Method for preparing antibacterial and stain-resistant handbags by recycling waste fiber cloth
Through the steps of crushing and opening, cleaning and impurity removal, decolorization, sterilization, and sorting and blending, combined with seaweed fiber and antibacterial and stain-resistant finishing agents, the problem of removing impurities and bacteria in waste fiber cloth was solved, and a portable handbag with good antibacterial and stain-resistant properties was solved. bag, extending service life.
Patent Information
- Application Number
- CN202210801311.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-07-08
AI Technical Summary
In the prior art, antibacterial and stain-resistant handbags made from waste fiber cloth cannot completely remove impurities and bacteria, resulting in insufficient performance.
It adopts the steps of crushing and opening, cleaning and impurity removal, decolorization and sterilization, sorting and blending, antibacterial and stain-resistant finishing, dyeing and color fixation, cutting and casting, and handle installation. It is cleaned with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide. Use decolorizing liquid and sterilizing liquid to remove impurities and bacteria, add seaweed fiber to improve antibacterial performance, and use antibacterial and stain-resistant finishing agents to form a hydrophobic, oleophobic, and self-cleaning film.
It achieves good antibacterial and stain-resistant performance and extends the service life of the handbag, ensuring that the outer surface is clean and waterproof and stain-resistant.
Smart Images

Figure BDA0003737858260000051 
Figure BDA0003737858260000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber cloth regeneration, and in particular to a method for preparing an antibacterial and stain-resistant handbag by regenerating waste fiber cloth. Background Art
[0002] A large amount of waste fiber textiles are generated in the process of enterprise production, daily life and fiber product manufacturing. At present, mechanical methods, chemical methods or energy recovery methods are mainly used to recycle and reuse waste fiber textiles. The mechanical method reprocesses them into short fibers and yarns through processing and cutting techniques; the chemical method modifies the surface of synthetic fiber macromolecules to obtain new fibers; the energy recovery method generates heat through incineration for thermal power generation.
[0003] There are many reports on the preparation of antibacterial and stain-resistant fabrics or textiles in the prior art. For example, the patent with publication number CN113802366A discloses a salt water-resistant and stain-resistant textile fabric, which is made of 20-23tex blended yarn, and the blended yarn contains the following weight percentages: 70% acrylic fiber, 10% wool, 10% nylon, and 10% antibacterial fiber; during preparation, the anti-stain and water-resistant finishing agent is diluted 80-100 times with water to obtain a mixed treatment liquid, and the fabric base is immersed in the mixed treatment liquid, heated, rinsed with water, dried, and then dyed and fixed. However, there are few reports on the preparation of antibacterial and stain-resistant handbags from waste fiber cloth, and there are the following technical problems: impurities, pigments, and bacteria in the waste fiber cloth cannot be completely removed, and the prepared handbags cannot have good antibacterial and stain-resistant properties. Summary of the invention
[0004] The purpose of the present invention is to provide a method for regenerating waste fiber cloth to prepare antibacterial and stain-resistant handbags, which is used to solve the technical problem in the prior art that impurities, pigments and bacteria in the waste fiber cloth cannot be completely removed and the prepared handbags cannot have good antibacterial and stain-resistant properties.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The method for preparing antibacterial and stain-resistant handbags by regenerating waste fiber cloth comprises the following steps:
[0007] Crushing and opening: Select waste cotton fiber and polyester fiber blended fiber cloth, crush it to a length and width of 1 to 3 cm, pass it into the opening machine for opening and combing, remove magnetic impurities to obtain opened mixed fiber;
[0008] Cleaning and removing impurities: the opened mixed fiber is sequentially cleaned and filtered with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide, and then dried to obtain the impurity-removed mixed fiber;
[0009] Decolorization and sterilization: immerse the impurity-removed mixed fiber in a decolorization solution at 60-72°C for 30-50 minutes, rinse with clean water, dry, immerse in a sterilization solution at 40-55°C for 45-60 minutes, rinse with clean water, and dry to obtain the sterilized mixed fiber;
[0010] Sorting and blending: feeding the sterilized mixed fiber into a fiber sorting machine, and sorting the cotton fiber and the polyester fiber according to the different densities to obtain the regenerated cotton fiber and the regenerated polyester fiber; weighing 65% of the regenerated polyester fiber, 20% of the regenerated cotton fiber and 15% of the seaweed fiber according to the weight percentage, spinning and weaving to obtain the blended base fabric;
[0011] Antibacterial and stain-resistant finishing: the blended base fabric is immersed in the antibacterial and stain-resistant finishing agent, immersed three times and dried three times to obtain the antibacterial and stain-resistant blended fabric;
[0012] Dyeing and color fixing: the antibacterial and stain-resistant blended fabric is dyed and fixed to obtain a dyed blended fabric;
[0013] Cutting and casting: After the dyed blended fabric is cut to the required size of the handbag, a waterproof and stain-resistant film material is coated on its inner surface through a casting machine, and a waterproof and stain-resistant inner film is obtained after drying, and then a bag-making machine is used to make bags to obtain the semi-finished handbags;
[0014] Handle installation: Sew or glue the non-woven fabric handle onto the semi-finished handbag to obtain the finished handbag.
[0015] The crushing and opening step of the present invention crushes and rips apart the fiber cloth and removes the magnetic impurities inside. The cleaning and impurity removal step uses distilled water, ethanol, acetone, phosphoric acid and potassium hydroxide to clean and remove water-soluble impurities, oil-soluble impurities, acidic impurities and alkaline impurities in the opened mixed fiber, thereby obtaining the impurity-removed mixed fiber with a clean outer surface.
[0016] The decolorization and sterilization steps are sequentially performed by decolorization with a decolorization solution and sterilization with a sterilization solution. 1-aminoethyl-2-heptadecylimidazolium hydrochloride in the decolorization solution is used as a cationic surfactant. Sodium aluminate plays a role in purifying water quality during the decolorization process. Polyvinyl alcohol dispersed in water has certain viscosity and film-forming properties and can adsorb solid pigment components. Ammonium chloride is dissolved in water to ionize ammonium radicals and chloride ions, which can be combined with charged pigment components in the form of electrons for removal. The carboxymethyl chitosan in the sterilization solution has a good inhibitory effect on common bacteria such as Escherichia coli. Glyceryl monostearate is used as a nonionic surfactant, so that the carboxymethyl chitosan is dispersed in water under the dispersing and defoaming effects of glyceryl monostearate, and penetrates into the mixed fiber more evenly, killing and inhibiting bacteria and viruses in the mixed fiber.
[0017] In the sorting and blending step, the regenerated polyester fiber, the regenerated cotton fiber and the antibacterial, mildew-proof and flame-retardant seaweed fiber are spun and woven to obtain a blended base fabric. The regenerated polyester fiber has good wrinkle resistance, elasticity and dimensional stability, and the regenerated cotton fiber has good strength and hygroscopicity, so that the blended base fabric has good strength, antibacterial and hygroscopicity.
[0018] In the antibacterial and stain-resistant finishing step, epichlorohydrin and perfluorotripropylamine hydrochloride are reacted in anhydrous ethanol as a solvent to undergo a nucleophilic substitution reaction, and intermediate a is obtained by post-treatment; multi-walled carbon nanotubes are oxidized by nitric acid vapor to obtain oxidized multi-walled carbon nanotubes with carboxyl groups on the surface; intermediate a and oxidized multi-walled carbon nanotubes are reacted under the catalysis of triethylamine to obtain antibacterial and stain-resistant powder grafted with quaternary ammonium salts; the antibacterial and stain-resistant powder is mixed with water to obtain an antibacterial and stain-resistant finishing agent. Among them, perfluorotripropylamine hydrochloride has multiple fluorine-carbon bonds, good stability and extremely low surface energy; multi-walled carbon nanotubes have excellent physical and mechanical properties, and the surface has carboxyl groups after oxidation to improve the reaction activity; the antibacterial and stain-resistant powder grafted with quaternary ammonium salts enters the blended base fabric under the dispersion effect of water, and forms a hydrophobic, oil-repellent, self-cleaning, high-strength film after drying, which has excellent waterproof and stain-resistant effects.
[0019] In the cutting and casting step, a layer of waterproof and stain-resistant film material is coated on the inner surface of the dyed blended fabric; the antibacterial and stain-resistant powder is dispersed in dimethyl carbonate under the bonding and adhesion effect of polyvinylidene fluoride resin and the film-forming and solubilizing effect of polyvinyl pyrrolidone. Due to the wear resistance, impact resistance and high toughness of polyvinylidene fluoride resin itself, the antibacterial and stain-resistant powder is dispersed therein, and then coated and dried to obtain a hydrophobic, oil-repellent, wear-resistant and impact-resistant waterproof and stain-resistant inner film.
[0020] Furthermore, the preparation method of the antibacterial and stain-resistant finishing agent comprises the following steps:
[0021] Step S1, epichlorohydrin, perfluorotripropylamine hydrochloride and anhydrous ethanol are added to a three-necked flask in sequence, the temperature is raised to 85-95° C. under nitrogen protection, the mixture is kept under reflux and stirred for reaction for 26-32 hours, the anhydrous ethanol is removed by concentration under reduced pressure, the mixture is recrystallized with a mixed solvent of ethyl acetate and petroleum ether, and the pH is adjusted to 8 with a 10-15wt% sodium hydroxide solution to obtain an intermediate a;
[0022] Step S2, treating the multi-walled carbon nanotubes with nitric acid vapor, washing with anhydrous ethanol until neutral, and vacuum drying to obtain oxidized multi-walled carbon nanotubes;
[0023] Step S3, ultrasonically disperse the oxidized multi-walled carbon nanotubes in deionized water, add intermediate a and 20vt% triethylamine solution, heat to 75-85°C under nitrogen protection, keep warm and stir for 18-22 hours, wash and filter with acetone, and dry to obtain an antibacterial and stain-resistant powder, and mix the antibacterial and stain-resistant powder with 3-5 times its mass of water to obtain an antibacterial and stain-resistant finishing agent.
[0024] The synthetic reaction principle of antibacterial and stain-resistant finishing agent is as follows:
[0025]
[0026] Among them, MWNTs are multi-walled carbon nanotubes.
[0027] Furthermore, the molar ratio of epichlorohydrin to perfluorotripropylamine hydrochloride is 1:1.3-1.8, the amount of anhydrous ethanol used is 5-10 times the mass of epichlorohydrin, the volume ratio of ethyl acetate to petroleum ether in the mixed solvent is 1:5, the recrystallization temperature is -5-5°C; the mass ratio of intermediate a to oxidized multi-walled carbon nanotubes and triethylamine solution is 6-10:0.3-0.8:8-15.
[0028] Furthermore, the diameter of the opening roller of the opening machine is 400 mm, and the rotation speed is 900 r / min; the diameter of the evenly-haired roller of the opening machine is 300 mm.
[0029] Furthermore, phosphoric acid cleaning uses a phosphoric acid solution with a concentration of 15 to 30 wt%, a cleaning time of 10 to 30 min, and a cleaning temperature of 65 to 80° C.; potassium hydroxide cleaning uses a potassium hydroxide solution with a concentration of 8 to 15 wt%, a cleaning time of 10 to 20 min, and a cleaning temperature of 45 to 60° C.
[0030] Furthermore, the decolorizing solution is mixed by the following components by weight: 8 to 15 parts of 1-aminoethyl-2-heptadecylimidazolium hydrochloride, 6 to 13 parts of sodium aluminate, 3 to 10 parts of polyvinyl alcohol, 4 to 8 parts of ammonium chloride and 30 to 55 parts of water; the sterilizing solution is mixed by the following components by weight: 13 to 25 parts of carboxymethyl chitosan, 10 to 18 parts of monostearate glyceryl and 35 to 57 parts of water.
[0031] Furthermore, the seaweed fiber has a length of 40 mm and a fineness of 1.67 dtex; the warp density of the blended base fabric is 125 to 138 strands / cm, and the weft density is 85 to 96 strands / cm.
[0032] Furthermore, the preparation method of the waterproof and stain-resistant film material is as follows: according to weight, 0.6 to 1.8 parts of antibacterial and stain-resistant powder are mixed with 15 to 32 parts of polyvinylidene fluoride resin, 1 to 5 parts of polyvinyl pyrrolidone, and 45 to 70 parts of dimethyl carbonate, ultrasonically dispersed for 20 to 30 minutes, heated to 78 to 90° C., stirred and kept warm for 10 to 12 hours, and vacuum degassing is performed.
[0033] The present invention has the following beneficial effects:
[0034] 1. The method for preparing a handbag of the present invention comprises the steps of crushing and loosening, cleaning and removing impurities, decolorizing and sterilizing, sorting and blending, antibacterial and stain-resistant finishing, dyeing and fixing, cutting and casting, and handle installation. After crushing and loosening, cleaning and removing impurities, decolorizing and sterilizing are performed to completely remove impurities and bacteria in the gaps and inner surfaces of waste fiber cloths. Seaweed fiber is added during sorting and blending to improve the antibacterial and mildew-proof properties of the blended base cloth. During the antibacterial and stain-resistant finishing, a hydrophobic and oleophobic, self-cleaning, and high-strength film is formed on the surface of the blended base cloth. During the cutting and casting, a hydrophobic and oleophobic, wear-resistant, impact-resistant, waterproof and stain-resistant inner film is formed on the inner surface of the dyed blended cloth. The prepared handbag product is antibacterial and stain-resistant and has a long service life.
[0035] 2. When preparing the antibacterial and stain-resistant finishing agent, the raw material perfluorotripropylamine hydrochloride has multiple fluorine-carbon bonds, good stability and extremely low surface energy; multi-walled carbon nanotubes have excellent physical and mechanical properties, and the carboxyl groups on the surface after oxidation increase the reaction activity; the antibacterial and stain-resistant powder grafted with quaternary ammonium salt enters the blended base fabric under the dispersion effect of water, and forms a hydrophobic, oleophobic, self-cleaning, high-strength film after drying, which has excellent waterproof and stain-resistant effects.
[0036] 3. In the cutting and casting step, the antibacterial and stain-resistant powder is dispersed in dimethyl carbonate under the adhesive adhesion of polyvinylidene fluoride resin and the film-forming and solubilizing effect of polyvinyl pyrrolidone. Due to the wear resistance, impact resistance and high toughness of polyvinylidene fluoride resin itself, the antibacterial and stain-resistant powder is dispersed therein, and then coated and dried to obtain a hydrophobic, oil-resistant, wear-resistant and impact-resistant waterproof and stain-resistant inner film. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] This embodiment provides a method for regenerating waste fiber cloth to prepare an antibacterial and stain-resistant handbag, comprising the following steps:
[0040] Crushing and opening: Select waste cotton fiber and polyester fiber blended fiber cloth, crush it to a length and width of 1.5 cm, pass it into the opening machine for opening and combing, remove magnetic impurities to obtain opened mixed fiber; wherein, the opening roller of the opening machine has a diameter of 400 mm and a rotation speed of 900 r / min; the diameter of the even hair roller of the opening machine is 300 mm;
[0041] Cleaning and removing impurities: the opened mixed fiber is sequentially cleaned and filtered with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide, and then air-dried to obtain the impurity-removed mixed fiber; wherein, the phosphoric acid cleaning adopts a phosphoric acid solution with a concentration of 22wt%, the cleaning time is 17min, and the cleaning temperature is 76°C; the potassium hydroxide cleaning adopts a potassium hydroxide solution with a concentration of 10wt%, the cleaning time is 15min, and the cleaning temperature is 53°C;
[0042] Decolorization and sterilization: immerse the impurity-removed mixed fiber in a decolorization solution at 67°C, decolorize for 46 minutes, rinse with clean water, dry, immerse in a sterilization solution at 48°C, sterilize for 55 minutes, rinse with clean water, and dry to obtain a sterilized mixed fiber; wherein the decolorization solution is a mixture of the following components by weight: 12g 1-aminoethyl-2-heptadecylimidazolidine hydrochloride, 9g sodium aluminate, 7g polyvinyl alcohol, 6g ammonium chloride and 42g water; the sterilization solution is a mixture of the following components by weight: 16g carboxymethyl chitosan, 13g glyceryl monostearate and 53g water;
[0043] Sorting and blending: feeding the sterilized mixed fiber into a fiber sorting machine, and sorting the cotton fiber and the polyester fiber according to the different densities to obtain the regenerated cotton fiber and the regenerated polyester fiber; weighing 65% of the regenerated polyester fiber, 20% of the regenerated cotton fiber and 15% of the seaweed fiber according to the weight percentage, spinning and weaving to obtain the blended base fabric; wherein the seaweed fiber has a length of 40 mm and a fineness of 1.67 dtex; the warp density of the blended base fabric is 130 strands / cm, and the weft density is 90 strands / cm;
[0044] Antibacterial and stain-resistant finishing: the blended base fabric is immersed in the antibacterial and stain-resistant finishing agent, immersed three times and dried three times to obtain the antibacterial and stain-resistant blended fabric;
[0045] The preparation method of the antibacterial and stain-resistant finishing agent comprises the following steps:
[0046] Step S1, 92.5g of epichlorohydrin, 892.1g of perfluorotripropylamine hydrochloride, and 647.5g of anhydrous ethanol are added to a three-necked flask in sequence, the temperature is raised to 88°C under nitrogen protection, the temperature is kept under reflux and stirred for reaction for 29 hours, the anhydrous ethanol is removed by vacuum concentration, and the anhydrous ethanol is recrystallized through a mixed solvent of ethyl acetate and petroleum ether, and the pH is adjusted to 8 with a 13wt% sodium hydroxide solution to obtain an intermediate a; wherein the volume ratio of ethyl acetate to petroleum ether in the mixed solvent is 1:5, and the recrystallization temperature is -3°C;
[0047] Step S2, treating the multi-walled carbon nanotubes with nitric acid vapor, washing with anhydrous ethanol until neutral, and vacuum drying to obtain oxidized multi-walled carbon nanotubes;
[0048] Step S3, ultrasonically dispersing 7.2 g of oxidized multi-walled carbon nanotubes in deionized water, adding 76 g of intermediate a and 126 g of 20 vt% triethylamine solution, heating to 79° C. under nitrogen protection, stirring for 20 hours, washing with acetone, filtering, and drying to obtain an antibacterial and stain-resistant powder, and mixing the antibacterial and stain-resistant powder with 3.8 times the mass of water to obtain an antibacterial and stain-resistant finishing agent;
[0049] Dyeing and color fixing: the antibacterial and stain-resistant blended fabric is dyed and fixed to obtain a dyed blended fabric;
[0050] Cutting and casting: After cutting the dyed blended fabric to the required size of the handbag, a waterproof and stain-resistant film is coated on its inner surface through a casting machine, and a waterproof and stain-resistant inner film is obtained after drying, and then a bag-making machine is used to make bags to obtain a semi-finished handbag; wherein, the preparation method of the waterproof and stain-resistant film is as follows: 0.9g of antibacterial and stain-resistant powder is mixed with 27g of polyvinylidene fluoride resin, 3g of polyvinyl pyrrolidone, and 63g of dimethyl carbonate, ultrasonically dispersed for 25 minutes, heated to 86°C, stirred for 10.5 hours, and vacuum degassed. The antibacterial and stain-resistant powder is the same as the antibacterial and stain-resistant powder in the preparation method of the antibacterial and stain-resistant finishing agent.
[0051] Handle installation: Sew or glue the non-woven fabric handle onto the semi-finished handbag to obtain the finished handbag.
[0052] Example 2
[0053] This embodiment provides a method for regenerating waste fiber cloth to prepare an antibacterial and stain-resistant handbag, comprising the following steps:
[0054] Crushing and opening: Select waste cotton fiber and polyester fiber blended fiber cloth, crush it to a length and width of 2.2 cm, pass it into the opening machine for opening and combing, remove magnetic impurities to obtain opened mixed fiber; wherein, the opening roller of the opening machine has a diameter of 400 mm and a rotation speed of 900 r / min; the diameter of the even hair roller of the opening machine is 300 mm;
[0055] Cleaning and removing impurities: the opened mixed fiber is sequentially cleaned and filtered with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide, and then air-dried to obtain the impurity-removed mixed fiber; wherein, the phosphoric acid cleaning adopts a phosphoric acid solution with a concentration of 18wt%, the cleaning time is 30min, and the cleaning temperature is 78°C; the potassium hydroxide cleaning adopts a potassium hydroxide solution with a concentration of 14wt%, the cleaning time is 12min, and the cleaning temperature is 58°C;
[0056] Decolorization and sterilization: immerse the impurity-removed mixed fiber in a decolorization solution at 70°C, decolorize for 48 minutes, rinse with clean water, dry, immerse in a sterilization solution at 52°C, sterilize for 55 minutes, rinse with clean water, and dry to obtain a sterilized mixed fiber; wherein the decolorization solution is a mixture of the following components by weight: 10g 1-aminoethyl-2-heptadecylimidazolidine hydrochloride, 9g sodium aluminate, 7g polyvinyl alcohol, 6g ammonium chloride and 45g water; the sterilization solution is a mixture of the following components by weight: 21g carboxymethyl chitosan, 15g glyceryl monostearate and 47g water;
[0057] Sorting and blending: feeding the sterilized mixed fiber into a fiber sorting machine, and sorting the cotton fiber and the polyester fiber according to the different densities to obtain the regenerated cotton fiber and the regenerated polyester fiber; weighing 65% of the regenerated polyester fiber, 20% of the regenerated cotton fiber and 15% of the seaweed fiber according to the weight percentage, spinning and weaving to obtain the blended base fabric; wherein the seaweed fiber has a length of 40 mm and a fineness of 1.67 dtex; the warp density of the blended base fabric is 132 strands / cm, and the weft density is 93 strands / cm;
[0058] Antibacterial and stain-resistant finishing: the blended base fabric is immersed in the antibacterial and stain-resistant finishing agent, immersed three times and dried three times to obtain the antibacterial and stain-resistant blended fabric;
[0059] The preparation method of the antibacterial and stain-resistant finishing agent comprises the following steps:
[0060] Step S1, 92.5g of epichlorohydrin, 919.9g of perfluorotripropylamine hydrochloride, and 740g of anhydrous ethanol are added to a three-necked flask in sequence, the temperature is raised to 92°C under nitrogen protection, the temperature is kept under reflux and stirred for reaction for 31 hours, the anhydrous ethanol is removed by vacuum concentration, and the anhydrous ethanol is recrystallized through a mixed solvent of ethyl acetate and petroleum ether, and the pH is adjusted to 8 with a 12wt% sodium hydroxide solution to obtain an intermediate a; wherein the volume ratio of ethyl acetate to petroleum ether in the mixed solvent is 1:5, and the recrystallization temperature is 4°C;
[0061] Step S2, treating the multi-walled carbon nanotubes with nitric acid vapor, washing with anhydrous ethanol until neutral, and vacuum drying to obtain oxidized multi-walled carbon nanotubes;
[0062] Step S3, ultrasonically dispersing 5.5 g of oxidized multi-walled carbon nanotubes in deionized water, adding 82 g of intermediate a and 135 g of 20 vt% triethylamine solution, heating to 84° C. under nitrogen protection, keeping warm and stirring for 19 hours, washing with acetone, filtering, and drying to obtain an antibacterial and stain-resistant powder, and mixing the antibacterial and stain-resistant powder with 4.5 times the mass of water to obtain an antibacterial and stain-resistant finishing agent;
[0063] Dyeing and color fixing: the antibacterial and stain-resistant blended fabric is dyed and fixed to obtain a dyed blended fabric;
[0064] Cutting and casting: After cutting the dyed blended fabric to the required size of the handbag, a waterproof and stain-resistant film is coated on its inner surface through a casting machine, and a waterproof and stain-resistant inner film is obtained after drying, and then a bag-making machine is used to make bags to obtain a semi-finished handbag; wherein, the preparation method of the waterproof and stain-resistant film is as follows: 1.5g of antibacterial and stain-resistant powder is mixed with 19g of polyvinylidene fluoride resin, 2g of polyvinyl pyrrolidone, and 55g of dimethyl carbonate, ultrasonically dispersed for 27 minutes, heated to 86°C, stirred for 11.5 hours, and vacuum degassed. The antibacterial and stain-resistant powder is the same as the antibacterial and stain-resistant powder in the preparation method of the antibacterial and stain-resistant finishing agent.
[0065] Handle installation: Sew or glue the non-woven fabric handle onto the semi-finished handbag to obtain the finished handbag.
[0066] Example 3
[0067] This embodiment provides a method for regenerating waste fiber cloth to prepare an antibacterial and stain-resistant handbag, comprising the following steps:
[0068] Crushing and opening: Select waste cotton fiber and polyester fiber blended fiber cloth, crush it to a length and width of 2.6 cm, pass it into the opening machine for opening and combing, remove magnetic impurities to obtain opened mixed fiber; wherein, the opening roller of the opening machine has a diameter of 400 mm and a rotation speed of 900 r / min; the diameter of the even hair roller of the opening machine is 300 mm;
[0069] Cleaning and removing impurities: the opened mixed fiber is sequentially cleaned and filtered with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide, and then air-dried to obtain the impurity-removed mixed fiber; wherein, the phosphoric acid cleaning adopts a phosphoric acid solution with a concentration of 28wt%, the cleaning time is 28min, and the cleaning temperature is 78°C; the potassium hydroxide cleaning adopts a potassium hydroxide solution with a concentration of 14wt%, the cleaning time is 20min, and the cleaning temperature is 58°C;
[0070] Decolorization and sterilization: immerse the impurity-removed mixed fiber in a decolorization solution at 72°C, decolorize for 50 minutes, rinse with clean water, dry, immerse in a sterilization solution at 52°C, sterilize for 58 minutes, rinse with clean water, and dry to obtain a sterilized mixed fiber; wherein the decolorization solution is a mixture of the following components by weight: 15g 1-aminoethyl-2-heptadecylimidazolidine hydrochloride, 11g sodium aluminate, 5g polyvinyl alcohol, 6g ammonium chloride and 48g water; the sterilization solution is a mixture of the following components by weight: 24g carboxymethyl chitosan, 16g glyceryl monostearate and 56g water;
[0071] Sorting and blending: feeding the sterilized mixed fiber into a fiber sorting machine, and sorting the cotton fiber and the polyester fiber according to the different densities to obtain the regenerated cotton fiber and the regenerated polyester fiber; weighing 65% of the regenerated polyester fiber, 20% of the regenerated cotton fiber and 15% of the seaweed fiber according to the weight percentage, spinning and weaving to obtain the blended base fabric; wherein the seaweed fiber has a length of 40 mm and a fineness of 1.67 dtex; the warp density of the blended base fabric is 126 strands / cm, and the weft density is 88 strands / cm;
[0072] Antibacterial and stain-resistant finishing: the blended base fabric is immersed in the antibacterial and stain-resistant finishing agent, immersed three times and dried three times to obtain the antibacterial and stain-resistant blended fabric;
[0073] The preparation method of the antibacterial and stain-resistant finishing agent comprises the following steps:
[0074] Step S1, 92.5g of epichlorohydrin, 958.9g of perfluorotripropylamine hydrochloride, and 786.3g of anhydrous ethanol are added to a three-necked flask in sequence, the temperature is raised to 95°C under nitrogen protection, the temperature is kept under reflux and stirred for reaction for 31 hours, the anhydrous ethanol is removed by vacuum concentration, and the anhydrous ethanol is recrystallized through a mixed solvent of ethyl acetate and petroleum ether, and the pH is adjusted to 8 with a 14wt% sodium hydroxide solution to obtain an intermediate a; wherein the volume ratio of ethyl acetate to petroleum ether in the mixed solvent is 1:5, and the recrystallization temperature is 5°C;
[0075] Step S2, treating the multi-walled carbon nanotubes with nitric acid vapor, washing with anhydrous ethanol until neutral, and vacuum drying to obtain oxidized multi-walled carbon nanotubes;
[0076] Step S3, ultrasonically dispersing 5.7 g of oxidized multi-walled carbon nanotubes in deionized water, adding 92 g of intermediate a and 108 g of 20 vt% triethylamine solution, heating to 84° C. under nitrogen protection, stirring at this temperature for 21.5 hours, washing with acetone, filtering, and drying to obtain an antibacterial and stain-resistant powder, and mixing the antibacterial and stain-resistant powder with 3 to 5 times the mass of water to obtain an antibacterial and stain-resistant finishing agent;
[0077] Dyeing and color fixing: the antibacterial and stain-resistant blended fabric is dyed and fixed to obtain a dyed blended fabric;
[0078] Cutting and casting: After cutting the dyed blended fabric to the required size of the handbag, a waterproof and stain-resistant film is coated on its inner surface through a casting machine, and a waterproof and stain-resistant inner film is obtained after drying, and then a bag-making machine is used to make bags to obtain a semi-finished handbag; wherein, the preparation method of the waterproof and stain-resistant film is as follows: 1.2g of antibacterial and stain-resistant powder is mixed with 26g of polyvinylidene fluoride resin, 4.2g of polyvinyl pyrrolidone, and 60g of dimethyl carbonate, ultrasonically dispersed for 30 minutes, heated to 87°C, stirred for 12 hours, and vacuum degassed. The antibacterial and stain-resistant powder is the same as the antibacterial and stain-resistant powder in the preparation method of the antibacterial and stain-resistant finishing agent.
[0079] Handle installation: Sew or glue the non-woven fabric handle onto the semi-finished handbag to obtain the finished handbag.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 1 is that the decolorization and sterilization step is eliminated.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 1 is that in the sorting and blending step, 75% of the regenerated polyester fiber and 25% of the regenerated cotton fiber are spun and woven to obtain the blended base fabric.
[0084] Comparative Example 3
[0085] The difference between this comparative example and Example 1 is that the antibacterial and stain-resistant finishing step is eliminated.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 1 is that in the cutting and casting step, the inner surface is not coated with a waterproof and anti-fouling film material by a casting machine.
[0088] Performance Testing
[0089] The finished handbags prepared in Examples 1-3 and Comparative Examples 1-4 were cut into samples of 2cm*2cm in size, and the surface dynamic contact angle, antibacterial rate, and stain resistance were tested; the surface water static contact angle was measured by the droplet method to measure the surface water static contact angle of the inner surface of the sample, the antibacterial rate was measured by the plate coating method to measure the average of the three antibacterial rates of Escherichia coli and Staphylococcus aureus, and the stain resistance was measured according to the standard AATCC130:2010 "Test Method for Easily Decontamination Performance of Textiles" to measure the initial stain resistance and stain resistance after 50 washes. The specific test results are shown in the following table:
[0090]
[0091] As can be seen from the above table, the surface dynamic contact angle of the handbag prepared in the embodiment of the present invention is about 90°, indicating that the hydrophilic and hydrophobic properties of the outer surface of the handbag are moderate; the antibacterial rates against Escherichia coli and Staphylococcus aureus are better than those of the control example, and the initial stain resistance and stain resistance after 50 washings are excellent, indicating that the handbag prepared from the waste fiber cloth of the present invention is antibacterial and stain-resistant and has a long service life. In Comparative Example 1, since the decolorization and sterilization steps were eliminated, it was impossible to remove the pigment components and kill the bacteria and viruses in the mixed fibers before blending, resulting in reduced antibacterial and stain resistance. In Comparative Example 2, since seaweed fiber was not added for blending, the antibacterial, mildew-proof and flame-retardant properties of seaweed fiber could not be brought into play, resulting in a decrease in antibacterial performance. In Comparative Example 3, since the antibacterial and stain-resistant finishing step was eliminated, a hydrophobic, oleophobic, self-cleaning and high-strength film could not be formed, and the stain resistance was significantly reduced. In Comparative Example 4, since the waterproof and stain-resistant film material was not coated on the inner surface by a casting machine, a hydrophobic, oleophobic, wear-resistant and impact-resistant waterproof and stain-resistant inner film could not be obtained, and the hydrophobic and stain-resistant properties were significantly reduced.
[0092] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0093] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing antibacterial and stain-resistant handbags by regenerating waste fiber cloth, characterized in that: The following steps are involved: Crushing and opening: Select waste cotton fiber and polyester fiber blended fiber cloth, crush it to a length and width of 1 to 3 cm, pass it into the opening machine for opening and combing, remove magnetic impurities to obtain opened mixed fiber; Cleaning and removing impurities: the opened mixed fiber is sequentially cleaned and filtered with distilled water, ethanol, acetone, phosphoric acid, and potassium hydroxide, and then dried to obtain the impurity-removed mixed fiber; Decolorization and sterilization: immerse the impurity-removed mixed fiber in a decolorization solution at 60-72°C for 30-50 minutes, rinse with clean water, dry, immerse in a sterilization solution at 40-55°C for 45-60 minutes, rinse with clean water, and dry to obtain the sterilized mixed fiber; Sorting and blending: feeding the sterilized mixed fiber into a fiber sorting machine, and sorting the cotton fiber and the polyester fiber according to the different densities to obtain the regenerated cotton fiber and the regenerated polyester fiber; weighing 65% of the regenerated polyester fiber, 20% of the regenerated cotton fiber and 15% of the seaweed fiber according to the weight percentage, spinning and weaving to obtain the blended base fabric; Antibacterial and stain-resistant finishing: the blended base fabric is immersed in the antibacterial and stain-resistant finishing agent, immersed three times and dried three times to obtain the antibacterial and stain-resistant blended fabric; Dyeing and color fixing: the antibacterial and stain-resistant blended fabric is dyed and fixed to obtain a dyed blended fabric; Cutting and casting: After the dyed blended fabric is cut to the required size of the handbag, a waterproof and stain-resistant film material is coated on its inner surface through a casting machine, and a waterproof and stain-resistant inner film is obtained after drying, and then a bag-making machine is used to make bags to obtain the semi-finished handbags; Handle installation: sew or glue the non-woven fabric handle onto the semi-finished handbag to obtain the finished handbag; The preparation method of the antibacterial and stain-resistant finishing agent comprises the following steps: Step S1, epichlorohydrin, perfluorotripropylamine hydrochloride and anhydrous ethanol are added to a three-necked flask in sequence, the temperature is raised to 85-95° C. under nitrogen protection, the mixture is kept under reflux and stirred for reaction for 26-32 hours, the anhydrous ethanol is removed by concentration under reduced pressure, the mixture is recrystallized with a mixed solvent of ethyl acetate and petroleum ether, and the pH is adjusted to 8 with a 10-15wt% sodium hydroxide solution to obtain an intermediate a; Step S2, treating the multi-walled carbon nanotubes with nitric acid vapor, washing with anhydrous ethanol until neutral, and vacuum drying to obtain oxidized multi-walled carbon nanotubes; Step S3, ultrasonically dispersing the oxidized multi-walled carbon nanotubes in deionized water, adding intermediate a and 20vt% triethylamine solution, heating to 75-85°C under nitrogen protection, keeping warm and stirring for 18-22 hours, washing with acetone, filtering, and drying to obtain an antibacterial and stain-resistant powder, and mixing the antibacterial and stain-resistant powder with water of 3-5 times its mass to obtain an antibacterial and stain-resistant finishing agent; The molar ratio of epichlorohydrin to perfluorotripropylamine hydrochloride is 1:1.3-1.8, the amount of anhydrous ethanol used is 5-10 times the mass of epichlorohydrin, the volume ratio of ethyl acetate to petroleum ether in the mixed solvent is 1:5, and the recrystallization temperature is -5-5°C; the mass ratio of intermediate a to oxidized multi-walled carbon nanotubes and triethylamine solution is 6-10:0.3-0.8:8-15; The diameter of the opening roller of the opening machine is 400mm, and the rotation speed is 900r / min; the diameter of the hair leveling roller of the opening machine is 300mm; When phosphoric acid is used for cleaning, a phosphoric acid solution with a concentration of 15 to 30 wt% is used, the cleaning time is 10 to 30 minutes, and the cleaning temperature is 65 to 80° C.; when potassium hydroxide is used for cleaning, a potassium hydroxide solution with a concentration of 8 to 15 wt% is used, the cleaning time is 10 to 20 minutes, and the cleaning temperature is 45 to 60° C.; The decolorizing solution is prepared by mixing the following components by weight: 8 to 15 parts of 1-aminoethyl-2-heptadecylimidazolium hydrochloride, 6 to 13 parts of sodium aluminate, 3 to 10 parts of polyvinyl alcohol, 4 to 8 parts of ammonium chloride and 30 to 55 parts of water; the sterilizing solution is prepared by mixing the following components by weight: 13 to 25 parts of carboxymethyl chitosan, 10 to 18 parts of glyceryl monostearate and 35 to 57 parts of water; The seaweed fiber has a length of 40 mm and a fineness of 1.67 dtex; the warp density of the blended base fabric is 125 to 138 strands / cm, and the weft density is 85 to 96 strands / cm; The preparation method of the waterproof and stain-resistant film material is as follows: according to weight, 0.6 to 1.8 parts of antibacterial and stain-resistant powder are mixed with 15 to 32 parts of polyvinylidene fluoride resin, 1 to 5 parts of polyvinyl pyrrolidone, and 45 to 70 parts of dimethyl carbonate, ultrasonically dispersed for 20 to 30 minutes, heated to 78 to 90° C., stirred for 10 to 12 hours, and vacuum degassed.