in step (1) is used as a coating material, mixed and dispersed with the core layer material obtained in step (2), and then sintered in an atmosphere furnace. The sintered material is then crushed, pulverized, and sieved to obtain the single crystal nickel cobalt manganese oxide positive electrode material.

[0020] According to some specific and preferred aspects of the present invention, in step (1), the proportion of solids in the slurry is 30% to 50%.

[0021] According to some specific and preferred aspects of the present invention, in step (1), the molar ratio of lithium in the lithium source to the sum of nickel, cobalt and manganese in the precursor of formula (II) is 1.00-1.15:1.

[0022] According to some specific aspects of the present invention, in step (1), the water is ultrapure water, that is, water with a resistivity of 18 MΩ*cm (25° C.).

[0023] According to some specific and preferred aspects of the present invention, in step (2), the molar ratio of lithium in the lithium source to the sum of nickel, cobalt and manganese in the precursor of formula (I) is 1.00-1.15:1.

[0024] According to some specific and preferred aspects of the present invention, in step (1) or (2), the sintering temperature is 200-1000° C., the sintering time is 2-15 hours, and the sintering atmosphere in the atmosphere furnace is a gas containing oxygen with an oxygen content of 90% to 100%.

[0025] Furthermore, in step (1), the sintering temperature is 200-1000°C, and the sintering time is 5-15 hours. Furthermore, the sintering temperature is 400-1000°C, and the sintering time is 8-12 hours.

[0026] Furthermore, in step (2), the sintering temperature is 200-1000°C, and the sintering time is 5-15 hours. Furthermore, the sintering temperature is 400-1000°C, and the sintering time is 8-12 hours.

[0027] Furthermore, in step (3), the sintering temperature is 200-900°C, and the sintering time is 2-12 hours. Furthermore, the sintering temperature is 400-800°C, and the sintering time is 8-10 hours.

[0028] Another technical solution provided by the present invention is an application of the above-mentioned single crystal nickel cobalt lithium manganese oxide positive electrode material in a high voltage battery with a voltage of 4.5V.

[0029] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0030] In the present invention, the innovative use of Li r (Ni s Co t Mn 1-s-t ) 2 (II) A composite material of metal oxide and metal metaphosphate is used as the shell material. The use of metal oxide can facilitate the effective dispersion of metal metaphosphate. Moreover, since metal oxide is easy to obtain nano-sized particles, it can act as a spacer layer to play a steric hindrance effect and disperse the metal metaphosphate as much as possible. At the same time, the metal oxide can consume the hydrofluoric acid produced by the side reaction under high voltage in the electrolyte to reduce corrosion. The metal metaphosphate system can form a three-dimensional network structure due to the combination of metaphosphate and metal ions. The formed coating layer can hinder the passage of oxygen atoms, thereby effectively inhibiting the structural collapse of the ternary positive electrode material caused by the release of oxygen under relatively high voltage. Then, when the voltage continues to increase, for example, to 4.5V, the stability of the system of metal metaphosphate combined with metal oxide deteriorates. At this time, a certain content of Li r (Ni s Co t Mn 1-s-t ) 2The material will play a stabilizing role, which can enable the metal metaphosphate and the metal oxide to maintain good contact with the core layer, play a role in assisting in stabilizing the relative position relationship between the metal metaphosphate / metal oxide and the core layer, improving the stability of the overall shell layer, and ensuring sufficient capacity of the system, so that the single crystal nickel cobalt manganese oxide positive electrode material of the present invention can be used in high-voltage batteries with a voltage of up to 4.5V, and achieve ideal cycle stability performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The XRD pattern of the single crystal nickel cobalt lithium manganese oxide positive electrode material obtained in Example 1;

[0032] Figure 2 This is the SEM spectrum of the single crystal nickel cobalt lithium manganese oxide positive electrode material obtained in Example 1;

[0033] Figure 3 This is a test chart of button-type batteries of Examples 1-3 and Comparative Example 5 at 4.5V, 60°C, and 1C cycle;

[0034] Figure 4 This is a test chart of the button cell 4.5V of comparative example 1-4 at 60°C and 1C cycle. DETAILED DESCRIPTION

[0035] The above scheme is further described below in conjunction with specific examples; it should be understood that these examples are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following examples; the implementation conditions used in the examples can be further adjusted according to specific requirements, and the unspecified implementation conditions are usually the conditions in conventional experiments. Unless otherwise specified in the following examples, all raw materials are purchased from commercial sources or prepared by conventional methods in the art.

[0036] Embodiment 1:

[0037] This example provides a method for preparing a single-crystal nickel cobalt lithium manganese oxide positive electrode material and the prepared single-crystal nickel cobalt lithium manganese oxide positive electrode material.

[0038] The preparation method comprises: (1) adding a solid mixture of aluminum oxide and aluminum metaphosphate in a mass ratio of 1:2 into ultrapure water to form slurry A, so that the solid matter accounts for 30% of the slurry, and stirring the slurry at a speed of 600 rpm for 2 hours. Then, the obtained slurry A is mixed with single crystal Ni 0.5 Co 0.2 Mn 0.3 (OH) 2The precursor was added into the grinder at a mass ratio of 5:6, and the dispersed slurry was ground in a sand mill at a speed of 3000 rpm using a grinding ball with a particle size of 0.1 mm. The slurry was stirred with a dispersion disk at a speed of 600 rpm for 2 hours. The dispersed slurry was extracted into a spray dryer and spray-dried at a speed of 300 rpm. The spray-dried material was subjected to airflow pulverization at a pulverization frequency of 50 Hz to obtain composite material B.

[0039] (2) The lithium source and the composite material B were weighed according to the molar ratio of Li:(Ni+Co+Mn)=1.05:1, added into a high-speed mixer at 600 r / min and mixed for about 45 min, and then placed in an atmosphere furnace for sintering at a sintering temperature of 960±10°C and a sintering time of 12 h in an oxygen atmosphere. After sintering, the material was crushed, pulverized and sieved to obtain a shell material C.

[0040] (3) Preparation of core layer: Li source and ternary single crystal material precursor Ni were weighed according to the molar ratio of Li: ternary material precursor = 1.05:1. 0.6 Co 0.2 Mn 0.2 (OH) 2 The above materials were mixed in a high-speed mixer at 600 r / min for 45 minutes, and then put into an atmosphere furnace. The sintering temperature was 940±10°C, the sintering time was 12 hours, and the sintering atmosphere was an oxygen atmosphere to obtain the core layer material D.

[0041] (4) The shell material C is used as a coating layer and is added to the core layer material D at a mass ratio of 1:100 in a high-speed mixer at 600 r / min and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to obtain a single crystal nickel cobalt manganese oxide positive electrode material.

[0042] Embodiment 2:

[0043] This example provides a method for preparing a single-crystal nickel cobalt lithium manganese oxide positive electrode material and the prepared single-crystal nickel cobalt lithium manganese oxide positive electrode material.

[0044] The preparation method comprises: (1) obtaining a composite material B in the same manner as step (1) of Example 1.

[0045] (2) The method is the same as step (2) of Example 1 to obtain shell material C.

[0046] (3) Preparation of core layer: Li source and ternary single crystal material precursor Ni were weighed according to the molar ratio of Li: ternary material precursor = 1.05:1. 0.7 Co 0.1 Mn0.2 (OH) 2 After mixing the above materials in a high-speed mixer at 600 r / min for 45 minutes, the materials were put into an atmosphere furnace at a sintering temperature of 930±10°C, a sintering time of 12 hours, and an oxygen atmosphere to obtain core layer material E.

[0047] (4) The shell material C is used as a coating layer and is added to the core layer material E at a mass ratio of 1:100 in a high-speed mixer at 600 r / min and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to obtain a single crystal nickel cobalt manganese oxide positive electrode material.

[0048] Embodiment 3:

[0049] This example provides a method for preparing a single-crystal nickel cobalt lithium manganese oxide positive electrode material and the prepared single-crystal nickel cobalt lithium manganese oxide positive electrode material.

[0050] The preparation method comprises: (1) obtaining a composite material B in the same manner as step (1) of Example 1.

[0051] (2) The method is the same as step (2) of Example 1 to obtain shell material C.

[0052] (3) Preparation of core layer: Li source and ternary single crystal material precursor Ni were weighed according to the molar ratio of Li: ternary material precursor = 1.05:1. 0.83 Co 0.11 Mn 0.06 (OH) 2 After mixing the above materials in a high-speed mixer at 600 r / min for 45 minutes, the materials were put into an atmosphere furnace at a sintering temperature of 890±10°C, a sintering time of 12 hours, and an oxygen atmosphere to obtain a core layer material F.

[0053] (4) The shell material C is used as a coating layer and is added to the core layer material F at a mass ratio of 1:100 in a high-speed mixer at 600 r / min and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to obtain a single crystal nickel cobalt manganese oxide positive electrode material.

[0054] Comparative Example 1:

[0055] (1) Weigh the lithium source and single crystal Ni according to the molar ratio of Li: ternary material precursor = 1.05:1 0.5 Co 0.2 Mn 0.3 (OH) 2After mixing the above materials in a high-speed mixer at 600 r / min for 45 minutes, the materials are put into an atmosphere furnace at a sintering temperature of 960±10°C, a sintering time of 12 hours, and an oxygen atmosphere to obtain a shell material.

[0056] (2) The shell material prepared in step (1) is used as a coating agent. It is added to a high-speed mixer at 600 r / min with the core material D in Example 1 at a mass ratio of 1:100 and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the material is crushed, pulverized and sieved to obtain a coated material having single crystal NCM523 as the shell layer and single crystal NCM622 as the core layer.

[0057] Comparative Example 2:

[0058] (1) Add slurry A in Example 1 into a grinder, use grinding balls with a particle size of 0.1 mm, and grind the dispersed slurry in a sand mill at a speed of 3000 rpm. Use a dispersion disk to stir the slurry at a speed of 600 rpm for 2 hours. Draw the dispersed slurry into a spray dryer and spray dry it at a speed of 300 rpm. The spray-dried material is subjected to airflow pulverization at a pulverization frequency of 50 Hz to obtain a shell material.

[0059] (2) The shell material prepared in step (1) is used as a coating agent. It is added to a high-speed mixer at 600 r / min with the core material D in Example 1 at a mass ratio of 1:100 and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to obtain a coated material having an alumina-aluminum metaphosphate composite material as the shell layer and single crystal NCM622 as the core layer.

[0060] Comparative Example 3:

[0061] (1) Weigh the lithium source and single crystal Ni according to the molar ratio of Li: ternary material precursor = 1.05:1 0.5 Co 0.2 Mn 0.3 (OH) 2 After mixing the above materials in a high-speed mixer at 600 r / min for 45 minutes, the materials are put into an atmosphere furnace at a sintering temperature of 960±10°C, a sintering time of 12 hours, and an oxygen atmosphere to obtain a shell material.

[0062] (2) The shell material prepared in step (1) is used as a coating agent. It is added to a high-speed mixer at 600 r / min with the core material E in Example 2 at a mass ratio of 1:100 and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the material is crushed, pulverized and sieved to obtain a coated material having single crystal NCM523 as the shell layer and single crystal NCM712 as the core layer.

[0063] Comparative Example 4:

[0064] (1) Add slurry A in Example 1 into a grinder, use grinding balls with a particle size of 0.1 mm, and grind the dispersed slurry in a sand mill at a speed of 3000 rpm. Use a dispersion disk to stir the slurry at a speed of 600 rpm for 2 hours. Draw the dispersed slurry into a spray dryer and spray dry it at a speed of 300 rpm. The spray-dried material is subjected to airflow pulverization at a pulverization frequency of 50 Hz to obtain a shell material.

[0065] (2) The shell material prepared in step (1) is used as a coating agent. It is added to a high-speed mixer at 600 r / min with the core material E in Example 2 at a mass ratio of 1:100 and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to obtain a coated material having an alumina-aluminum metaphosphate composite material as the shell layer and single crystal NCM712 as the core layer.

[0066] Comparative Example 5:

[0067] The method is basically the same as Example 1, except that, in terms of mass percentage, the single crystal NCM523 accounts for 40% of the shell material. (1) A solid mixture of aluminum oxide and aluminum metaphosphate is added to ultrapure water in a mass ratio of 1:2 to form slurry A, so that the solid matter accounts for 30% of the slurry. The slurry is stirred at 600 rpm for 2 hours. Then, the obtained slurry A is mixed with single crystal Ni 0.5 Co 0.2 Mn 0.3 (OH) 2 The precursor was added into the grinder at a mass ratio of 4:3, and the dispersed slurry was ground in a sand mill at a speed of 3000 rpm using grinding balls with a particle size of 0.1 mm. The slurry was stirred with a dispersion disk at a speed of 600 rpm for 2 hours. The dispersed slurry was extracted into a spray dryer and spray-dried at a speed of 300 rpm. The spray-dried material was subjected to airflow pulverization at a pulverization frequency of 50 Hz to obtain composite material E.

[0068] (2) The lithium source and the composite material E were weighed according to the molar ratio of Li:(Ni+Co+Mn)=1.05:1, added into a high-speed mixer at 600 r / min and mixed for about 45 min, and then placed in an atmosphere furnace for sintering at a sintering temperature of 960±10°C and a sintering time of 12 h in an oxygen atmosphere. After sintering, the shell material F was obtained by jaw crushing, pulverizing and sieving.

[0069] (3) Preparation of core layer: Li source and ternary single crystal material precursor Ni were weighed according to the molar ratio of Li: ternary material precursor = 1.05:1. 0.6 Co 0.2 Mn 0.2 (OH) 2 After mixing the above materials in a high-speed mixer at 600 r / min for 45 minutes, the materials were put into an atmosphere furnace at a sintering temperature of 940±10°C, a sintering time of 12 hours, and an oxygen atmosphere to obtain a core layer material G.

[0070] (4) The shell material F is used as a coating layer and is added to the core layer material G at a mass ratio of 1:100 in a high-speed mixer at 600 r / min and mixed for 45 minutes. The mixture is then placed in an atmosphere furnace for sintering at a sintering temperature of 590±10°C and a sintering time of 6 hours in an oxygen atmosphere. After sintering, the mixture is crushed, pulverized and sieved to finally obtain a single crystal nickel cobalt manganese oxide positive electrode material.

[0071] Performance Testing

[0072] The XRD spectrum of the single crystal nickel cobalt manganese oxide positive electrode material obtained in Example 1 is as follows Figure 1 As shown, it was observed that there was no impurity peak in the sample, and the grain orientation was normal, with a good crystal structure.

[0073] The SEM spectrum of the single crystal nickel cobalt manganese oxide positive electrode material obtained in Example 1 is as follows Figure 2 As shown in the figure, the surface of the positive electrode material is obviously coated with particles, indicating that the shell material can be well attached to the surface of the core layer.

[0074] The materials prepared in the above examples were used as positive electrode materials and lithium sheets were used as negative electrodes to make and assemble 2016 button batteries. The charge and discharge voltage range was 3.0 to 4.5 V, the temperature was 60°C, and the test was carried out at a 1C discharge rate. The measured data are shown in Table 1-2 below.

[0075] Table 1

[0076]

[0077] Table 2

[0078]

[0079] It can be seen from Table 1 and Table 2 that the cycle capacity of Examples 1, 2, and 3 is significantly improved compared to Comparative Examples 1-4, indicating that the cycle performance of the positive electrode material coated with the shell material of the present invention is significantly improved. At the same time, although Comparative Example 5 is improved compared to Comparative Examples 1-4, the effect is still not good. At the same time, the cycle performance of the composite material coated with only aluminum oxide-aluminum metaphosphate (Comparative Example 2, Comparative Example 4) is improved after a period of circulation compared to the material coated with only NCM523 single crystal. This may be because at the beginning of the cycle, the material coated with only NCM523 single crystal can play a certain role in stabilizing the entire core-shell structure, but as the cycle proceeds, the interface side reactions intensify and the cycle performance begins to deteriorate. For the material coated with only oxide-metaphosphate, the oxide-metaphosphate system plays a role after a period of circulation and effectively suppresses the side reactions of the interface. However, with the continuous operation of 4.5V high voltage, the stability of the oxide-metaphosphate system begins to deteriorate, and the contact performance with the core layer decreases significantly, which leads to a decrease in cycle performance. The present invention adopts Li r (Ni s Co t Mn 1-s-t ) 2 (II) After the composite material of metal oxide and metal metaphosphate is coated as the shell material, it can not only effectively stabilize the structure of the material, inhibit the interfacial side reaction under high voltage and the structural collapse of the ternary positive electrode material caused by the escape of oxygen, but also the stability of the metal metaphosphate and metal oxide under a high voltage of 4.5V is significantly improved, thereby improving the stability of the positive electrode material as a whole, so that the positive electrode material can exert a higher cycle stability performance under a high voltage of 4.5V.

[0080] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

[0081] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A single crystal nickel cobalt manganese lithium positive electrode material, the positive electrode material is a core-shell structure, the core-shell structure includes a core layer and a shell layer coated on the core layer, the material of the core layer is a nickel cobalt manganese ternary single crystal positive electrode material, Features: The nickel-cobalt-manganese ternary single crystal positive electrode material has the following structure: Li x (Ni a Co b Mn 1-a-b ) 2 (I), where 1.0≤x≤1.15, 0.5 <a≤0.9,0.05≤b≤0.35,1-a-b>0; The material of the shell layer includes Li r (Ni s Co t Mn 1-s-t ) 2 (II), metal oxides and metal metaphosphates, wherein 0.9≤r≤1.05, 0.3≤s≤0.5, 0 <t<0.4,1-s-t> 0; wherein, in terms of mass percentage, in the material of the shell layer, the Li r (Ni s Co t Mn 1-s-t ) 2 The metal oxide accounts for more than 50%, and the mass ratio of the metal oxide to the metal metaphosphate is 1:0.1-10; The single crystal nickel cobalt lithium manganese oxide positive electrode material is prepared by the following method: (1) mixing a metal oxide and a metal metaphosphate, adding the mixture to water, dispersing and stirring to form a slurry, mixing the obtained slurry with a precursor of formula (II), grinding, and then spray drying, airflow milling the dried mixture to obtain a composite material, mixing the obtained composite material with a lithium source, sintering the mixture in an atmosphere furnace, and then crushing, pulverizing, and sieving the sintered material to obtain a shell material; (2) mixing the precursor of formula (I) with a lithium source, sintering the mixture in an atmosphere furnace, and then crushing, pulverizing, and sieving the sintered material to obtain a core layer material having a structure represented by formula (I); (3) The shell layer material obtained in step (1) is used as a coating material, mixed and dispersed with the core layer material obtained in step (2), and then sintered in an atmosphere furnace, and the sintered material is crushed, pulverized, and sieved to obtain the single crystal nickel cobalt lithium manganese oxide positive electrode material; the sintering temperature is 200-900° C., and the sintering time is 2-12 h.

2. The single crystal lithium nickel cobalt manganese oxide positive electrode material according to claim 1, It is characterized in that The total amount of the metal oxide and the metal metaphosphate is equal to the amount of Li r (Ni s Co t Mn 1-s-t ) 2 The mass ratio of the feed materials is 1:1-5, the mass ratio of the core layer to the shell layer is 50-200:1, and the thickness of the shell layer is 1-8 μm.

3. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 1, It is characterized in that The metal elements in the metal oxide and the metal metaphosphate are respectively selected from one or more of Al, Ti, Mg, Y, Zr, Nb, and W.

4. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 3, It is characterized in that The metal oxide is consistent with the metal element in the metal metaphosphate.

5. The single crystal lithium nickel cobalt manganese oxide positive electrode material according to claim 1, It is characterized in that The particle size of the metal oxide is 100-800 nm.

6. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 1, It is characterized in that The particle size of the nickel-cobalt-manganese ternary single crystal positive electrode material is 2-6 μm.

7. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 1, It is characterized in that In the preparation process of the single crystal nickel cobalt lithium manganese oxide positive electrode material, in step (1), the proportion of solids in the slurry is 30% to 50%, and the water is ultrapure water.

8. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 1, It is characterized in that In the preparation process of the single crystal nickel cobalt manganese oxide positive electrode material, in step (1), the molar ratio of the lithium in the lithium source to the total of the nickel, cobalt and manganese elements in the precursor of formula (II) is 1.00-1.15:1; in step (2), the molar ratio of the lithium in the lithium source to the total of the nickel, cobalt and manganese elements in the precursor of formula (I) is 1.00-1.15:1; In step (1) or (2), the sintering temperature is 200-1000° C., the sintering time is 2-15 hours, and the sintering atmosphere in the atmosphere furnace is a gas containing oxygen with an oxygen content of 90% to 100%.

9. The single crystal lithium nickel cobalt manganese oxide positive electrode material according to claim 8, It is characterized in that In step (1) or (2), the sintering temperature is 400-1000° C. and the sintering time is 8-12 hours.

10. The single crystal nickel cobalt lithium manganese oxide positive electrode material according to claim 1, It is characterized in that In the preparation process of the single crystal nickel cobalt lithium manganese oxide positive electrode material, in step (3), the sintering temperature is 400-800° C. and the sintering time is 8-10 hours.

Citation Information

Patent Citations

  • Transition metal-metaphosphate anode active material, manufacturing method therefor, and lithium secondary battery or hybrid capacitor comprising same

    CN104641498A

  • Core-double-shell structure composite nickel-cobalt-manganese ternary precursor material and preparation method and application thereof

    CN111092205A

  • Preparation method of core-shell type high-voltage single-crystal lithium nickel cobalt manganate positive electrode material

    CN112054173A

  • Modification method of single-crystal ternary positive electrode material

    CN112080800A

  • Single-crystal nickel cobalt lithium manganate positive electrode material and preparation method and application thereof

    CN113629240A