Strengthened dual-phase magnetic material component and method of forming the same
By forming dual-phase magnetic components in the motor and using nitriding treatment and metal coating diffusion technology, the problems of magnetic microstructure stability and coercivity in motor design are solved, power density and efficiency are improved, and magnetic flux loss is reduced.
Patent Information
- Application Number
- CN202210410569.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-21
- Filing Date
- 2022-04-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-04-19
AI Technical Summary
In hybrid/electric vehicle traction applications with existing motors, there are trade-offs between power density, efficiency, and the machine's constant power speed range, resulting in design challenges, especially the presence of carbides in the magnetic microstructure that increases coercivity and reduces magnetic saturation. problem.
Dual-phase magnetic components are used to ensure the Stability at room temperature and the presence of high permeability regions.
It achieves the existence of the austenite phase in the middle region of the soft magnet that is stabilized at room temperature, reduces the coercive force, improves the strength and magnetic properties of the magnetic components, and at the same time reduces the magnetic flux loss.
Smart Images

Figure CN115216723B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to components having multiple magnetic and non-magnetic regions, and methods of forming the components. More specifically, the present disclosure relates to components having multiple magnetic and non-magnetic regions, and components formed by nitridation (eg, solution nitridation). Background Art
[0002] The need for high power density and high efficiency electric machines (i.e., motors and generators) has long been prevalent in a variety of applications, particularly hybrid and / or electric vehicle traction / propulsion applications. The current trend in hybrid / electric vehicle traction / propulsion electric machine applications is to increase the speed to increase the power density of the machine, thereby reducing its mass and cost. However, it is recognized that when electric machines are used in hybrid / electric vehicle traction applications, there is a clear tradeoff between power density, efficiency, and the machine's constant power speed range (limited by the mechanical strength of the rotor) - a tradeoff that presents many design challenges.
[0003] The power output of the motor can be increased by increasing the motor size, improving thermal management, increasing the rotor speed, or by increasing the magnetic utilization. The magnetic utilization can be increased by using a combination of machining and alloying of the rotor laminations to create a dual-phase magnetic material by forming localized regions of high and low magnetic permeability. The localized regions of high and low magnetic permeability generally reduce the flux losses during rotor operation.
[0004] A range of iron-based soft magnetic compositions of rotor laminations can be austenitized by a combination of processes to form low permeability regions. In the presence of carbides in the alloy, this phase transformation can be thermally driven in selected areas. Upon local heating, carbides located at selected locations dissolve in the matrix and reduce the martensite start temperature, thereby contributing to the stabilization of the austenitic regions at room temperature. However, the presence of carbides in the magnetic microstructure is known to increase the coercivity and reduce the magnetic saturation compared to conventional iron-based magnetic steels. A different approach is needed to stabilize the austenitic phase in the soft magnetic intermediate region at room temperature, starting from a substantially single-phase microstructure, in order to reduce the coercivity. Summary of the invention
[0005] Aspects and advantages will be set forth in part in the following description, or may be obvious from the description, or may be learned through practice of the invention.
[0006] A dual-phase magnetic component and a method for forming the same are generally provided. In one embodiment, the dual-phase magnetic component includes a first region and a second region intermixed with each other formed of a single material, wherein the first region has a magnetic region and a diffused metal therein, and the second region has a non-magnetic region. Nitrogen in the second region is typically greater than 0.1 wt%.
[0007] In one embodiment, a method of forming a dual-phase magnetic component may include forming a metal coating on a portion of a surface of an initial component to form a masked region while leaving an unmasked region on the surface. Thereafter, the initial component may be heated to a processing temperature in the presence of nitrogen so that the nitrogen diffuses into the unmasked region of the initial component to transform the magnetic iron composition in the unmasked region into a non-magnetic austenite composition. Heating may also diffuse the metal coating into the masked region of the initial component. Thereafter, the initial component may be cooled from the processing temperature to form a dual-phase magnetic component having a magnetic region corresponding to the masked region and a non-magnetic region corresponding to the unmasked region.
[0008] These and other features, aspects and advantages will be better understood with reference to the following description and appended claims.The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments of the invention and, together with the description, serve to explain certain principles of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] With reference to the accompanying drawings, the specification sets forth a complete and enabling disclosure of the present invention to one of ordinary skill in the art, including the best mode thereof, wherein:
[0010] Figure 1 shows a form of a masking component forming a dual-phase magnetic component according to one embodiment of the present invention;
[0011] Figure 2 A masking component form for forming a dual-phase magnetic component according to another embodiment of the present invention is shown;
[0012] Figure 3 A masking component form for forming a dual-phase magnetic component according to another embodiment of the present invention is shown;
[0013] Figure 4 For example, Figure 3 The dual-phase magnetic component formed after the coating is removed as shown;
[0014] Figure 5 An exemplary topology diagram of a dual-phase magnetic component according to an embodiment of the present invention is shown, which dual-phase magnetic component can be obtained by using the method described herein.
[0015] Repeated use of reference characters in the present specification and drawings is intended to represent the same or analogous features or elements of the present invention. DETAILED DESCRIPTION
[0016] Reference will now be made in detail to embodiments of the present invention, more than one example of which is shown in the accompanying drawings. Each example is provided to explain the present invention, rather than to limit the present invention. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present invention without departing from the scope of the present invention. For example, a feature illustrated or described as part of one embodiment may be used together with another embodiment to produce yet another embodiment. Therefore, the present invention is intended to encompass these modifications and variations within the scope of the appended claims and their equivalents.
[0017] Various embodiments of the present invention are directed to a reinforced dual phase magnetic component, a magnetic composition of a reinforced dual phase magnetic component, and a method of forming a reinforced dual phase magnetic component.
[0018] In one embodiment of the present invention, a reinforced dual-phase magnetic component is disclosed. As used herein, the term "dual-phase magnetic component" may be a magnetic portion of any product, such as a rotor or stator lamination of an electric machine, having a first region and a second region intermixed with each other, wherein the first region includes a magnetic phase and the second region includes a non-magnetic phase. "Intermixed first region and second region" herein means that there are multiple first regions and second regions adjacent to each other.
[0019] Therefore, the dual-phase magnetic component has a dual magnetic region, in which one set of regions has a magnetic phase and the other set of regions has a non-magnetic phase. As used herein, a "magnetic phase" is a region in which more than 99% by volume is magnetic, and is generally used as a magnetic region. In addition, a "non-magnetic phase" can be a region in which more than 90% by volume is non-magnetic. The magnetic component as used herein is generally prepared from a single material. As an example, the material can be a composite magnetic member formed by providing a ferromagnetic portion and a non-magnetic portion and nitriding in a controlled atmosphere. When the magnetic component is made of a single material, the negative impact when the ferromagnetic portion and the non-magnetic portion are combined is reduced by ensuring the reliability, airtightness and bonding strength of the magnetic component.
[0020] As used herein, a "magnetic phase" is a material in a magnetic state having a relative magnetic permeability greater than 1. In one embodiment, the magnetic phase of the first region of the magnetic component has a relative magnetic permeability greater than 100 and a saturation magnetization greater than 1.5 Tesla. As used herein, a "non-magnetic phase" is a material having a magnetic permeability of about 1 greater than 90% by volume and a saturation magnetization of about zero.
[0021] Austenite, also known as gamma iron (γ-Fe), is a metallic non-magnetic allotrope of iron or a solid solution of iron. Heating iron, an iron-based metal, or steel to a temperature at which the crystal structure changes from ferrite to austenite is called austenitizing. The addition of certain alloying elements, such as manganese, nickel, nitrogen, and carbon, stabilizes the austenite structure even at room temperature. Dual-phase magnetic components can be formed by stabilizing austenite in some areas of the magnetic component at room temperature while retaining a strongly ferromagnetic martensite phase or ferrite phase in some other areas of the magnetic component.
[0022] The presence of carbon is known to stabilize the non-magnetic austenite structure. Early studies have involved dissolving the formed carbides in selected areas of the magnetic component to stabilize the non-magnetic phase at that area of the magnetic component. In one embodiment of the present invention, the non-magnetic region of the magnetic component is formed by adding nitrogen (rather than carbon) to stabilize the low permeability austenite structure. It is known that carbides as a second phase are undesirable for magnetic components. Therefore, in some embodiments of the present invention, the material forming the magnetic component is substantially free of carbon.
[0023] However, in other embodiments of the invention, the composition may include relatively small amounts of carbon, which can sometimes increase the tensile strength of the magnetic region. In these embodiments, the total amount of carbon in the magnetic and nonmagnetic regions must be less than about 0.05 wt%.
[0024] The second (non-magnetic) region contains nitrogen in an amount that can stabilize the austenite phase. Like carbon, when nitrogen is dissolved in an iron alloy, the austenite phase is stabilized. Typically, the presence of carbides (which are used to stabilize the austenite phase during local heat treatment and dissolution) is established by alloying the initial material with carbon in the melt. When nitrogen is used to alloy iron, the machinability of the alloy is typically reduced. In certain embodiments of the present application, nitriding is used after the machining of the component has been substantially completed.
[0025] In one embodiment, a method for preparing a magnetic component is disclosed. Thermodynamic and empirical calculations can be used to predict iron alloy compositions that form an austenite phase after the addition of nitrogen at high temperatures. Magnetic components using the designed iron alloy compositions can be formed using conventional methods. In one embodiment, the formed magnetic component is subjected to selective nitridation close to the final component without significantly changing the shape and size of the formed magnetic component after nitriding. As used herein, the term "selective nitridation" is the nitridation of some (desired) regions of a magnetic component, which does not substantially change the ferromagnetic properties of nearby regions. The ferromagnetic properties of nearby regions can be considered to be "significantly changed" if the average saturation magnetization of these regions is reduced by more than 5%.
[0026] In one embodiment, selective nitridation of the magnetic component may be achieved by using a metal coating that prevents nitrogen from diffusing into the magnetic component, which may act as a "nitrogen barrier" material in some areas.
[0027] Nitriding can be performed by solid, liquid, gas or plasma routes. In one embodiment of the invention, high temperature gas nitriding is the preferred method for introducing nitrogen into the component. The high temperatures in this technique allow for rapid diffusion of nitrogen, providing a rapid processing route. Alternatively, plasma nitriding can be used for nitrogen diffusion. In order to avoid diffusion of nitrogen in those areas that are intended to maintain ferrite (and therefore magnetic properties), in one embodiment, a metal coating is applied to locations where nitrogen diffusion is not desired. Therefore, in this embodiment, preselected areas corresponding to areas where magnetism should be maintained are masked, using the metal coating as a nitrogen barrier material (i.e., inhibiting and / or substantially preventing nitrogen from entering the masked area).
[0028] exist Figure 1 , a magnetic component that has been selectively nitrided and diffused into a metal coating into a substrate to form a reinforced dual-phase magnetic component is exemplified. The initial component 10 is formed of a ferromagnetic material and has a size and shape that is desired for the final application of the resulting component. In one embodiment, the initial component 10 is formed of a composition having a very low carbon concentration (e.g., a carbon concentration of less than 0.05% by weight, such as being substantially free of carbon) and can be of any shape and size. Although it should be understood that the shape of the initial component 10 can be determined as required by the component application, for ease of understanding, the initial component 10 is shown in FIG. Figure 1 and 2 The initial component 10 in FIG. 1 is depicted as having a rectangular shape, with an upper surface 12 and a lower surface 14. The initial component 10 has a certain length (l), width (w) and thickness (t).
[0029] More specifically Figure 3 As shown, the metal coating 16 is applied to a portion of the surfaces 12, 14 to define a first region 20 (corresponding to the masked region 21) and a second region 30 (corresponding to the unmasked exposed region 31).
[0030] The magnetic component 10 has a certain length (l), width (w) and thickness (t). The magnetic component 10 includes two marking areas, a first area 20 and a second area 30. The positions of these areas are such that the first area 20 (corresponding to the masked area 21 below it) has a metal coating 16 on the surface portion of its component, and the second area 30 (corresponding to the unmasked area 31) has an unmasked surface (i.e., there is basically no metal coating on it). The first area 20 is designed as a magnetic area and is masked using the metal coating 16 in the component 10. The second area 30 is not masked, so nitrogen is allowed to diffuse through the component 10, making these areas non-magnetic. It will be appreciated by those skilled in the art that the mask can be designed in different shapes on different surfaces according to the shape and size of the desired magnetic and non-magnetic areas.
[0031] The nitrogen may be diffused into the component 10 by gas nitridation in a nitrogen-rich atmosphere at a process pressure and process temperature sufficient to diffuse the nitrogen into the second region 30 of the component 10. Generally, it is expected that the diffusion of nitrogen will increase with higher heat treatment temperatures and increased nitrogen equilibrium surface concentrations. An increase in the gas pressure surrounding the magnetic component 10 often results in an increase in the surface concentration of nitrogen. Therefore, under given conditions in a pure nitrogen atmosphere, higher than atmospheric pressure and higher temperatures generally provide a faster nitridation process. For example, nitridation and metal diffusion use a process pressure greater than 1 atmosphere and a process temperature greater than 900°C (e.g., 900°C to 1400°C), such as a process temperature greater than 1000°C (e.g., 1000°C to 1250°C). In a particular embodiment, the process temperature may be higher than the melting point of the metal coating (e.g., higher than the melting point of the metal coating to 140% of the melting point of the metal coating, such as higher than the melting point of the metal coating to 130% of the melting point of the metal coating). For example, when the metal coating is made of pure copper (melting point is 1085° C.), the processing temperature may be higher than 1085° C. (eg, higher than 1085° C. to 1410° C.).
[0032] In one embodiment, a nitrogen-rich atmosphere is used. For example, the nitrogen-rich atmosphere may include more than 90% by volume of nitrogen (e.g., more than 95% by volume of nitrogen). In one embodiment, the nitridation is performed in a substantially pure nitrogen atmosphere. The substantially pure nitrogen atmosphere may be generated by filling the furnace chamber with nitrogen after evacuating air from the furnace chamber, and then purging with nitrogen or continuously flowing nitrogen into the atmosphere chamber during the process.
[0033] The metal coating 16 may be applied to the surfaces 12, 14 of the component 10, depending on the desired pattern of metal diffusion (without nitrogen diffusion) versus nitrogen diffusion of the component 10. In one embodiment, all of the surface of the component 10 is defined by either the first region 20 or the second region 30 of the component 10, such that the entire surface of the component 10 is either a metal diffusion region (i.e., a magnetic region) or a nitrogen diffusion region (i.e., a non-magnetic phase). Typically, the nitrogen diffusion region is substantially free of any added (from metal diffusion) metal other than the metal originally present in the initial alloy itself, since no metal coating is present on the surface forming the non-magnetic region.
[0034] The metal coating 16 may be formed by any suitable method to a coating thickness sufficient to inhibit nitridation therethrough and sufficient to increase the strength properties of the component 10 through its diffusion. However, if the metal coating 16 is too thick, the excess diffused metal may alter the magnetic properties of the component 10 below it. Without wishing to be bound by any particular theory, it is believed that higher amounts of diffused metal (particularly copper) increase the strength of the component 10, but excess diffused metal may alter the magnetic saturation of the component 10. In a particular embodiment, the metal coating 16 is formed to a coating thickness of 0.1 μm to 25 μm in the masked area, such as a coating thickness of 0.5 μm to 10 μm (e.g., 1 μm to 5 μm) in the masked area.
[0035] The metallic coating 16 may be formed of a metal or metal alloy that is suitable for inhibiting nitridation therethrough and for diffusing into the ferrite composition of the component 10 to provide solid solution strengthening or precipitation strengthening. Without wishing to be bound by any particular theory, it is believed that metals with slow nitrogen diffusion rates are suitable for use as masking agents. Without wishing to be bound by any particular theory, it is believed that the diffused metal (e.g., copper) is incorporated as a solid solution in the ferrite matrix or forms a precipitation dispersion in the ferrite matrix, which increases the strength of the component 10. Particularly suitable metals for the metallic coating 16 include those that form solid solutions and precipitates in the host metal composition (e.g., ferrite composition).
[0036] In particular embodiments, the metal coating 16 may include copper, nickel, tin, chromium, silver, platinum, gold, boron, magnesium, thorium, zirconium, hafnium, niobium, tantalum, molybdenum, tungsten, rhenium, vanadium, or alloys thereof. For example, the metal coating 16 can be a copper-based composition (i.e., greater than 50 weight percent copper), a nickel-based composition (i.e., greater than 50 weight percent nickel), a tin-based composition (i.e., greater than 50 weight percent tin), a chromium-based composition (i.e., greater than 50 weight percent chromium), a silver-based composition (i.e., greater than 50 weight percent silver), a platinum-based composition (i.e., greater than 50 weight percent platinum), a gold-based composition (i.e., greater than 50 weight percent gold), a boron-based composition (i.e., greater than 50 weight percent boron), a magnesium-based composition (i.e., greater than 50 weight percent magnesium), a thorium-based composition (i.e., greater than 50 weight percent thorium), a zirconium-based composition (i.e., greater than 50 weight percent zirconium), a hafnium-based composition (i.e., greater than 50 weight percent hafnium), a niobium-based composition (i.e., greater than 50 weight percent niobium), a tantalum-based composition (i.e., greater than tantalum), a molybdenum-based composition (i.e., greater than 50 weight percent molybdenum), a tungsten-based composition (i.e., greater than 50 weight percent tungsten), a rhenium-based composition (i.e., greater than 50 weight percent rhenium), or a vanadium-based composition (i.e., greater than 50 weight percent vanadium). In one particular embodiment, the metallic coating 16 may have a copper-based composition that is greater than 50 wt. % copper (eg, 75 wt. % to 100 wt. % copper).
[0037] exist Figure 1 In the embodiment, the metal coating 16 is applied on the surfaces 12, 14 corresponding to the first region 20 and on the surface covering the thickness of the component 10. Thus, Figure 1 In the embodiment of the present invention, nitridation will only proceed through the second region 30 on the upper surface 12 and the lower surface 14 to form the unmasked region 31, rather than through the thickness of the component. Figure 2 In the embodiment, the surface through the thickness of the component 10 also includes masked areas and unmasked areas, so that nitrogen diffusion occurs in a controlled manner on the upper surface, the lower surface and the side surfaces.
[0038] When the magnetic component is gas nitrided, nitrogen diffuses into the component 10 and through all unmasked surfaces of the component 10, including the upper surface 12, the lower surface 14, and all unmasked side surfaces of the component. The nitrogen during the nitriding process diffuses from the surface of the component 10 to the interior in the unmasked areas 30. This diffused nitrogen combines with the composition of the magnetic component to change the local phase stability in these areas and transform these areas into non-magnetic austenite. Even though the nitrogen diffuses through the surface, the nitriding parameters allow the nitrogen to diffuse further through all surfaces of the magnetic component 10 into the length, width, and thickness of the magnetic component, while the masked areas 30 prevent a significant amount of nitrogen from diffusing through these areas.
[0039] Nitrogen can diffuse into the interior of the component 10 through the unmasked surface area, but depending on the pressure and temperature and certain other parameters, the diffused nitrogen can also slightly undercut the surface masked area 20, thereby diffusing into the interior of some masked areas 21. Therefore, the strict boundary of the magnetic area and the non-magnetic area in the surface portion may diffuse more in the inner portion. As a result, the percentage of non-magnetic area in the inner portion may be greater than the percentage of non-magnetic area in the surface portion. Therefore, in one embodiment, the volume percentage of the second area in the inner portion is equal to or greater than the volume percentage of the second area in the surface portion. Therefore, if a hypothetical line starting from the surface of the second (non-magnetic) area passes through the inner portion in a direction perpendicular to the surface portion, it is very likely that the perpendicular line intersects the second area substantially 100%. However, this may not always be the case for a line drawn in the same way starting from the surface of the first (magnetic) area. In one embodiment, the "undercut" of the non-magnetic phase is less than 200 microns.
[0040] Through experience and thermodynamic calculations, the parameters of nitridation can be adjusted and nitrogen diffusion in different directions for certain regions of the magnetic component 10 can be predicted, so that the size and shape of the mask can be changed to obtain a final product that is approximately the desired result of the nitridation process.
[0041] In thinner magnetic components, the undercutting of the nonmagnetic phase may be less. In thinner components, most of the nitrogen is introduced through the upper surface 12 and the lower surface 14 ( Figure 2 ) diffusion, and the amount of undercutting can be reduced. In addition, less time is required to achieve full thickness nitrogen penetration, thereby reducing the amount of time that additional nitrogen diffuses under the mask to produce undercutting. In one embodiment, the thickness of the component 10 is in the range of 0.1 mm to 5 mm. The desired pattern of magnetic and non-magnetic regions of the component can be obtained by diffusing nitrogen through the selectively masked upper surface 12 and lower surface 14, while keeping the side surfaces of thickness t completely masked.
[0042] The width 22 of the mask of the masking area 20 ( Figure 2 ) is the dimension between the unmasked areas 30 and can be designed according to the desired magnetic component 10. In one embodiment, the width 34 of each second area 30 in the surface is greater than 0.5 mm. In a further embodiment, the width of each second area 30 in a plane perpendicular to the thickness t is greater than 0.5 mm. (As previously described, Figure 2 The dimension "w" in FIG. 1 represents the overall width of the magnetic component 10. )
[0043] Nitriding the magnetic component under designed conditions allows a quantitative amount of nitrogen to be introduced and diffused into the magnetic component intermittently. In one embodiment, the second (unmasked) region 30 contains more than 0.4% nitrogen. The mixing and concentration of nitrogen is not limited to the unmasked area of the surface, but also exists in the surface portion and the internal portion of the magnetic component 10. The nitrogen concentration of the surface portion and the internal portion does not need to be uniform.
[0044] Figure 4 The dual phase magnetic component 100 is shown after nitridation and diffusion of a metal coating therein. The dual phase magnetic component 100 includes a magnetic region 102 (corresponding to Figure 3 The masking area 21 and the non-magnetic area 104 (corresponding to Figure 3 In a specific embodiment, the magnetic region 102 comprises an iron alloy composition having a nitrogen concentration of 0.1 wt % or less (e.g., 0.05 wt % or less) and a diffused metal 103 therein. The magnetic region 103 (corresponding to Figure 3 The diffused metal 103 in the masked region 21 of the magnetic region 103 can form a substantially uniform composition in the magnetic region 103, or form a composition gradient through the thickness in the magnetic region 103. For example, in a specific embodiment, the composition gradient in the magnetic region 103 is such that the diffused metal in the magnetic region 103 (corresponding to Figure 3 The surface concentration on the first region 20 and the masking region 21) is greater than that on the magnetic region 103 (corresponding to Figure 3 In contrast, the nitrogen concentration of the nonmagnetic region 104 of the dual-phase magnetic component 100 may be greater than 0.1 wt %, such as greater than 0.4 wt %.
[0045] The metal coating 16 diffuses into the masking region 21 at a processing temperature during nitridation or at a diffusion temperature after nitridation (which is greater than the processing temperature), forming a diffusion region 103. In some embodiments, the depth of the diffusion region 103 from the surface 12, 14 into the component 100 can be greater than the thickness of the original metal coating.
[0046] Similar to nitridation, the diffusion of the metal coating 16 to the interior of the masked area 21 may also slightly undercut the unmasked area 30 of the surface, thereby diffusing to the interior of some of the unmasked areas 31. Therefore, the strict boundary of the metal diffusion area in the surface portion may be more diffuse in the inner portion. However, the metal concentration of the diffusion metal of the masked area 21 corresponding to the first area 20 is greater than that of the unmasked area 31 corresponding to the second area 30. For example, the diffusion metal concentration of the masked area 21 corresponding to the first area 20 may be 10 times higher than that of the diffusion metal concentration of the unmasked area 31 corresponding to the second area 30.
[0047] In certain embodiments, diffusion of the metal coating 16 into the masked areas 21 removes the need for a mask removal process (eg, mechanical or chemical etching) on the surface of the component 10 .
[0048] Depending on the application, the shape and ratio of the desired magnetic and non-magnetic regions can vary, and the diffusion of nitrogen can be designed to meet these requirements. Therefore, in one embodiment, the volume percentage of the first region in the surface portion and the interior portion is equal to or greater than the volume percentage of the second region in the surface portion and the interior portion. In one embodiment, at least one of the first region and the second region has an interconnected geometry. As used herein, "interconnected geometry" refers to a region that is fully connected through a component and is therefore not completely isolated from similar regions, and is completely surrounded by other regions.
[0049] By using this technique, different topological structures with dual-phase magnetic materials can be presented. Figure 5 An example of a topology that can benefit from a two-phase material is shown. Component 40 can represent a portion of a reluctance machine, including a magnetic region 42 and a non-magnetic region 44, hereinafter collectively referred to as a "stack segment". The selectively shaped rotor 43 of component 40 is configured as a four-pole machine. Each pole can include a plurality of axially extending, radially positioned ("stacked") stack segments 45, 47, 49, etc., extending from each pole and terminating at a central rotor axis 51. As described in the Shah patent, the number of poles and the number of stacks can vary greatly, depending on the specific design of the reluctance machine.
[0050] Continue to refer Figure 5 , the lamination segments effectively direct the magnetic flux into and out of the rotor 43. The magnetic regions 42 restrict the path of the magnetic flux, while the non-magnetic regions 44 ensure a relatively high density of magnetic flux lines out of the rotor surface and into the air gap between the rotor and stator. When manufacturing these types of reluctance machines according to conventional techniques, the magnetic laminations and non-magnetic laminations must typically be assembled through various mechanical / metalworking steps such as cutting and welding. The inventors have discovered that many of the desired techniques can be more efficiently obtained through the masking and nitriding processes described herein.
[0051] Example
[0052] A copper coating having a thickness of less than 1 mil is applied to a portion of the magnetic ferrous substrate by electroplating. Another portion of the magnetic ferrous substrate is uncoated (ie, the exposed surface of the magnetic ferrous substrate).
[0053] The selectively coated substrate is then nitrided for 30 minutes at a nitriding temperature of 1150°C under a nitrogen atmosphere. The heating rate of the substrate is 10°C per minute until the nitriding temperature. The nitrided substrate is then quenched with nitrogen for rapid cooling. In this embodiment, the substrate is moved from the hot zone to the cold zone and nitrogen quenched by increasing the nitrogen flow rate (e.g., 25 cubic feet per hour or more). Other nitrogen quenching methods may be used (e.g., forced nitrogen cooling by increasing the nitrogen flow rate at the processing temperature with the heat source turned off / removed).
[0054] The nitriding temperature is above the melting point of copper (about 1,085°C). Without wishing to be bound by any particular theory, it is believed that the copper coating melts at the nitriding temperature and forms an alloy with the substrate. The rapid cooling from the nitriding temperature then causes fine Cu precipitates to form within the substrate.
[0055] After nitridation, the copper-coated areas remained magnetic, indicating that the copper effectively blocked the diffusion of nitrogen into the substrate. In addition, it was clear from the color change of the substrate's outer surface that the copper coating diffused into the iron substrate.
[0056] The saturation magnetization measured in the Cu diffused region was 14.9 kG, close to the 15.3 kG of the initial substrate. Thus, there was little or no debit in the magnetic properties of the substrate due to the copper diffusion therein. In addition, the hardness was shown to increase from 2 HRC to 25 HRC, which also confirmed the strengthening of the Cu precipitates.
[0057] The unmasked areas became nonmagnetic, indicating that nitridation occurred in the unmasked areas.
[0058] Other aspects of the invention are provided by the following clauses:
[0059] 1. A dual-phase magnetic component comprising: a first region and a second region formed of a single material and intermixed with each other, the first region comprising a magnetic region and having diffused metal therein, the second region comprising a non-magnetic region, the second region containing more than 0.1 wt % nitrogen.
[0060] 2. A component according to any preceding clause, wherein the diffusion metal comprises copper, nickel, tin, boron, magnesium, thorium, zirconium, hafnium, niobium, tantalum, molybdenum, tungsten, rhenium, vanadium or alloys thereof.
[0061] 3. A component according to any preceding clause, wherein the diffusion metal comprises a copper-based metal, a nickel-based metal or a tin-based metal.
[0062] 4. A component according to any preceding clause, wherein the diffusion metal comprises at least 50 wt. % copper.
[0063] 5. A component according to any preceding clause, wherein the strength of the component in the first region is greater than the strength of an otherwise identical component apart from the diffusion metal coating therein.
[0064] 6. A component according to any preceding clause, wherein the diffusion metal forms a composition gradient within the first region such that a surface concentration of the diffusion metal on the first region is greater than an internal concentration within the first region.
[0065] 7. A component according to any preceding clause, wherein the second region comprises greater than 0.4 wt. % nitrogen.
[0066] 8. A component according to any preceding clause, wherein the nitrogen concentration of the first region is less than 0.1 wt. %.
[0067] 9. A component according to any preceding clause, wherein the carbon concentration in both the first region and the second region is less than 0.05 wt. %.
[0068] 10. A method of forming a dual-phase magnetic component from an initial component, the initial component comprising a magnetic iron composition and having a surface, the method comprising: forming a metal coating on a portion of the surface of the initial component to obtain masked areas while leaving unmasked areas on the surface; thereafter, heating the initial component to a treatment temperature in the presence of nitrogen so that the nitrogen diffuses into the unmasked areas of the initial component, transforming the magnetic iron composition into a non-magnetic austenitic composition in the unmasked areas, wherein the heating also diffuses the metal coating into the masked areas of the initial component; thereafter, cooling the initial component from the treatment temperature to form a dual-phase magnetic component having magnetic areas corresponding to the masked areas and non-magnetic areas corresponding to the unmasked areas.
[0069] 11. A method according to any preceding clause, wherein the diffused metal coating increases the strength of the initial component in the magnetic region.
[0070] 12. A method according to any preceding clause, wherein the metal coating comprises copper, nickel, tin, boron, magnesium, thorium, zirconium, hafnium, niobium, tantalum, molybdenum, tungsten, rhenium, vanadium or alloys thereof.
[0071] 13. A method according to any preceding clause, wherein the metal coating comprises a copper-based composition, a nickel-based composition or a tin-based composition.
[0072] 14. A method according to any preceding clause, wherein the metallic coating comprises greater than 75 wt. % copper.
[0073] 15. A method according to any preceding clause, wherein the non-magnetic region contains greater than 0.4 wt% nitrogen, and the metal coating inhibits diffusion of nitrogen into the masking region such that the nitrogen concentration of the magnetic region is less than 0.1 wt%.
[0074] 16. A method according to any preceding clause, wherein the metal coating is formed in the masked area to a thickness of 0.1 μm to 25 μm.
[0075] 17. A method according to any preceding clause, wherein the treatment temperature is above 900°C.
[0076] 18. A method according to any preceding clause, wherein the metal coating has a melting point and the processing temperature is above the melting point of the metal coating to 130% of the melting point of the metal coating.
[0077] 19. A method according to any preceding clause, wherein heating the initial component to a processing temperature in the presence of nitrogen comprises: forming a nitrogen-rich atmosphere around the initial component, the nitrogen-rich atmosphere comprising more than 90 volume % nitrogen, the processing pressure of the nitrogen-rich atmosphere being more than 0.5 atmospheres.
[0078] 20. The method of any preceding clause, wherein the diffused metal forms a composition gradient within the magnetic region such that the diffused metal has a surface concentration on the surface of the magnetic region that is greater than an interior concentration within the magnetic region.
[0079] This written description uses exemplary embodiments to disclose the invention, including the best mode, and also enables any person skilled in the art to practice the invention, including making and using any device or system and performing any combined method. The patent scope of the invention is defined by the claims, and may include other examples that occur to one skilled in the art. If these other examples include structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that do not differ substantially from the literal language of the claims, they fall within the scope of the claims.
Claims
1. Dual-phase magnetic components, including: The first region and the second region are formed of a single material and mixed with each other, wherein the first region includes a magnetic region and has a diffused metal therein, the diffused metal forming a composition gradient within the first region such that a surface concentration of the diffused metal on the first region is greater than an internal concentration within the first region; The second region includes a nonmagnetic region, wherein the second region includes greater than 0.1 wt % nitrogen.
2. The component according to claim 1, wherein The diffusion metal includes copper, nickel, tin, boron, magnesium, thorium, zirconium, hafnium, niobium, tantalum, molybdenum, tungsten, rhenium, vanadium or alloys thereof.
3. The component according to claim 1, wherein The diffusion metal includes a copper-based metal, a nickel-based metal or a tin-based metal.
4. The component according to claim 1, wherein The diffusion metal comprises at least 50 wt % copper.
5. The component according to claim 1, wherein The strength of the component in the first region is greater than the strength of an otherwise identical component except for the diffusion metal coating therein.
6. The component according to claim 1, wherein The second region comprises greater than 0.4 wt % nitrogen.
7. The component according to claim 1, wherein The nitrogen concentration of the first region is less than 0.1 wt %.
8. The component according to claim 1, wherein The carbon concentration in both the first region and the second region is less than 0.05 wt %.
9. A method of forming a dual phase magnetic component according to any one of claims 1 to 8 from an initial component comprising a magnetic iron composition and having a surface, the method comprising: forming a metal coating on a portion of the surface of the initial component to obtain masked areas while leaving unmasked areas on the surface; thereafter, heating the initial component to a treatment temperature in the presence of nitrogen gas so that the nitrogen gas diffuses into unmasked areas of the initial component, transforming the magnetic ferrous composition into a non-magnetic austenitic composition in the unmasked areas, wherein the heating also diffuses the metal coating into masked areas of the initial component to form a diffused metal coating; Thereafter, the initial component is cooled from the processing temperature to form a dual-phase magnetic component having magnetic regions corresponding to the masked regions and non-magnetic regions corresponding to the unmasked regions.
10. The method according to claim 9, wherein: The diffused metal coating increases the strength of the initial component in the magnetic region.
11. The method according to claim 9, wherein: The metal coating includes copper, nickel, tin, boron, magnesium, thorium, zirconium, hafnium, niobium, tantalum, molybdenum, tungsten, rhenium, vanadium or alloys thereof.
12. The method according to claim 9, wherein: The metal coating includes a copper-based composition, a nickel-based composition, or a tin-based composition.
13. The method according to claim 9, wherein: The metal coating contains more than 75 wt % copper.
14. The method according to claim 9, wherein: The nonmagnetic region contains greater than 0.4 wt % nitrogen, and the metal coating inhibits diffusion of nitrogen into the masking region such that the magnetic region has a nitrogen concentration of less than 0.1 wt %.
15. The method according to claim 9, wherein: The metal coating is formed in the masked area to have a thickness of 0.1 μm to 25 μm.
16. The method according to claim 9, wherein: The processing temperature is above 900°C.
17. The method according to claim 9, wherein: The metal coating has a melting point, and the processing temperature is higher than the melting point of the metal coating to 130% of the melting point of the metal coating.
18. The method according to claim 17, wherein: Heating the initial component to a processing temperature in the presence of nitrogen comprises: A nitrogen-rich atmosphere is formed around the initial component, wherein the nitrogen-rich atmosphere includes 90 volume % or more of nitrogen, and a treatment pressure of the nitrogen-rich atmosphere is 0.5 atmospheres or more.
19. The method according to claim 9, wherein: The diffused metal forms a composition gradient within the magnetic region such that a surface concentration of the diffused metal on the surface of the magnetic region is greater than an interior concentration within the magnetic region.