A method for manufacturing an axially-lead organic polymer tantalum fixed capacitor

Through the manufacturing method of axially drawing organic polymer tantalum fixed capacitors, using vacuum impregnation PEDOT solution and dense electrolyte layer, the problem of unstable electrical performance of traditional tantalum capacitors in high frequencies and complex environments has been solved, and high-frequency performance improvement and Security enhancements.

CN115223798BActive Publication Date: 2024-10-11CHANG CHUN WEI HONG DONG GUANG DIAN ZI QI CAI YOU XIAN GONG SI

Patent Information

Application Number
CN202210905178.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-10-11
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

The electrical performance of existing tantalum capacitors is unstable under high frequencies and complex environments. Traditional manganese dioxide electrolytes have combustion risks and low conductivity, resulting in poor frequency tolerance characteristics.

Method used

The axially drawn organic polymer tantalum fixed capacitor manufacturing method is used to form a polymer electrolyte layer by vacuum impregnating the PEDOT solution, solidifying it at high temperature, and combining the graphite and silver paste layers to form a dense capacitor structure.

Benefits of technology

It improves high-frequency performance, avoids the risk of combustion, enhances the stability and capacity retention of the capacitor, has self-healing capabilities and high-frequency filtering performance, and is environmentally friendly and efficient in production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115223798B_ABST
    Figure CN115223798B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of capacitor manufacturing, and mainly comprises the following steps: pressing an anode embryo; calcining the anode embryo to form an anode body; energizing the anode body, and using a vacuum impregnation tank to impregnate the anode body with a polymer solution to form a polymer layer; first coating the polymer layer with a graphite layer, and then coating the silver paste layer to form a semi-finished product, assembling the semi-finished product to form a finished product, and aging and screening the finished product; the axially lead organic polymer tantalum fixed capacitor produced by the method has the advantages of good high-frequency performance, high safety, resistance to large ripple and surge current impact, strong self-repairing ability, high voltage, large capacity, avoidance of secondary damage to the oxide film, low leakage current, high production efficiency, environmental protection, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of capacitor manufacturing, and in particular relates to a method for manufacturing an axially-leaded organic polymer tantalum fixed capacitor. Background Art

[0002] The progress of electronic technology in today's society has accelerated the development of the tantalum capacitor industry and the pace of continuous technological breakthroughs. Tantalum capacitors are not only used in the aerospace field, but also in a large number of high-precision military electronic equipment in the fields of ships, weapons, etc. With the large-scale application of low-impedance and high-frequency circuits, higher requirements are placed on tantalum capacitors. Solid electrolyte tantalum capacitors have the characteristics of low ESR (ESR is Equivalent Series Resistance), low loss tangent, high stability, long service life, and high reliability. Therefore, they are widely used in the whole machine circuit.

[0003] At present, solid electrolyte tantalum capacitors with manganese dioxide as electrolyte need to be decomposed at high temperature during the manufacturing process. The gas released after thermal decomposition is not environmentally friendly, and high temperature can easily cause damage to the dielectric film. This affects the electrical properties of the capacitor. MnO2 has a high oxygen content. When there are defects in the dielectric layer, it is easy to cause combustion under the action of an applied voltage. In addition, manganese dioxide has low conductivity as an electrolyte and poor frequency-to-capacity characteristics. As the frequency continues to increase, the capacity decay is serious. For this reason, the market has become the mainstream of development with polymer conductive polymer materials referred to as PEDOT as electrolytes. Polymer conductive polymer materials are a new generation of conductive polymers developed by German scientists in the mid-to-late 1980s. PEDOT not only has a high conductivity (about 300s / era), but also has a high stability in an oxidized state. At present, most of the chip tantalum capacitors that use polymer conductive polymers as electrolytes on the market are small-sized, limited in capacity, and are resin-encapsulated. If the package is placed in the air for a long time, the electrical performance parameters will be affected by moisture. Summary of the invention

[0004] The main purpose of the present invention is to solve the shortcomings of tantalum capacitors with polymers as electrolytes on the market and the performance problems of traditional manganese dioxide as electrolytes. Combining the polymerization characteristics of high conductivity of polymer materials, a manufacturing method for axially leading organic polymer tantalum fixed capacitors is proposed to make the electrical properties (including capacity, leakage current, ESR and loss) very stable under various complex environments, and the organic polymer tantalum fixed capacitors manufactured by the present invention have the advantages of high voltage resistance and the like.

[0005] The technical solution of the present invention is:

[0006] A method for manufacturing an axially-lead organic polymer tantalum fixed capacitor, characterized by comprising the following steps:

[0007] Step 1: Put tantalum powder and tantalum wire into the mold cavity, and use a molding machine to apply pressure to the tantalum powder in the mold cavity to form an anode blank with a tantalum core;

[0008] Step 2: placing the pressed anode body into a sintering furnace for calcining to form an anode body with a microscopic porous structure;

[0009] Step 3: Use a spot welder to weld the tantalum core of the anode body to the steel bar to form a group, and place the steel bar on the process frame, and use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body;

[0010] Step 4: using a vacuum impregnation tank to carry a polymer material solution, and at a pressure of (-60 to -80 kPa) ± 2 kPa, impregnating the oxide film anode body formed in step 3, wherein the polymer material solution is a PEDOT solution, the solid content of which is 0.8% to 9%, and the viscosity is 1000 to 2500 mPa.S; the vacuum impregnation tank automatically descends and rises at a speed of 0.01 to 0.03 mm / s, and the impregnation time is 10 min to 15 min;

[0011] Step 5: Dry the impregnated anode body at room temperature for 5 to 8 minutes, then perform high temperature curing, raise the temperature to 125°C, and maintain the constant temperature for 10 to 15 minutes after reaching the target temperature;

[0012] Step 6: Repeat the process of step 4 to step 5 12 to 25 times according to the specifications of the capacitor to form a polymer layer on the surface of the oxide film of the anode body;

[0013] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the constant temperature is maintained for 30min±3min, and then the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0014] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0015] Step 9: Screen the finished products in step 8 and eliminate unqualified products.

[0016] Further, the process of energizing the anode body by an electrochemical method described in step three is to place the anode body in an energizing liquid at 80°C, and apply a constant energizing voltage of 24V to 320V according to the specifications of the capacitor for 240 minutes; the selection of the energizing liquid is related to the energizing voltage. When the energizing voltage is <80V, the energizing liquid is selected as a 0.1% HNO3 solution; when 80V≤energizing voltage<180V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 20% ethylene glycol; when 180V≤energizing voltage<300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 50% ethylene glycol; when the energizing voltage is ≥300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 75% ethylene glycol.

[0017] Furthermore, when the process of step 4-step 5 is repeated in step 6, the solid content of the polymer material solution in step 4 needs to be measured before each specification product is impregnated. If the conditions are not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured.

[0018] Furthermore, the method for determining the viscosity of the polymer solution is as follows: pour the polymer material solution into a 1000mL beaker, adjust the viscometer to a horizontal position, select a rotor with a range of 0 to 25000mPa·S, select a speed of 120r / min, ensure that the solution must be submerged in the scale specified on the rotor, start the viscometer host, start measuring, and after the value stabilizes, record the read data, then press the reset button, measure three sets of data and take the average value, which is the viscosity value of the solution.

[0019] Furthermore, in step 1, camphor powder is uniformly mixed in the tantalum powder, and the mass of the camphor powder is 3% of the mass of the tantalum powder.

[0020] Furthermore, the aging process in step nine is to apply an aging voltage of 1.1 to 1.2 times of the rated voltage to the finished axially lead organic polymer tantalum fixed capacitor.

[0021] Furthermore, the high temperature curing process in step five is to increase the temperature from room temperature to 55°C, maintain for 6 minutes, then increase the temperature to 85°C, maintain for 1 minute, then increase the temperature to 105°C, maintain for 3 minutes, and finally increase the temperature to 125°C and maintain for 10 to 15 minutes according to the process.

[0022] The present invention using the above technical solution can bring the following beneficial effects:

[0023] 1. High frequency performance advantage

[0024] The polymer material has a conductivity several dozen times higher than that of traditional MnO2, and forms a polymer electrolyte on the tantalum core of the solid tantalum capacitor. The high-frequency performance is improved by the manufacturing method of the present invention. The traditional manganese dioxide solid electrolyte tantalum capacitor will lose more than half of its capacity at a frequency of 100KHZ, and the polymer tantalum capacitor on the market as an electrolyte will lose more than 80% of its capacity at a frequency of 100KHZ, while the axial organic polymer tantalum fixed capacitor will retain at least 95% of its capacity at a frequency of 100KHZ. The small sudden drop in capacitance below the frequency of 100KHZ improves the circuit filtering performance of the capacitor in the frequency range of the DC-DC conversion circuit.

[0025] 2. High security

[0026] When the organic polymer tantalum fixed capacitor fails, the cathode polymer undergoes an oxygen absorption reaction, isolating the anode tantalum powder from oxygen. Even if the product fails, it will not burn, and is safe.

[0027] 3. Withstand large ripple and surge current impact

[0028] The organic polymer tantalum fixed capacitor manufactured according to the method of the present invention has high capacitance and small loss tangent in the high frequency range and can accommodate a larger ripple current.

[0029] 4. Strong self-repair ability

[0030] The polymer electrolyte layer manufactured by the manufacturing method of the present invention has a denser molecular gap of micron level than that manufactured by the prior art. When the capacitor is damaged, the current will converge at the defective position, and local overheating will cause the polymer at the defective position to vaporize and repair the defect.

[0031] 5. High voltage and large capacity

[0032] The polymer impregnation work in the vacuum impregnation equipment breaks the tension between molecules, and more molecules can be brought in under the vacuum state. In addition, the product invented in combination with the manufacturing method has better capacity extraction as electrolyte, dense membrane layer and high pressure resistance than organic polymer materials on the market.

[0033] 6. Avoid secondary damage to the oxide film and reduce leakage current

[0034] The temperature of the entire process of manufacturing polymer as electrolyte does not exceed 150°C, which prevents the oxide film from being damaged by exceeding the tolerable temperature range and improves the leakage current level.

[0035] 7. High production efficiency and environmental protection

[0036] The entire manufacturing process of the present invention has no environmental pollution. The most important thing is that the polymer used as the electrolyte manufacturing process adopts physical polymerization. Compared with the chemical polymerization method on the market, the whole process has no residues to be cleaned, the operation is simple, the production efficiency is high, and there is no chemical product, which is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A schematic diagram of the structure of an axially-lead organic polymer tantalum fixed capacitor manufactured by the method of the present invention;

[0038] Figure 2 It is a process flow chart of the present invention;

[0039] Figure 3 It is a curing temperature-time curve diagram of the present invention.

[0040] In the figure, 1-anode lead, 2-tantalum wire, 3-copper shell, 4-tantalum core, 5-solder, 6-Ta2O5 oxide film, 7-high molecular polymer layer, 8-graphite layer, 9-silver paste layer, and 10-cathode lead. DETAILED DESCRIPTION

[0041] like Figure 2 As shown, a method for manufacturing an axially-lead organic polymer tantalum fixed capacitor is characterized by comprising the following steps:

[0042] Step 1: Put tantalum powder and tantalum wire into the mold cavity, and use a molding machine to apply pressure to the tantalum powder in the mold cavity to form an anode blank with a tantalum core;

[0043] Step 2: placing the pressed anode body into a sintering furnace for calcining to form an anode body with a microscopic porous structure;

[0044] Step 3: Use a spot welder to weld the tantalum core of the anode body to the steel bar to form a group, and place the steel bar on the process frame, and use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body;

[0045] Step 4: using a vacuum impregnation tank to carry a polymer material solution, and at a pressure of (-60 to -80 kPa) ± 2 kPa, impregnating the oxide film anode body formed in step 3, wherein the polymer material solution is a PEDOT solution, the solid content of which is 0.8% to 9%, and the viscosity is 1000 to 2500 mPa.S; the vacuum impregnation tank automatically descends and rises at a speed of 0.01 to 0.03 mm / s, and the impregnation time is 10 min to 15 min;

[0046] Step 5: Dry the impregnated anode body at room temperature for 5 to 8 minutes, then perform high temperature curing, raise the temperature to 125°C, and maintain the constant temperature for 10 to 15 minutes after reaching the target temperature;

[0047] Step 6: Repeat the process of step 4 to step 5 12 to 25 times according to the specifications of the capacitor to form a polymer layer on the surface of the oxide film of the anode body;

[0048] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the constant temperature is maintained for 30min±3min, and then the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0049] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0050] Step 9: Screen the finished products in step 8 and eliminate unqualified products.

[0051] Further, the process of energizing the anode body by an electrochemical method described in step three is to place the anode body in an energizing liquid at 80°C, and apply a constant energizing voltage of 24V to 320V according to the specifications of the capacitor for 240 minutes; the selection of the energizing liquid is related to the energizing voltage. When the energizing voltage is <80V, the energizing liquid is selected as a 0.1% HNO3 solution; when 80V≤energizing voltage<180V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 20% ethylene glycol; when 180V≤energizing voltage<300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 50% ethylene glycol; when the energizing voltage is ≥300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 75% ethylene glycol.

[0052] Further, when the process of step 4-step 5 is repeated in step 6, the solid content of the polymer material solution in step 4 needs to be measured before each specification product is impregnated. If the conditions are not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5-7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured. Further, the method for measuring the viscosity of the polymer solution is to pour the polymer material solution into a 1000mL beaker, adjust the viscometer to a horizontal position, select a rotor with a range of 0-25000mPa·S, and select a speed of 120r / min. It is necessary to ensure that the solution must not exceed the scale specified on the rotor, start the viscometer host, start measuring, and after the value stabilizes, record the read data, and then press the reset button to measure three sets of data and take the average value, which is the viscosity value of the solution.

[0053] Furthermore, in step 1, camphor powder is uniformly mixed in the tantalum powder, and the mass of the camphor powder is 3% of the mass of the tantalum powder.

[0054] Furthermore, the aging process in step nine is to apply an aging voltage of 1.1 to 1.2 times of the rated voltage to the finished axially lead organic polymer tantalum fixed capacitor.

[0055] Furthermore, the high temperature curing process in step 5 is to heat from room temperature to 55°C, hold for 6 minutes, then heat to 85°C, hold for 1 minute, then heat to 105°C, hold for 3 minutes, and finally heat to 125°C, hold for 10 to 15 minutes. Please refer to the temperature rise process Figure 3 The curing curve of the figure shows that the horizontal axis is time and the vertical axis is temperature. The room temperature is 25°C. Although the heating rate is fast and the physical polymerization speed will also be accelerated, as the curing temperature increases, the curing speed is accelerated, and larger particles are easily formed. On the one hand, the impregnation is reduced, so that there are still air bubbles inside the tantalum block; on the other hand, some side chains may be formed in the main chain of the polymer, thereby changing the conjugated structure of the main chain and reducing its own conductivity. Ultimately, it leads to an increase in the ESR and loss of the capacitor. According to the curing curve, the surface of the polymer electrolyte layer formed after the polymer is impregnated and cured can be dense and flat.

[0056] Example 1

[0057] The production specifications are: 16V, 680μF axial lead organic polymer tantalum fixed capacitor;

[0058] Step 1: 2251 mg of tantalum powder and 67.53 mg of camphor powder are uniformly mixed and placed in a mold cavity of Φ7 mm*9 mm in size, and a Φ0.6 mm tantalum wire is inserted into the center of the mixed powder for pressing, wherein the camphor powder is used as a binder to form an anode blank with a Φ0.6 mm tantalum wire core, which is then placed in a sintering furnace for calcination to form an anode body with a microporous structure;

[0059] Step 3: Use a spot welder to weld the tantalum core of the anode body to a steel bar, and place the steel bar on a process rack. Use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body. The specific process is to place the anode body in a 0.1% HNO3+20% ethylene glycol energizing solution at 80°C, apply a constant energizing voltage of 80V, and continue for 240 minutes;

[0060] Step 4: Use a vacuum impregnation tank to carry the PEDOT solution, and impregnate the oxide film anode body formed in step 3 under a vacuum state of -60kpa±2kpa, wherein the solid content of the PEDOT solution is 0.8-9%, and the viscosity value is 1500mPa.S; the vacuum impregnation tank is automatically lowered and raised at a speed of 0.03mm / s, and the impregnation time is 12min. During the manufacturing process, the polymer liquid level is required to be level, the overflow is consistent, there are no bubbles, no turbidity and any visible impurities. Since the uneven distribution of the particle size of each molecule immersed in the polymer material solution forms tension on the product surface, the vacuum negative pressure value and the impregnation automation parameters are set to allow each molecule to break through the tension formed on the product surface during the entire impregnation process and impregnate into the internal pores of the tantalum core;

[0061] Step 5: Dry the impregnated anode body at room temperature for 6 minutes, and then solidify the anode body after drying. Figure 3 The curing temperature curve in the figure is from room temperature to 55°C, kept for 6 minutes, then raised to 85°C, kept for 1 minute, then raised to 105°C, kept for 3 minutes, and finally raised to 125°C, kept for 10 minutes. The horizontal axis in the figure is time, the vertical axis is temperature, and the room temperature is 25°C.

[0062] Step 6: Repeat the process of step 4-step 5 22 times to form a polymer layer on the surface of the oxide film of the anode body. It should be noted that when repeating the process of step 4-step 6, the solid content of the polymer material solution in step 4 should be measured before each immersion of a product of a certain specification. If the condition is not met, the polymer material solution should be supplemented. After the solution is supplemented, the polymer solution should be stirred for 5 to 7 minutes with a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring should be measured until the fixed content reaches the set value;

[0063] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3℃; after the temperature rises from room temperature to the target temperature, the drying time is: 30±3min, and the timing starts when the target temperature is reached, and the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0064] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0065] Step 9: Apply 1.2 times the rated voltage to the finished product in step 8 for aging screening to eliminate unqualified products.

[0066] Table 1 below shows the loss, ESR, and leakage comparison of the 16V, 680uF axial lead organic polymer tantalum fixed capacitor manufactured by the method of Example 1, the existing polymer electrolyte capacitor of the same specification, and the chip tantalum polymer electrolyte capacitor of the same specification:

[0067]

[0068] Table 1

[0069] Example 2

[0070] The production specifications are: 4V, 5600μF axial lead organic polymer tantalum fixed capacitor;

[0071] Step 1: 4000 mg of tantalum powder and 120 mg of camphor powder are uniformly mixed and placed in a mold cavity of Φ7 mm*16 mm in size, and a Φ0.6 mm tantalum wire is inserted into the center of the mixed powder for pressing, wherein the camphor powder is used as a binder to form an anode blank with a Φ0.6 mm tantalum wire core, which is then placed in a sintering furnace for calcination to form an anode body with a microporous structure;

[0072] Step 3: Use a spot welder to weld the tantalum core of the anode body to a steel bar, and place the steel bar on a process rack. Use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body. The specific process is to place the anode body in a 0.1% HNO3 energizing solution at 80°C, apply a 13V energizing constant voltage, and continue for 240 minutes;

[0073] Step 4: Use a vacuum impregnation tank to carry the PEDOT solution, and impregnate the oxide film anode body formed in step 3 under a vacuum state of -60kpa±2kpa, wherein the solid content of the PEDOT solution is 0.8-9%, and the viscosity value is 1500mPa.S; the vacuum impregnation tank is automatically lowered and raised at a speed of 0.03mm / s, and the impregnation time is 15min. During the manufacturing process, the polymer liquid level is required to be level, the overflow is consistent, there are no bubbles, no turbidity, and no visible impurities. Since the uneven distribution of the particle size of each molecule immersed in the polymer material solution forms tension on the product surface, the vacuum negative pressure value and the impregnation automation parameters are set to allow each molecule to break through the tension formed on the product surface during the entire impregnation process and impregnate into the internal pores of the tantalum core;

[0074] Step 5: Dry the impregnated anode body at room temperature for 6 minutes, and then solidify the anode body after drying. Figure 3 The curing temperature curve in the figure is from room temperature to 55°C, kept for 6 minutes, then raised to 85°C, kept for 1 minute, then raised to 105°C, kept for 3 minutes, and finally raised to 125°C, kept for 10 minutes. The horizontal axis in the figure is time, the vertical axis is temperature, and the room temperature is 25°C.

[0075] Step 6: Repeat the process of step 4-step 6 25 times to form a polymer layer on the surface of the oxide film of the anode body. It should be noted that when repeating the process of step 4-step 6, the solid content of the polymer material solution in step 4 needs to be measured before each immersion of a product of a certain specification. If the condition is not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured until the fixed content reaches the set value;

[0076] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the drying time is: 30min±3min, and the timing starts when the target temperature is reached, and the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0077] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0078] Step 9: Apply 1.2 times the rated voltage to the finished product in step 8 for aging screening to eliminate unqualified products.

[0079] Table 2 below shows the loss, ESR, and leakage comparison of the 4V, 5600uF axial lead organic polymer tantalum fixed capacitor manufactured by the method of Example 2, the existing polymer electrolyte capacitor of the same specification, and the chip tantalum polymer electrolyte capacitor of the same specification:

[0080]

[0081] Table 2

[0082] Example 3

[0083] The production specifications are: 125V, 68μF axial lead organic polymer tantalum fixed capacitor;

[0084] Step 1: 6028 mg of tantalum powder and 180.84 mg of camphor powder are uniformly mixed and placed in a mold cavity with a size of Φ8 mm*15 mm, and a Φ0.6 mm tantalum wire is inserted into the center of the mixed powder for pressing, wherein the camphor powder is used as a binder to form an anode blank with a Φ0.6 mm tantalum wire core pressed and placed in a sintering furnace for calcination to form an anode body with a microporous structure;

[0085] Step 3: Use a spot welder to weld the tantalum core of the anode body to a steel bar, and place the steel bar on a process rack. Use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body. The specific process is to place the anode body in a 0.1% H3PO4+75% ethylene glycol energizing solution at 80°C, apply a 310V energizing constant voltage, and continue for 240 minutes;

[0086] Step 4: Use a vacuum impregnation tank to carry the PEDOT solution, and impregnate the oxide film anode body formed in step 3 under a vacuum state of -65kpa±2kpa, wherein the solid content of the PEDOT solution is 0.8-9%, and the viscosity value is 1500mPa.S; the vacuum impregnation tank is automatically lowered and raised at a speed of 0.03mm / s, and the impregnation time is 10min. During the manufacturing process, the polymer liquid level is required to be level, the overflow is consistent, there are no bubbles, no turbidity and any visible impurities. Since the uneven distribution of the particle size of each molecule immersed in the polymer material solution forms tension on the product surface, the vacuum negative pressure value and the impregnation automation parameters are set to allow each molecule to break through the tension formed on the product surface during the entire impregnation process and impregnate into the internal pores of the tantalum core;

[0087] Step 5: Dry the impregnated anode body at room temperature for 6 minutes, and then solidify the anode body after drying. Figure 3 The curing temperature curve in the figure is from room temperature to 55°C, kept for 6 minutes, then raised to 85°C, kept for 1 minute, then raised to 105°C, kept for 3 minutes, and finally raised to 125°C, kept for 10 minutes. The horizontal axis in the figure is time, the vertical axis is temperature, and the room temperature is 25°C.

[0088] Step 6: Repeat the process of step 4-step 6 25 times to form a polymer layer on the surface of the oxide film of the anode body. It should be noted that when repeating the process of step 4-step 6, the solid content of the polymer material solution in step 4 needs to be measured before each immersion of a product of a certain specification. If the condition is not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured until the fixed content reaches the set value;

[0089] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the drying time is: 30min±3min, and the timing starts when the target temperature is reached, and the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0090] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0091] Step 9: Apply 1.1 times the rated voltage to the finished product in step 8 for aging screening to remove unqualified products.

[0092] Table 3 below shows the loss, ESR, and leakage comparison of the 125V, 68μF axial lead organic polymer tantalum fixed capacitor manufactured by the method of Example 3, the existing polymer electrolyte capacitor of the same specification, and the chip tantalum polymer electrolyte capacitor of the same specification:

[0093]

[0094] Table 3

[0095] Example 4

[0096] The production specifications are: 4V, 4.7μF axial lead organic polymer tantalum fixed capacitor;

[0097] Step 1: 17 mg of tantalum powder and 0.51 mg of camphor powder are uniformly mixed and placed in a mold cavity of Φ1.5 mm*1.5 mm in size, and a Φ0.4 mm tantalum wire is inserted into the center of the mixed powder for pressing, wherein the camphor powder is used as a binder to form an anode blank with a Φ0.6 mm tantalum wire core, which is then placed in a sintering furnace for calcination to form an anode body with a microporous structure;

[0098] Step 3: Use a spot welder to weld the tantalum core of the anode body to a steel bar, and place the steel bar on a process rack. Use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body. The specific process is to place the anode body in a 0.1% HNO3 energizing solution at 80°C, apply a 60V energizing constant voltage, and continue for 240 minutes;

[0099] Step 4: Use a vacuum impregnation tank to carry the PEDOT solution, and impregnate the oxide film anode body formed in step 3 under a vacuum state of -65kpa±2kpa, wherein the solid content of the PEDOT solution is 0.8-9%, and the viscosity value is 1500mPa.S; the vacuum impregnation tank is automatically lowered and raised at a speed of 0.03mm / s, and the impregnation time is 10min. During the manufacturing process, the polymer liquid level is required to be level, the overflow is consistent, there are no bubbles, no turbidity and any visible impurities. Since the uneven distribution of the particle size of each molecule immersed in the polymer material solution forms tension on the product surface, the vacuum negative pressure value and the impregnation automation parameters are set to allow each molecule to break through the tension formed on the product surface during the entire impregnation process and impregnate into the internal pores of the tantalum core;

[0100] Step 5: Dry the impregnated anode body at room temperature for 6 minutes, and then solidify the anode body after drying. Figure 3 The curing temperature curve in the figure is from room temperature to 55°C, kept for 6 minutes, then raised to 85°C, kept for 1 minute, then raised to 105°C, kept for 3 minutes, and finally raised to 125°C, kept for 10 minutes. The horizontal axis in the figure is time, the vertical axis is temperature, and the room temperature is 25°C.

[0101] Step 6: Repeat the process of step 4-step 6 12 times to form a polymer layer on the surface of the oxide film of the anode body. It should be noted that when repeating the process of step 4-step 6, the solid content of the polymer material solution in step 4 needs to be measured before each immersion of a product of a certain specification. If the condition is not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured until the fixed content reaches the set value;

[0102] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the drying time is: 30min±3min, and the timing starts when the target temperature is reached, and the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0103] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0104] Step 9: Apply 1.2 times the rated voltage to the finished product in step 8 for aging screening to eliminate unqualified products.

[0105] Table 4 below shows the loss, ESR, and leakage comparison of the 4V, 4.7μF axial lead organic polymer tantalum fixed capacitor manufactured by the method of Example 4, the existing polymer electrolyte capacitor of the same specification, and the chip tantalum polymer electrolyte capacitor of the same specification:

[0106]

[0107] Table 4

[0108] Example 5

[0109] The production specifications are: 50V, 280μF axial lead organic polymer tantalum fixed capacitor;

[0110] Step 1: 6899 mg of tantalum powder and 206.97 mg of camphor powder are uniformly mixed and placed in a mold cavity with a size of Φ8.3 mm*17 mm, and a Φ0.6 mm tantalum wire is inserted into the center of the mixed powder for pressing, wherein the camphor powder is used as a binder to form an anode blank with a Φ0.6 mm tantalum wire core, which is then placed in a sintering furnace for calcination to form an anode body with a microporous structure;

[0111] Step 3: Use a spot welder to weld the tantalum core of the anode body to a steel bar, and place the steel bar on a process rack. Use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body. The specific process is to place the anode body in a 0.1% H3PO4+50% ethylene glycol energizing solution at 80°C, apply a 197V energizing constant voltage, and continue for 240 minutes;

[0112] Step 4: Use a vacuum impregnation tank to carry the PEDOT solution, and impregnate the oxide film anode body formed in step 3 under a vacuum state of -65kpa±2kpa, wherein the solid content of the PEDOT solution is 0.8-9%, and the viscosity value is 1500mPa.S; the vacuum impregnation tank is automatically lowered and raised at a speed of 0.03mm / s, and the impregnation time is 10min. During the manufacturing process, the polymer liquid level is required to be level, the overflow is consistent, there are no bubbles, no turbidity and any visible impurities. Since the uneven distribution of the particle size of each molecule immersed in the polymer material solution forms tension on the product surface, the vacuum negative pressure value and the impregnation automation parameters are set to allow each molecule to break through the tension formed on the product surface during the entire impregnation process and impregnate into the internal pores of the tantalum core;

[0113] Step 5: Dry the impregnated anode body at room temperature for 6 minutes, and then solidify the anode body after drying. Figure 3 The curing temperature curve in the figure is from room temperature to 55°C, kept for 6 minutes, then raised to 85°C, kept for 1 minute, then raised to 105°C, kept for 3 minutes, and finally raised to 125°C, kept for 10 minutes. The horizontal axis in the figure is time, the vertical axis is temperature, and the room temperature is 25°C.

[0114] Step 6: Repeat the process of step 4-step 6 24 times to form a polymer layer on the surface of the oxide film of the anode body. It should be noted that when repeating the process of step 4-step 6, the solid content of the polymer material solution in step 4 needs to be measured before each immersion of a product of a certain specification. If the condition is not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and the viscosity of the polymer solution after stirring is measured until the fixed content reaches the set value;

[0115] Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and the coating is carried out at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the drying time is: 30min±3min, and the timing starts when the target temperature is reached, and the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product;

[0116] Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product;

[0117] Step 9: Apply 1.2 times the rated voltage to the finished product in step 8 for aging screening to eliminate unqualified products.

[0118] Table 5 below shows the loss, ESR, and leakage comparison of the 50V, 280μF axial lead organic polymer tantalum fixed capacitor manufactured by the method of Example 5, the existing polymer electrolyte capacitor of the same specification, and the chip tantalum polymer electrolyte capacitor of the same specification:

[0119]

[0120] Table 5

[0121] By utilizing the manufacturing method of an axially leaded organic polymer tantalum fixed capacitor provided by the present invention, an axially leaded organic polymer tantalum fixed capacitor with a rated voltage of 4 to 125 V, a capacity of 4.7 to 5600 μF, and an ESR of 30 to 500 mΩ can be manufactured. On the one hand, the performance is greatly improved compared with the same specification products in the prior art, and on the other hand, it fills the market gap and has extremely high promotion value.

Claims

1. A method for manufacturing an axially-lead organic polymer tantalum fixed capacitor, characterized in that: The following steps are involved: Step 1: Put tantalum powder and tantalum wire into the mold cavity, and use a molding machine to apply pressure to the tantalum powder in the mold cavity to form an anode blank with a tantalum core; Step 2: placing the pressed anode body into a sintering furnace for calcining to form an anode body with a microscopic porous structure; Step 3: Use a spot welder to weld the tantalum core of the anode body to the steel bar to form a group, and place the steel bar on the process frame, and use an electrochemical method to energize the anode body so that a dense Ta2O5 oxide film is formed on the surface of the anode body; Step 4: using a vacuum impregnation tank to carry a polymer material solution, and at a pressure of (-60 to -80 kPa) ± 2 kPa, impregnating the oxide film anode body formed in step 3, wherein the polymer material solution is a PEDOT solution, the solid content of which is 0.8% to 9%, and the viscosity is 1000 to 2500 mPa.S; the vacuum impregnation tank automatically descends and rises at a speed of 0.01 to 0.03 mm / s, and the impregnation time is 10 min to 15 min; Step 5: Dry the impregnated anode body at room temperature for 5 to 8 minutes, then perform high temperature curing, raise the temperature to 125°C, and maintain the constant temperature for 10 to 15 minutes after reaching the target temperature; Step 6: Repeat the process of step 4 to step 5 12 to 25 times according to the specifications of the capacitor to form a polymer layer on the surface of the oxide film of the anode body; Step 7: The high molecular polymer layer of the anode body that has completed the process of step 6 is coated with a graphite layer and a silver paste layer in sequence, wherein the graphite viscosity requirement is: 300-500mPa·s; the silver paste viscosity requirement is: 2000-3000mPa·s viscosity, and both are coated at room temperature. After the graphite layer and the silver paste layer are coated, they need to be placed for 30 minutes before drying. The drying temperature of the graphite layer and the silver paste layer is: 150±3°C; after the temperature rises from room temperature to the target temperature, the constant temperature is maintained for 30min±3min, and then the tantalum wire is welded to lead out the anode lead of the capacitor to form a semi-finished product; Step 8: The semi-finished product in step 7 is set on the copper shell by soldering, the cathode lead of the cathode capacitor is led out from the bottom of the copper shell, and the upper part of the copper shell is sealed with glass insulating powder to form an axially led organic polymer tantalum fixed capacitor finished product; Step 9: Perform aging screening on the finished products in step 8 and eliminate unqualified products; The process of using the electrochemical method to energize the anode body described in step three is to place the anode body in an energizing liquid at 80°C, and apply a constant energizing voltage of 24V to 320V according to the specifications of the capacitor for 240 minutes; the selection of the energizing liquid is related to the energizing voltage. When the energizing voltage is <80V, the energizing liquid is selected as a 0.1% HNO3 solution; when 80V≤energizing voltage<180V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 20% ethylene glycol; when 180V≤energizing voltage<300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 50% ethylene glycol; when the energizing voltage is ≥300V, the energizing liquid is selected as a mixed solution of 0.1% H3PO4 and 75% ethylene glycol; When the process of step 4 to step 5 is repeated in step 6, the solid content of the polymer material solution in step 4 needs to be measured before each specification product is impregnated. If the condition is not met, the polymer material solution needs to be supplemented. After the solution is supplemented, the polymer solution needs to be stirred for 5 to 7 minutes using a stirring paddle until there is no obvious agglomeration; and The viscosity of the polymer solution after stirring was measured. The method for determining the viscosity of the polymer solution is as follows: pour the polymer material solution into a 1000mL beaker, adjust the viscometer to a horizontal position, select a rotor with a range of 0 to 25000mPa·S, select a rotation speed of 120r / min, ensure that the solution must be submerged in the scale specified on the rotor, start the viscometer host, start measuring, record the read data after the value stabilizes, then press the reset button, measure three sets of data and take the average value, which is the viscosity value of the solution.

2. The method for manufacturing an axially-lead organic polymer tantalum fixed capacitor according to claim 1, characterized in that: In step 1, the tantalum powder is uniformly mixed with camphor powder, and the mass of the camphor powder is 3% of the mass of the tantalum powder.

3. The method for manufacturing an axially-lead organic polymer tantalum fixed capacitor according to claim 1, characterized in that: The aging process described in step nine is to apply an aging voltage of 1.1 to 1.2 times of the rated voltage to the finished axially lead organic polymer tantalum fixed capacitor.

4. The method for manufacturing an axially-lead organic polymer tantalum fixed capacitor according to claim 1, characterized in that: The high temperature curing process in step five is to increase the temperature from room temperature to 55°C, maintain for 6 minutes, then increase the temperature to 85°C, maintain for 1 minute, then increase the temperature to 105°C, maintain for 3 minutes, and finally increase the temperature to 125°C, maintain for 10 to 15 minutes.

Citation Information

Patent Citations

  • A two-step method for manufacturing PEDT cathode plate tantalum electrolytic capacitors

    CN102270535A

  • Metal shell packaged polymer tantalum capacitor and preparation method thereof

    CN104319103A

  • Preparation method for ultra-high-capacity tantalum capacitor

    CN105977030A

  • Preparation method of high-voltage chip solid electrolyte tantalum capacitor

    CN111696786A

  • Chip tantalum electrolytic capacitor and preparation method thereof

    CN113077987A

Cited By

  • Solid aluminum electrolytic capacitor and preparation method of composite anode foil thereof

    CN122800447A