An oxygen reduction catalyst having a platinum-bismuth alloy shell layer and its preparation method and application
Through microwave-assisted ethylene glycol reduction method and acidification heat treatment technology, an oxygen reduction catalyst with a platinum bismuth alloy shell structure was prepared, which solved the problem of poor durability of platinum carbon catalysts, improved the activity and stability of the catalyst, and was suitable for fuel cells, etc. field.
Patent Information
- Application Number
- CN202211053562.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-31
AI Technical Summary
The existing platinum carbon catalysts have poor durability in oxygen reduction reactions, and their activity decreases over time, making it difficult to meet the needs of high efficiency and high stability.
Platinum alloy solid solution nanoparticles were prepared by microwave-assisted ethylene glycol reduction method, and an oxygen reduction catalyst with a platinum bismuth alloy shell structure was obtained through acidification and heat treatment, which regulates the electronic structure on the surface of the material and improves the activity and stability of the catalyst.
The activity and stability of the catalyst are significantly improved, making it better than commercial platinum carbon catalysts under acidic conditions, and are suitable for proton exchange membrane fuel cells and metal-air fuel cells.
Smart Images

Figure 220831140139 
Figure 220831140144 
Figure 220831140151
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of catalysts, and in particular relates to an oxygen reduction catalyst having a platinum-bismuth alloy shell layer, and a preparation method and application thereof. Background Art
[0002] In fuel cells, metal-air batteries, chlor-alkali industry, etc., the slow reaction kinetics of the oxygen reduction reaction process at the cathode directly affects the reaction efficiency of the entire electrochemical energy device and becomes a key factor restricting development. At present, platinum-carbon catalysts are still the most commonly used catalysts to improve the efficiency of oxygen reduction reactions. However, the activity of platinum-carbon catalysts tends to decrease over time during the catalytic process, and the activity needs to be further improved, which restricts large-scale applications. Therefore, the development of catalysts with both high efficiency and high stability for oxygen reduction reactions is an urgent problem to be solved. Platinum alloy catalysts have received widespread attention due to their structure and electronic effects. However, transition metals on the surface and near the surface are still difficult to withstand harsh working environments (high potential, strong acid, high oxygen, water, frequent start-stop, etc.) and lead to precipitation. Therefore, it is of great significance to study and develop highly stable and highly active platinum-based oxygen reduction catalysts and their preparation methods. Summary of the invention
[0003] The purpose of the present invention is to solve the problems of poor durability of platinum-carbon catalysts in oxygen reduction reactions, while ensuring high activity of the catalyst, and provide a simple and effective method for preparing an oxygen reduction catalyst with a platinum-bismuth alloy shell structure to promote the improvement of catalyst activity and stability. First, platinum alloy solid solution nanoparticles are prepared as a precursor by microwave-assisted ethylene glycol reduction, and platinum alloy intermetallic compound nanoparticles obtained by subsequent heat treatment are used as precursors. The surface energy of bismuth is low and it is easy to form a platinum-bismuth alloy with platinum. The prepared platinum alloy solid solution / intermetallic compound nanoparticles are acidified and heat-treated to obtain a platinum alloy oxygen reduction catalyst with a platinum-bismuth alloy shell structure. The coordination and strain effects produced by the platinum alloy oxygen reduction catalyst with a platinum-bismuth alloy shell structure effectively regulate the electronic structure of the material surface, improve the activity of the catalyst, and promote the improvement of catalyst stability. The preparation method adopted by the catalyst is easy to operate and controllable, and has strong operability.
[0004] In order to achieve the purpose of the invention, the present invention adopts the following technical scheme: an oxygen reduction catalyst with a platinum-bismuth alloy shell layer, wherein the catalyst is a black solid powder, with carbon black loaded platinum alloy solid solution / intermetallic compound as the core and platinum-bismuth alloy as the shell layer.
[0005] In a preferred embodiment of the present invention, in the catalyst, the mass ratio of platinum to bismuth is 6:1 to 9:1, and the mass ratio of platinum to carbon black carrier is 1:1 to 1:10.
[0006] In a preferred embodiment of the present invention, the particle size of the catalyst is 5 to 15 nm.
[0007] The present invention also protects a method for preparing the oxygen reduction catalyst having a platinum-bismuth alloy shell, which specifically comprises the following steps:
[0008] (1) Add carbon black to a solvent and disperse it to obtain a black suspension, add chloroplatinic acid solution and potassium iodide, and then add at least one of an iron source, a cobalt source, and a nickel source, continue to disperse it by ultrasonication until it is uniform, and adjust the pH value to 7-14;
[0009] (2) placing the black suspension obtained in step (1) into a container, heating the suspension in an environment of 150-200°C for reaction, and after the reaction is completed, filtering the obtained solution, washing and drying the solution to obtain carbon black-loaded platinum alloy nanoparticles, which are catalyst precursors;
[0010] (3) heating the carbon black-loaded platinum alloy solid solution nanoparticles obtained in step (2) to 600-1000° C. in a reducing atmosphere for less than 3 h, cooling to room temperature, and grinding to obtain platinum alloy intermetallic compound nanoparticles, i.e., catalyst precursors;
[0011] (4) Acidification process: soak the catalyst precursor obtained in step (2) or step (3) in an acid containing bismuth ions for 4 to 24 hours for acidification treatment, and then wash and dry;
[0012] (5) Annealing process: The sample dried in step (4) is heated to 200-600°C in a reducing atmosphere, kept at this temperature for less than 10 h, cooled to room temperature, and ground to obtain an oxygen reduction catalyst having a platinum-bismuth alloy shell.
[0013] In a preferred embodiment of the present invention, in step (1), potassium iodide is used as an additive to promote the formation of an alloy structure, and the mass ratio of the added potassium iodide content to the platinum content is 1:2 to 3:1; the concentration of the chloroplatinic acid solution is 0.001 to 0.1 mol / L, and the mass ratio of the added platinum content to the carbon black carrier content is 1:1 to 1:10.
[0014] In a preferred embodiment of the present invention, in step (1), the solvent used is ethylene glycol; the iron source is an ethylene glycol solution of ferrous chloride, the cobalt source is an ethylene glycol solution of cobalt chloride, and the nickel source is an ethylene glycol solution of nickel chloride; and the pH value of the black suspension is adjusted by potassium hydroxide aqueous solution, and the concentration of the potassium hydroxide solution is 0.5 to 3 mol / L.
[0015] In a preferred embodiment of the present invention, the annealing process contained in step (3) is specifically as follows: the carbon black-loaded platinum-based solid solution nanoparticles obtained in step (2) are heated to 600-1000°C at a heating rate of 5-10°C / min under a reducing atmosphere, and kept warm for 1-3 hours, then cooled to room temperature, and ground.
[0016] In a preferred embodiment of the present invention, in step (4), bismuth chloride is used as a bismuth source for preparing a platinum alloy oxygen reduction catalyst having a platinum-bismuth alloy shell structure, and its concentration is 0.001 to 0.1 mol / L, and the mass ratio of the added bismuth content to the platinum content is 1:6 to 1:9.
[0017] In a preferred embodiment of the present invention, in step (4), perchloric acid is used for acidification, and the concentration thereof is 0.01 to 1 mol / L.
[0018] In a preferred embodiment of the present invention, in step (5), the annealing process is: in a reducing atmosphere, the temperature is raised to 300-600°C at a heating rate of 5-10°C / min, and kept at this temperature for 1-3 hours, then cooled to room temperature, and ground to obtain a catalyst having a carbon black-loaded platinum alloy as a core and a platinum-bismuth alloy as a shell.
[0019] The invention also protects the use of the catalyst as an oxygen reduction catalyst in an acidic or alkaline medium.
[0020] Compared with the prior art, the present invention uses ethylene glycol as a solvent and a reducing agent, and the prepared carbon black-loaded platinum alloy nanoparticles and the platinum alloy intermetallic compound nanoparticles obtained by subsequent heat treatment are used as precursors, and then adopts an acidification and heat treatment method to obtain an oxygen reduction catalyst with a carbon black-loaded platinum alloy as a core and a platinum-bismuth alloy as a shell. Compared with the prior art, the present invention has the following advantages: the preparation of platinum alloy nanoparticles is experimented with an improved microwave-assisted ethylene glycol reduction method, and a platinum alloy oxygen reduction catalyst with a platinum-bismuth alloy shell structure is obtained by acidification and annealing. The catalyst with a platinum-bismuth alloy shell structure promotes the improvement of catalytic activity and stability, and the performance of oxygen reduction catalytic activity and stability under acidic conditions are better than those of commercial platinum-carbon catalysts.
[0021] The preparation method of the present invention is easy to implement and controllable, and has strong operability. The catalyst prepared by the present invention can be widely used in the fields of proton exchange membrane fuel cells, metal-air fuel cells, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention will be further described below in conjunction with the accompanying drawings.
[0023] Figure 1This is a transmission electron microscope photograph of the catalyst prepared in Example 1, which has a carbon black-supported platinum-iron intermetallic compound as a core and a platinum-bismuth alloy as a shell.
[0024] Figure 2 This is the X-ray diffraction pattern of the catalyst prepared in Example 1, which has a carbon black-supported platinum-iron intermetallic compound as a core and a platinum-bismuth alloy as a shell.
[0025] Figure 3 This is a rotating disk curve diagram of the stability test of the catalyst prepared in Example 1, which has a carbon black-supported platinum-iron intermetallic compound as a core and a platinum-bismuth alloy as a shell. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0027] Example 1
[0028] 0.05 g of Vulcan XC-72 was added to 30 mL of ethylene glycol solution, and then stirred and ultrasonicated for about 0.5 h until uniformly dispersed to obtain a black suspension A.
[0029] Add 0.1 mol / L ethylene glycol solution of chloroplatinic acid, 2 mg of potassium iodide, and 0.1 mol / L ethylene glycol solution of ferrous chloride in sequence, continue ultrasonication until uniform dispersion, then add 0.5 mol / L sodium hydroxide solution and adjust the pH value to 8. Pour into a reactor, microwave heating at 200 °C for 1 h, and after the reaction, filter the obtained solution, wash and dry to obtain a black solid powder.
[0030] Primary annealing process: The obtained black solid powder is placed in a tubular furnace, and heated to 900 °C at a rate of 10 °C / min under a reducing atmosphere, and kept warm for 2 h, then cooled to room temperature, and ground to obtain a carbon black-loaded platinum-iron intermetallic compound catalyst.
[0031] Acidification process: The carbon black-supported platinum-iron intermetallic compound catalyst is immersed in perchloric acid containing bismuth ions for 12 hours, then washed and dried to obtain an acidified black solid powder.
[0032] Secondary annealing process: The black solid powder obtained after acidification was placed in a tubular furnace, and heated to 500 °C at a rate of 10 °C / min under a reducing atmosphere, and kept warm for 1 h. It was then cooled to room temperature and ground to obtain a catalyst with a carbon black-loaded platinum-iron intermetallic compound as the core and a platinum-bismuth alloy as the shell.
[0033] Example 2
[0034] 0.6 g BP2000 was added into 300 mL ethylene glycol solution, and then ultrasonicated for about 1 h until the mixture was evenly dispersed to obtain a black suspension A.
[0035] 1 mol / L chloroplatinic acid in ethylene glycol solution, 50 mg potassium iodide, and 1 mol / L cobalt chloride in ethylene glycol solution were added in sequence, and ultrasonication was continued until uniform dispersion, and then 1 mol / L sodium hydroxide solution was added to adjust the pH value to 9. The mixture was poured into a reactor and heated in a microwave at 180 °C for 2 h. After the reaction, the obtained solution was filtered, washed, and dried to obtain a black solid powder.
[0036] Acidification process: The carbon black-loaded platinum-cobalt intermetallic compound catalyst is immersed in perchloric acid containing bismuth ions for 24 hours, then washed and dried to obtain an acidified black solid powder.
[0037] Annealing process: The black solid powder obtained after acidification was placed in a tubular furnace, and heated to 400 °C at a rate of 5 °C / min under a reducing atmosphere, and kept warm for 2 h. It was then cooled to room temperature and ground to obtain a catalyst with a carbon black-loaded platinum-cobalt alloy as the core and a platinum-bismuth alloy as the shell.
[0038] Example 3
[0039] 0.05 g of Vulcan XC-72 was added to 30 mL of ethylene glycol solution, and then stirred and ultrasonicated for about 1 h until the dispersion was uniform to obtain a black suspension A.
[0040] Add 0.5 mol / L chloroplatinic acid in ethylene glycol, 10 mg potassium iodide, and 0.5 mol / L nickel chloride in ethylene glycol in sequence, continue ultrasonication until uniform dispersion, then add 0.1 mol / L sodium hydroxide solution and adjust the pH value to 10. Pour into a reactor, microwave heating at 190 °C for 3 h, and after the reaction, filter the obtained solution, wash and dry to obtain a black solid powder.
[0041] Primary annealing process: The obtained black solid powder was placed in a tubular furnace, and heated to 700 °C at a rate of 8 °C / min under a reducing atmosphere, and kept warm for 3 h, then cooled to room temperature, and ground to obtain a carbon black-loaded platinum-nickel intermetallic compound catalyst.
[0042] Acidification process: The carbon black-loaded platinum-cobalt intermetallic compound catalyst is immersed in perchloric acid containing bismuth ions for 18 hours, then washed and dried to obtain an acidified black solid powder.
[0043] Secondary annealing process: The black solid powder obtained after acidification was placed in a tubular furnace, and heated to 550 °C at a rate of 8 °C / min under a reducing atmosphere, and kept warm for 3 h. It was then cooled to room temperature and ground to obtain a catalyst with a carbon black-loaded platinum-nickel intermetallic compound as the core and a platinum-bismuth alloy as the shell.
[0044] The product prepared in Example 1 was characterized and analyzed. Figure 1 It can be seen that the catalyst is evenly dispersed on the surface of the carbon support. Figure 2 It can be seen that the catalyst has an intermetallic compound structure, and an asymmetric peak appears at the (111) crystal plane, indicating the formation of a platinum-bismuth shell structure. Figure 3 It can be seen that the prepared catalyst with carbon black loaded platinum-iron intermetallic compound as the core and platinum-bismuth alloy as the shell still maintains a relatively high half-wave potential after 5000 and 10000 cycles of testing, and has very excellent stability.
[0045] The above specific implementation methods describe the basic principles and main features of the present invention. Those skilled in the art should understand that the protection scope of the present invention is not limited by the above embodiments, and any changes or substitutions that are not conceived through creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.
Claims
1. An oxygen reduction catalyst having a platinum-bismuth alloy shell, characterized in that: The catalyst is a black solid powder, wherein the carbon black-supported platinum alloy solid solution / intermetallic compound is the core and the platinum-bismuth alloy is the shell; in the catalyst, the mass ratio of platinum to bismuth is 6:1-9:1, and the mass ratio of platinum to carbon black carrier is 1:1-1:10; the particle size of the catalyst is 5-15 nm; and the preparation method thereof comprises the following steps: (1) Add carbon black to a solvent and disperse it to obtain a black suspension, add chloroplatinic acid solution and potassium iodide, and then add at least one of an iron source, a cobalt source, and a nickel source, continue to disperse it by ultrasonication until it is uniform, and adjust the pH value to 7-14; (2) placing the black suspension obtained in step (1) into a container, heating the suspension in a microwave at 180-200° C. for reaction, and filtering, washing and drying the obtained solution after the reaction to obtain carbon black-loaded platinum alloy solid solution nanoparticles, i.e., catalyst precursor; (3) heating the carbon black-loaded platinum alloy solid solution nanoparticles obtained in step (2) to 600-1000° C. in a reducing atmosphere for less than 3 h, cooling to room temperature, and grinding to obtain platinum alloy intermetallic compound nanoparticles, i.e., catalyst precursors; (4) Acidification process: the catalyst precursor obtained in step (2) or step (3) is soaked in an acid containing bismuth ions for 4-24 hours for acidification treatment, and then washed and dried; (5) Annealing process: heating the sample dried in step (4) to 200-600° C. in a reducing atmosphere, keeping the temperature for less than 10 h, cooling to room temperature, and grinding to obtain an oxygen reduction catalyst having a platinum-bismuth alloy shell; In step (1), potassium iodide is used as an additive to promote the formation of the alloy structure, and the mass ratio of the added potassium iodide content to the platinum content is 1:2-3:1; the concentration of the chloroplatinic acid solution is 0.001-0.1 mol / L, and the mass ratio of the added platinum content to the carbon black carrier content is 1:1-1:10; The annealing process in step (3) is specifically as follows: heating the carbon black-loaded platinum-based solid solution nanoparticles obtained in step (2) to 600-1000°C at a heating rate of 5-10°C / min under a reducing atmosphere, and keeping the temperature for 1-3 hours, then cooling to room temperature, and grinding; In step (5), the annealing process is: in a reducing atmosphere, the temperature is raised to 300-600°C at a rate of 5-10°C / min, and kept at this temperature for 1-3 hours, then cooled to room temperature, and after grinding, a catalyst having a carbon black-loaded platinum solid solution / intermetallic compound as a core and a platinum-bismuth alloy as a shell is obtained.
2. The oxygen reduction catalyst according to claim 1, characterized in that In step (1), the solvent used is ethylene glycol; the iron source is an ethylene glycol solution of ferrous chloride, the cobalt source is an ethylene glycol solution of cobalt chloride, and the nickel source is an ethylene glycol solution of nickel chloride; and a potassium hydroxide aqueous solution is used to adjust the pH value of the black suspension, and the concentration of the potassium hydroxide solution is 0.5-3 mol / L.
3. The oxygen reduction catalyst according to claim 1, characterized in that In step (4), bismuth chloride is used as a bismuth source for preparing a platinum alloy oxygen reduction catalyst having a platinum-bismuth alloy shell structure, and its concentration is 0.001-0.1 mol / L, and the mass ratio of the added bismuth content to the platinum content is 1:6 - 1:9; and the acidification treatment is carried out using perchloric acid, and its concentration is 0.01-1 mol / L.
4. Use of the oxygen reduction catalyst according to any one of claims 1 to 3 as an oxygen reduction catalyst in an acidic or alkaline medium.
Citation Information
Patent Citations
Preparation method of electro-catalyst Pt1Bi1 intermetallic compounds used for fuel batteries
CN101785999A
Carbon-supported core-shell type platinum cobalt-platinum catalyst for fuel cells and preparation method for carbon-supported core-shell type platinum cobalt-platinum catalyst
CN104475126A
Solid high molecular type fuel cell
JP1998092441A
Irreversible adsorption catalyst, manufacturing method of the same and fuel cell including the irreversible adsorption catalyst
KR1020180051730A
Electrode catalyst for fuel cell and method for production thereof
US20050075240A1
Cited By
Platinum-bismuth alloy catalyst, preparation method thereof and direct methanol fuel cell
CN121862772A
Platinum-bismuth alloy catalyst, method for preparing the same, and direct methanol fuel cell
CN121862772B