Preparation method of polyetherketoneketone and polyetherketoneketone prepared thereby

By controlling the catalyst addition rate and blowing in inert gas, the scaling formation of polyetherketoneketone is suppressed, the yield and particle size are improved, the scaling problem during the preparation process of polyetherketoneketone is solved, and efficient polymerization is achieved process.

CN115244104BActive Publication Date: 2024-10-15HANWHA SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080098293.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-09
Publication Date
2024-10-15
Estimated Expiration
2040-04-09

AI Technical Summary

Technical Problem

During the preparation process of polyetherketoneketone, scaling is prone to occur, resulting in reduced productivity. The existing technology fails to effectively solve the relationship between the catalyst addition rate and the yield.

Method used

By controlling the addition rate of the catalyst, using catalysts such as aluminum trichloride, potassium carbonate or ferric chloride, inert gas is blown into the reaction solution and stirred to form a vortex phenomenon, inhibiting the agglomeration of resin particles, thereby improving the performance of polyetherketoneketone. yield and particle size.

Benefits of technology

It achieves high yield (more than 90%) and large particle size (250-2000 μm) of polyetherketoneketone, reduces the possibility of dust scattering, facilitates operation, and obtains particles of various sizes through crushing after drying.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115244104B_ABST
    Figure CN115244104B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing polyetherketoneketone, which improves the yield by controlling the addition rate of a catalyst during preparation to suppress the formation of scale, and more specifically to a method for preparing polyetherketoneketone, which prevents the agglomeration phenomenon between resin particles while maintaining the intrinsic viscosity value without significant change to suppress the formation of scale, thereby obtaining a high molecular weight polyetherketoneketone with a high yield, preferably a yield of 90% or more, and the particle size of the polyetherketoneketone can be controlled, and the polyetherketoneketone prepared thereby.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing polyetherketoneketone, and more particularly to a method for preparing polyetherketoneketone, which can improve the yield by controlling the catalyst addition rate of the polyetherketoneketone during the preparation to inhibit the formation of scale and the polyetherketoneketone prepared thereby. Background Art

[0002] Polyetherketone is a general term for known industrial resins, and includes polyetherketone, polyetheretherketone, polyetherketoneketone, and a copolymer obtained by mixing a part of polyetherketone and polyetherketoneketone.

[0003] Polyether Ketone Ketone (PEKK) represented by the following chemical formula has high heat resistance and excellent strength and is widely used as an engineering plastic. Engineering plastics are used in the fields of automobiles, aircraft, electrical and electronic equipment, and machinery, and their application fields are gradually expanding.

[0004] Chemical formula:

[0005]

[0006] As the application fields of engineering plastics expand, the use environment becomes more and more severe, and a polyetherketone compound showing further improved physical properties is needed. In addition, in order to reduce the cost during the polymerization reaction, a preparation process with improved yield is needed.

[0007] That is, there is a problem that fouling is easily generated during the polymerization of polyetherketoneketone, which leads to a problem of reduced productivity. In this regard, a prior art is known that controls the catalyst addition rate to increase the actual polymer resin yield.

[0008] Although US Patent No. 4,891,167 discloses adding a catalyst at a specified rate, it is limited to polyaryl ether ketone (PAEK) and does not clearly disclose the relationship between the catalyst addition rate and the yield.

[0009] Korean Patent No. 0314176 discloses a catalyst adding device for olefin polymerization, which is similar in that the catalyst addition rate is controlled during polymer polymerization, but the polymer is limited to polyolefins rather than polyetherketoneketones.

[0010] Although U.S. Patent No. 4,841,013 discloses a method for obtaining a polymerized product by an additional step of crushing agglomerated particles after polymerization of polyaryl etherketone (PAEK) through a pulverization process, it does not directly mention improving the yield by inhibiting the formation of scale, which is a limitation in this regard.

[0011] US Patent No. 9,803,050 discloses a technique for controlling particle size using a dispersant.

[0012] Although the non-patent publication Chemical Engineering Science, (2011) Vol. 66 pp. 1189-1199 discloses that the production rate of a polymer increases with the increase in the rate of catalyst addition, the polymer disclosed is polypropylene, not polyetherketoneketone.

[0013] Finally, the non-patent publication High Perform.Polym.(2014)Vol.27,pp.705-713 only discloses the use of a catalyst in the preparation of polyetherketoneketone and that the catalyst feed ratio affects the intrinsic viscosity, but does not disclose any information related to the catalyst addition rate.

[0014] Therefore, it is necessary to develop a method for preparing polyetherketoneketone by inhibiting the formation of scale during the polymerization of polyetherketoneketone to improve the yield.

[0015] Prior Literature

[0016] (Patent Document 1) US 4891167

[0017] (Patent Document 2) KR 0314176

[0018] (Patent Document 3) US 4841013

[0019] (Patent Document 4) US 9803050

[0020] (Non-patent document 1) Chemical Engineering Science, (2011) Vol. 66 pp. 1189-1199

[0021] (Non-patent document 2) High Perform. Polym. (2014) Vol. 27, pp. 705-713 Summary of the invention

[0022] Technical issues

[0023] The object of the present invention is to solve all the above problems.

[0024] The object of the present invention is to provide a method for preparing polyetherketoneketone, which can improve the yield and increase the particle size by controlling the catalyst addition rate.

[0025] Technical Solution

[0026] In order to achieve the above-mentioned objects of the present invention and realize the specific effects of the present invention described below, the specific configuration of the present invention is as follows.

[0027] The preparation method of polyetherketoneketone involved in the present invention may include the following steps: step (a), in a reactor, adding at least one selected from diphenyl oxide (DPO) and 1,4-bis(4-phenoxybenzoyl)benzene (EKKE), terephthaloyl chloride (TPC) and isophthaloyl chloride (IPC) to a liquid reaction medium and dissolving them simultaneously to prepare a reaction solution; step (b), cooling the reaction solution and adding a catalyst; and step (c), after adding the catalyst, directly blowing an inert gas into the reaction solution and stirring it.

[0028] The catalyst is selected from at least one of aluminum chloride (Aluminum chloride, AlCl3), potassium carbonate (Potassium carbonate, K2CO3) and iron (III) chloride (Iron (III) chloride, FeCl3).

[0029] The catalyst was added at a rate of 1 to 10 g / min.

[0030] In the step (b), the cooling temperature is -10°C to -5°C.

[0031] In the step (c), a stirrer having a plurality of stirring blades is rotated to disperse the added inert gas.

[0032] At least two agitators are arranged in the reactor, rotating in at least two directions, thereby generating a vortex phenomenon.

[0033] A nozzle for directly blowing the inert gas into the reaction solution is formed at the upper part or the lower part of the reactor so as to be injected from multiple directions.

[0034] The inert gas is at least one selected from nitrogen, helium, neon, argon and krypton.

[0035] The step (c) comprises the step of raising the temperature of the reactor to 80° C. to 100° C. while stirring.

[0036] The method comprises the step of washing with deionized water (DI water) after step (c).

[0037] The method further comprises a step of vacuum drying at 170° C. to 190° C. after the water washing step.

[0038] The reaction solution includes at least one capping agent selected from benzoyl chloride, benzenesulfonyl chloride, 4-chlorobiphenyl, 4-phenoxybenzophenone, 4-(4-phenoxyphenoxy)benzophenone, and biphenyl-4-phenylsulfonylphenyl ether.

[0039] The liquid reaction medium is at least one solvent selected from o-dichlorobenzene (oDCB) and dichloromethane.

[0040] The polyetherketoneketone is prepared by the preparation method.

[0041] The yield of the polyetherketoneketone is 90% or more. In this case, the particle size of the polyetherketoneketone is 250 to 2000 μm.

[0042] Effects of the Invention

[0043] The preparation method of polyetherketoneketone disclosed by the present invention suppresses the formation of scale by controlling the catalyst addition rate, thereby improving the yield of polyetherketoneketone.

[0044] The preparation method of polyetherketoneketone of the present invention has a yield of more than 90% while maintaining the intrinsic viscosity (IV).

[0045] The preparation method of polyetherketoneketone of the present invention suppresses the formation of scale by controlling the catalyst addition rate to increase the particle size, thereby reducing the possibility of dust scattering, thereby facilitating operation.

[0046] The method for preparing polyetherketoneketone of the present invention can obtain particles of various sizes at high yields by drying large particles of polyetherketoneketone obtained at high yield and then further pulverizing the particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a photograph showing the shape of particles (particle size of 250 to 500 μm) prepared in Examples according to the present invention.

[0048] Figure 2 This is a photograph showing the shape of particles (particle size of 500 to 1000 μm) prepared in Examples according to the present invention.

[0049] Figure 3 This is a photograph showing the shape of particles (particle diameter: 20 to 100 μm) of a comparative example.

[0050] Figure 4 and Figure 5 This is a diagram showing an apparatus capable of stirring while introducing nitrogen gas into a reaction solution according to the method for producing polyetherketoneketone of the present invention. DETAILED DESCRIPTION

[0051] The detailed description of the present invention described below refers to the accompanying drawings, which illustrate specific embodiments in which the present invention can be implemented by way of example. These embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention. Although the various embodiments of the present invention are different, they are not necessarily mutually exclusive. For example, with respect to one embodiment, the specific features, structures and characteristics described herein may be implemented in other embodiments without departing from the spirit and scope of the present invention. In addition, the position or arrangement of individual constituent elements in each disclosed embodiment may be changed without departing from the spirit and scope of the present invention. Therefore, the detailed description described below is not intended to be limiting, and as long as it is properly described, the scope of the present invention is limited only by the full range of equivalents claimed by the claims and the appended claims. In the drawings, the same figure numerals refer to the same or similar functions in various aspects.

[0052] Hereinafter, in order to enable those skilled in the art to easily implement the present invention, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0053] In the present invention, scaling during the polymerization of polyetherketoneketone (PEKK) becomes an operational problem. In order to solve the resulting reduction in productivity, a technology is proposed for controlling the catalyst addition rate to increase the particle size and inhibit the formation of scaling, thereby improving the yield.

[0054] In the prior art, there is a problem that the prepared product is obtained by an additional process of controlling the particle size by using a dispersant or breaking the agglomerated particles by a pulverization process after polymerization. However, the present invention provides a preparation method based on the catalyst addition rate that can suppress the formation of scale by preventing the aggregation of resin particles by controlling the catalyst addition rate.

[0055] The polyetherketoneketone preparation method of the present invention is used to obtain high-molecular-weight polyetherketoneketone with high yield, and comprises the following steps: step (a), in a reactor, adding at least one selected from diphenyl oxide (Diphenyl oxide, DPO) and 1,4-bis (4-phenoxybenzoyl) benzene (1,4-bis (4-Phenoxybenzoyl) benzene, EKKE) and terephthaloyl chloride (Terephthaloyl chloride, TPC) and isophthaloyl chloride (Isophthaloyl chloride, IPC) to a liquid reaction medium, and dissolving them simultaneously to prepare a reaction solution; step (b), cooling the reaction solution and adding a catalyst; and step (c), after adding the catalyst, directly blowing an inert gas into the reaction solution and stirring it.

[0056] Polyetherketoneketone is a polymer formed by chain polymerization of terephthaloyl represented by the following chemical structure 1 and isophthaloyl represented by the following chemical structure 2, and its properties are determined by their ratio. The terephthaloyl moiety is linear and has a strong hardness. On this basis, the isophthaloyl moiety has a curved structure that gives it structural diversity. Isophthaloyl affects the flexibility, fluidity and crystallization properties of the polymer chain.

[0057] Chemical Structure 1:

[0058]

[0059] Chemical Structure 2:

[0060]

[0061] The catalyst may be selected from at least one of aluminum chloride (AlCl3), potassium carbonate (K2CO3) and iron (III) chloride (FeCl3), but is not limited thereto, as long as it can be used as a catalyst for Friedel-Crafts Acylation polymerization reaction.

[0062] Wherein, the catalyst can be added at a rate of 1 to 10 g / min. Preferably, it is added at a rate of 1 to 3 g / min, and more preferably at a rate of 1 to 1.5 g / min. When the catalyst is added at a rate of 1 to 10 g / min, the particle size of the prepared polyetherketoneketone can be increased. In addition, the yield of the prepared polyetherketoneketone can be improved. At this time, the yield of the polyetherketoneketone can be more than 90%.

[0063] In addition, the particle size of the polyetherketoneketone may be 250 to 2000 μm.

[0064] Due to the increase in particle size, the possibility of dust dispersion during the addition of products is reduced, making it easier to operate. Depending on the product requirements, when a small particle size is required, the particle size can be reduced by further pulverization after drying. In this way, the yield can be maintained while the particle size can be controlled.

[0065] In the preparation method of the present invention, the reaction solution is cooled before adding the catalyst. At this time, the temperature may vary depending on the catalyst, but is preferably -10°C to -5°C.

[0066] In the step (c), a stirrer having a plurality of stirring blades is rotated to disperse the added inert gas, and at least two stirrers are provided in the reactor to rotate in at least two directions, thereby generating a vortex phenomenon. The rotating shaft of the stirrer can be arranged to rotate alternately in a positive direction and a reverse direction at a predetermined angle. In addition, the stirring blades are formed to form a predetermined angle with the rotating shaft, thereby increasing the dispersing force of the composition in the reactor.

[0067] Figure 4 and Figure 5 : is a diagram showing an apparatus capable of stirring while introducing nitrogen into a reaction solution according to the method for producing polyetherketoneketone of the present invention. Figure 4 and Figure 5 The present invention relates to a method for preparing polyetherketoneketone, wherein a nozzle for directly blowing the inert gas into the reaction solution is formed at the upper or lower part of the reactor, so that the inert gas can be injected from multiple directions. Thus, the hydrochloric acid can be removed more quickly and effectively by the inert gas.

[0068] At this time, the inert gas is at least one selected from nitrogen, helium, neon, argon and krypton. The inert gas can be used alone or in combination during the polymerization reaction.

[0069] After adding the inert gas, the temperature of the reactor is raised to 80°C to 100°C while stirring to polymerize the polyetherketoneketone. The polymerization reaction involved in the present invention can be carried out in various reactors, but is preferably carried out in a continuous stirred reactor (CSTR) or a loop reactor.

[0070] The preparation method of polyetherketoneketone of the present invention comprises the steps of washing the polymerized polyetherketoneketone and washing with deionized water (DIwater). Methanol (CH3OH), hydrochloric acid and sodium hydroxide (NaOH) solutions may be provided in the washing, and preferably, the washing times are 3 times with methanol, 1 time with hydrochloric acid and 1 time with sodium hydroxide. The washing with hydrochloric acid and sodium hydroxide may be omitted.

[0071] After the washing, deionized water may be provided in the water washing step, and preferably, the number of times may be 3 times.

[0072] The method may further include vacuum drying at 170° C. to 190° C. after the water washing step to obtain a polyetherketoneketone polymer resin powder.

[0073] When the three monomers are added to a liquid reaction medium for dissolution, a capping agent can be added simultaneously and dissolved together. At this time, the capping agent is added to the medium of the polymerization reaction and acts to cap the polymer at at least one end of the polymer chain. Thus, the continuous extension of the chain is terminated and the molecular weight of the polymerized polymer is controlled. Preferably, benzoyl chloride, benzenesulfonyl chloride, 4-chlorobiphenyl, 4-phenoxybenzophenone, 4-(4-phenoxyphenoxy)benzophenone, biphenyl-4-benzenesulfonylphenyl phenyl ether, etc. can be used as the capping agent.

[0074] In addition, the liquid reaction medium may be at least one solvent selected from o-dichlorobenzene (oDCB) and dichloromethane, but is not limited thereto, as long as it can be used as a solvent for Friedel-Crafts Acylation polymerization reaction.

[0075] The polyetherketoneketone prepared by the preparation method has better physical properties than the polyetherketoneketone prepared by the prior art. In addition, according to the present invention, a catalyst is added at a rate of 1 to 10 g / min to prevent the agglomeration phenomenon between resin particles, thereby inhibiting the formation of scale, and thus a high molecular weight polyetherketoneketone can be obtained with a high yield. Preferably, the yield of the polyetherketoneketone can be 90% or more.

[0076] In addition, the particle size of the polyetherketoneketone may be 250 to 2000 μm.

[0077] In the method for preparing polyetherketoneketone of the present invention and the polyetherketoneketone prepared thereby, a catalyst is added at a rate of 1 to 20 g / min to prevent agglomeration between resin particles, thereby inhibiting the formation of scale and increasing the particle size. In addition, while maintaining the intrinsic viscosity (IV) value without significant change, a high molecular weight polyetherketoneketone is obtained with a high yield, preferably a yield of 90% or more.

[0078] The structure and function of the present invention are described in more detail below by using the preferred embodiments of the present invention. However, this is only provided as a preferred example of the present invention and should not be interpreted as limiting the present invention in any way.

[0079] The contents not described here can be fully inferred technically by a technician, so their description is omitted.

[0080] <Example>

[0081] Embodiment 1:

[0082] In the reactor, 26.6g of at least one of diphenyl oxide (DPO) and 1,4-bis(4-Phenoxybenzoyl)benzene (EKKE) as a monomer, 4.26g of terephthaloyl chloride (TPC) and 6.75g of isophthaloyl chloride (IPC), and 0.48g of benzoyl chloride as a capping agent were added to 750g of o-dichlorobenzene (oDCB) as a reaction solvent, and dissolved at the same time, and the reactor temperature was reduced to -10°C to -5°C. While keeping the dissolution temperature constant at -10°C to -5°C, 48g of AlCl3 as a catalyst was added at a rate of 1.1g / min. After the addition of the catalyst was completed, the temperature of the reactor was raised to 90° C. while stirring the solution while blowing N2 into the solution, and maintained for 30 minutes to polymerize the polyetherketoneketone. The polymerized resin was washed 3 times with methanol, 1M hydrochloric acid and 0.5M NaOH solution, and 3 times with deionized water, and vacuum dried at 180° C. to obtain a polyetherketoneketone polymerized resin.

[0083] Embodiment 2:

[0084] A polyetherketoneketone polymer resin was obtained in the same manner as in Example 1, except that the catalyst was added at a rate of 1.2 g / min.

[0085] Embodiment 3:

[0086] A polyetherketoneketone polymer resin was obtained in the same manner as in Example 1, except that the catalyst was added at a rate of 1.3 g / min.

[0087] Comparative Example 1:

[0088] A polyetherketoneketone polymer resin was obtained in the same manner as in Example 1, except that the catalyst was added at a rate of 0.8 g / min.

[0089] Comparative Example 2:

[0090] A polyetherketoneketone polymer resin was obtained in the same manner as in Example 1, except that the catalyst was added at a rate of 0.7 g / min.

[0091] Comparative Example 3:

[0092] A polyetherketoneketone polymer resin was obtained in the same manner as in Example 1, except that the catalyst was added at a rate of 0.6 g / min.

[0093] <Experimental Example> Inherent Viscosity (IV) and Yield Analysis

[0094] The intrinsic viscosity and yield of Examples 1 to 3 and Comparative Examples 1 to 3 prepared according to the present invention were measured, and the results are shown in Table 1 below.

[0095]

Table 1

[0096] distinguish Catalyst addition rate (g / min) IV (dL / g) Yield (%) Example 1 1.1 0.9 93 Example 2 1.2 0.9 96 Example 3 1.3 0.8 92 Comparative Example 1 0.8 0.9 66 Comparative Example 2 0.7 0.9 59 Comparative Example 3 0.6 1.0 62

[0097] Reference Figures 1 to 3 As shown in Table 1, the yields of polyetherketoneketones of Examples 1 to 3 prepared by adding the catalyst at a rate of 1 to 10 g / min according to the present invention are higher than those of Comparative Examples 1 to 3. In particular, Example 2 prepared by adding the catalyst at a rate of 1.2 g / min showed the highest yield, so it can be seen that the rate of 1.2 g / min is a preferred rate.

[0098] From the results of Comparative Examples 1 to 3, it can be seen that when the catalyst is added at a rate of less than 1 g / min, the yield is significantly reduced. Therefore, it can be seen that the catalyst addition rate range of 1 to 10 g / min of the present invention is preferred. Therefore, it can be seen that when the catalyst is added at a rate of 1 to 10 g / min of the present invention for preparation, the formation of scale can be suppressed, thereby improving the yield.

[0099] In addition, it can be seen that the polyether ketone ketone preparation method of the present invention and the polyether ketone ketone prepared by the method add a catalyst at a rate of 1 to 10 g / min, so that a high molecular weight polyether ketone ketone can be obtained with a high yield, preferably a yield of more than 90%, while maintaining the value of the intrinsic viscosity related to the molecular weight without significant change.

[0100] In addition, comparison Figure 1 and Figure 2 The particle shape and Figure 3 When the particle shape is obtained, Examples 1 to 3 prepared according to the present invention show that the particle size of the polyetherketoneketone increases. Therefore, it can be seen that the catalyst addition rate range of 1 to 10 g / min of the present invention is preferred, and it can be seen that when the catalyst is added at a rate of 1 to 10 g / min of the present invention for preparation, there is an effect of increasing the particle size.

[0101] Therefore, the method for preparing polyetherketoneketone of the present invention and the polyetherketoneketone prepared thereby inhibit the formation of scale by controlling the catalyst addition rate, thereby having the effect of improving the yield of polyetherketoneketone.

[0102] In addition, the polyetherketoneketone preparation method of the present invention and the polyetherketoneketone prepared thereby can prevent the agglomeration phenomenon between resin particles while maintaining the value of the intrinsic viscosity without significant change by adding a catalyst at a rate of 1 to 10 g / min to inhibit the formation of scale, thereby obtaining a high molecular weight polyetherketoneketone with a high yield, preferably a yield of more than 90%.

[0103] In addition, the polyetherketoneketone preparation method of the present invention and the polyetherketoneketone prepared thereby suppress the formation of scale by controlling the addition rate of the catalyst, increase the particle size, and thereby reduce the possibility of dust dispersion, thereby facilitating operation.

[0104] Furthermore, the method for producing polyetherketoneketone according to the present invention can obtain particles of various sizes at high yields by drying large particles of polyetherketoneketone obtained at high yields and then further pulverizing them.

[0105] The present invention has been described above through specific matters such as specific constituent elements and limited embodiments and drawings, but this is only used to help a more comprehensive understanding of the present invention. The present invention is not limited to the above-mentioned multiple embodiments, and those skilled in the art can make various modifications and variations based on these descriptions.

[0106] Therefore, the concept of the present invention is not limited to the embodiments described above, and the appended claims and all modifications equivalent to the claims belong to the scope of the concept of the present invention.

Claims

1. A method for preparing polyetherketoneketone, for obtaining polyetherketoneketone with a yield of more than 90%, characterized in that: The steps include: Step (a), in a reactor, adding at least one selected from diphenyl oxide and 1,4-bis(4-phenoxybenzoyl)benzene, terephthaloyl chloride and isophthaloyl chloride to a liquid reaction medium and dissolving them simultaneously to prepare a reaction solution; Step (b), cooling the reaction solution and adding a catalyst; as well as Step (c), after adding the catalyst, blowing inert gas directly into the reaction solution and stirring, wherein the catalyst is added at a rate of 1 to 1.5 g / min, The catalyst is aluminum chloride.

2. The method for preparing polyetherketoneketone according to claim 1, characterized in that: In the step (b), the cooling temperature is -10°C to -5°C.

3. The method for preparing polyetherketoneketone according to claim 1, characterized in that: A nozzle for directly blowing the inert gas into the reaction solution is formed at the upper part or the lower part of the reactor so as to be injected from multiple directions.

4. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The inert gas is at least one selected from nitrogen, helium, neon, argon and krypton.

5. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The step (c) comprises the step of raising the temperature of the reactor to 80° C. to 100° C. while stirring.

6. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The method comprises the step of washing with deionized water after step (c).

7. The method for preparing polyetherketoneketone according to claim 6, characterized in that: The method further comprises a step of vacuum drying at 170° C. to 190° C. after the water washing step.

8. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The reaction solution includes at least one end-capping agent selected from benzoyl chloride, benzenesulfonyl chloride, 4-chlorobiphenyl, 4-phenoxybenzophenone, 4-(4-phenoxyphenoxy)benzophenone, and biphenyl-4-phenylsulfonylphenyl ether.

9. The method for preparing polyetherketoneketone according to claim 1, characterized in that: The liquid reaction medium is at least one solvent selected from o-dichlorobenzene and dichloromethane.