A preparation method and application of propolis treated powder

By mixing propolis with solvent and performing surface treatment on the powder, the problem of difficulty in adding and dispersing propolis in cosmetic products is solved, the propolis-treated powder is evenly distributed and coated, and the antioxidant and anti-oxidation properties of the product are improved. The inflammatory effect and skin feel enhance the durability of the product.

CN115252527BActive Publication Date: 2024-10-29SHANGHAI CHUANGYUAN COSMETICS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210680968.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-15
Publication Date
2024-10-29
Estimated Expiration
2042-06-15

AI Technical Summary

Technical Problem

Propolis is difficult to add or disperse evenly in cosmetic products, especially products with a high powder content, which makes it difficult to exert its antioxidant, antibacterial and other effects, affecting the skin feel and durability of the product.

Method used

By mixing propolis with a solvent to form a solution, spraying and drying it evenly with the base powder in a mixer, and finally crushing it, the surface treatment of propolis is achieved and a propolis-treated powder that can be evenly distributed on the surface of the powder is formed.

Benefits of technology

It achieves uniform distribution and coating of propolis in the powder, improves the antioxidant and anti-inflammatory effects of the product, enhances adhesion and ductility, and provides a softer skin feel and long-lasting use effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115252527B_ABST
    Figure CN115252527B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of propolis treated powder, the preparation method comprising: step 1: mixing a certain proportion of propolis with a solvent to prepare a propolis solution; step 2: putting a basic powder into a mixer and mixing; step 3: spraying the propolis solution obtained in step 1 when mixing the basic powder, and mixing evenly; step 4: drying the treated powder obtained in step 3; step 5: crushing the dried powder in step 4 with a crusher to obtain a finished product. The embodiment of the present invention utilizes the multifunctional characteristics of propolis, and designs a treatment method that makes propolis disperse more evenly to cover the surface of the powder, and the obtained propolis treated powder has obvious skin nourishing, anti-oxidation and anti-inflammatory effects, and can achieve the characteristics of skin firming and wrinkle reduction after long-term use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cosmetics, and in particular to a preparation method of propolis treated powder and application thereof. Background Art

[0002] At present, as a huge branch of cosmetics, color cosmetics are widely welcomed by female consumers because of their functions of modifying the face, shaping the image, and covering blemishes. With the improvement of living standards, Chinese people are paying more and more attention to national color cosmetics for healthy skin care.

[0003] Propolis contains a large amount of physiologically active substances and trace elements, has a wide range of pharmacological effects, and has excellent antibacterial and antifungal properties. It is very suitable for therapeutic cosmetics. On the one hand, propolis contains flavonoids, aromatic oxidized heterocyclic compounds, including acacia, galangin, galangin, galangin, pinocytol and galangin. The above ingredients have the effects of promoting blood circulation, improving capillary vitality, and delaying skin aging. They are ideal additives for anti-wrinkle and anti-aging cosmetics; on the other hand, the vitamin E contained in propolis can protect unsaturated fatty acids and can also serve as an antioxidant to prevent damage caused by fatty acid oxides due to cell damage or enzyme inactivation; on the other hand, the flavonoids contained in propolis have good antioxidant properties and can be used in skin health care and hygiene to absorb oxygen free radicals and protect the skin. Currently, some skin care creams, shampoos, conditioners, sunscreen products and other skin care cosmetics on the market use propolis as a functional factor. However, since propolis is insoluble in water and general esters, its use in cosmetics development is limited. Color cosmetics, especially those with high powder content, want to add some natural skin care ingredients to the cosmetics, but it is difficult to add or disperse them evenly, which makes it technically difficult to achieve.

[0004] In the known prior art, propolis is used in skin care lotions or bath products, usually dispersed through a large amount of emulsifiers and ethanol, oils, to make emulsion products. However, in high-content powders in cosmetics, propolis is difficult to add and mix due to its insoluble properties in water and general esters. So far, there is no technical research or report in this regard. Summary of the invention

[0005] The present invention is made in view of the above-mentioned problems of the prior art, and its purpose is to use propolis to treat the surface of powder so as to meet the needs of cosmetic products with high powder content, while achieving antioxidant, anti-wrinkle, and anti-corrosion products, and a preparation method and application of propolis-treated powder that makes the product closer to the skin and more durable.

[0006] In order to solve the above problems in the prior art, the inventors have designed a method for preparing propolis treated powder after in-depth research. The technical solution is:

[0007] Step 1: Mix a certain proportion of propolis and a solvent to prepare a propolis solution;

[0008] Step 2: Add the base powder into the mixer and mix;

[0009] Step 3: Spray the propolis solution obtained in step 1 while mixing the base powder and mix well;

[0010] Step 4: Drying the treated powder obtained in step 3;

[0011] Step 5: Crush the dried powder from step 4 with a crusher to obtain a finished product.

[0012] As a preferred embodiment, when the propolis solution is prepared in step 1, it is stirred by a stirrer and heated to maintain a temperature of 25 to 90° C., and preferably 30 to 70° C.

[0013] As a preferred embodiment, in step 1, the ratio of propolis to the solvent is 1:1 to 1:100, and the ratio of propolis to the solvent is preferably 1:10 to 1:100, 1:20 to 1:100, 1:30 to 1:100, 1:40 to 1:100, 1:50 to 1:100, 1:60 to 1:100, 1:70 to 1:100, 1:80 to 1:100, 1:90 to 1:100, 1:1 to 1:90, 1:1 to 1:80, 1:1 to 1:70, 1:1 to 1:60, 1:1 to 1:50, 1:1 to 1:40, 1:1 to 1:30, 1:1 to 1:20, 1:1 to 1:10, and the more preferred ratio is 1:5 to 1:30.

[0014] The solvent in step 1 is at least one of alcohol, chloroform and ether, and the base powder in step 2 is a powder treated with triethoxyoctylsiloxane.

[0015] As a preferred embodiment, the solvent in step 1 is at least one of alcohol, chloroform and ether; or,

[0016] It is a mixture of alcohol and silicone coupling agent.

[0017] As a preferred embodiment, the silicon coupling agent is triethoxyoctylsiloxane, wherein the ratio of the alcohol to the triethoxyoctylsiloxane is 5:1-50:1; the preferred ratio is preferably 5:1-50:1, 10:1-50:1, 20:1-50:1, 30:1-50:1, 40:1-50:1, 1:1-10:1, 1:1-20:1, 1:1-30:1, 1:1-40:1, and the more preferred ratio is 10:1-30:1; further, the preferred ratio is 10:1-30:1. Specifically, the ratio of the solvent to the propolis needs to be limited, but the mass ratio of the propolis, the solvent mixture and the powder is not particularly limited.

[0018] As a preferred embodiment, the base powder in step 2 is at least one of inorganic powder, pearl powder, organic powder, organic pigment powder, and composite powder. Preferably, the base powder also includes one or more of inorganic plate-like powder and metal oxide, the inorganic plate-like powder also includes mica, talc, and calcium carbonate, and the metal oxide includes titanium oxide, zinc oxide, and iron oxide. Further, the iron oxide is one or more of FeO, Fe2O3, and Fe3O4.

[0019] As a preferred embodiment, the method for processing the powder obtained by drying step 3 in step 4 comprises:

[0020] Under vacuum, the treated powder mixture obtained in step 3 is mixed while removing the solvent, and taken out immediately when it becomes powder; or,

[0021] Under non-vacuum conditions, the treated powder mixture obtained in step 3 is heated and dried, and taken out immediately when it is dried into powder.

[0022] The technical solution of the present invention realizes heating and drying of the treated powder mixture obtained in step 3 by designing a drying method in a vacuum state and a non-vacuum state without a vacuum device.

[0023] As a preferred embodiment, the vacuum value in the vacuum drying state is 0.03Mpa to 0.08Mpa; in the non-vacuum state, the heating drying temperature is 20-160°C; the preferred temperature is 30-120°C.

[0024] The embodiment of the present invention also relates to the use of propolis treated powder in the preparation of cosmetics, wherein the cosmetics include any one of pressed powder, loose powder, foundation, lipstick, lip cream, eyebrow pencil, eyebrow powder and skin care lotion.

[0025] Among them, the preparation method of loose powder is: mix the weighed raw materials together according to a certain formula, then crush them with a powder grinder, and then mix the powders evenly to obtain; the preparation method of pressed powder is: mix the weighed raw materials together according to a certain formula, then crush them with a powder grinder, and then press them after mixing evenly to obtain.

[0026] The present invention uses a uniformly dissolved solution liquid obtained by mixing propolis with a solvent, and then uses the solution liquid to treat the powder to obtain the following beneficial effects:

[0027] 1. Propolis can be evenly distributed on the surface of the color powder under the carrier of the solvent to obtain a surface-coated powder with uniform properties and high quality. The time required for coating can be shortened through vacuum drying. At the same time, the obtained propolis-treated color powder has excellent hydrophobicity and can achieve a long-lasting color retention effect.

[0028] 2. The propolis treated powder obtained by the present invention has good adhesion and ductility on the skin, and has a softer and more advanced skin feel when used;

[0029] 3. Because propolis is coated on the surface of the powder, it can meet the basic functions of the powder while adding antioxidant, anti-inflammatory and other efficacy characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly understand the purpose, features and advantages of the present invention, the preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein:

[0031] Figure 1 The facial wrinkle image analysis diagram of the tester before and after using the propolis-treated powder provided in Example 19 to apply to the anhydrous powder product;

[0032] Figure 2 An image analysis diagram of facial wrinkles of a tester before and after using the propolis-treated powder provided in Example 20 to apply to an anhydrous powder product;

[0033] Figure 3 The facial wrinkle image analysis diagram of the tester before and after using the propolis-treated powder provided in Example 21 to apply to the anhydrous powder product;

[0034] Figure 4 Analysis chart of facial wrinkles of the tester before and after using the propolis treated powder provided in Example 22 to apply to the anhydrous powder product;

[0035] Figure 5 The figure is a test result diagram of the antibacterial test of Example 19;

[0036] Figure 6 The figure is a test result diagram of the antibacterial test of Example 20;

[0037] Figure 7 This is a test result diagram of the antibacterial test of Example 21;

[0038] Figure 8 This is a graph showing the test results of the antibacterial test on Example 22. DETAILED DESCRIPTION

[0039] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the present invention is further explained below in combination with specific text, graphic illustrations and specific embodiment descriptions.

[0040] Propolis is difficult to add or disperse evenly in cosmetic products, especially in formulas with high powder content, which results in the inability to fully exert the antioxidant / antibacterial effects of propolis, and the silky skin feel, water resistance and skin adhesion cannot be improved. In view of this, the technical personnel of this case have conducted repeated and in-depth discussions and studies in order to develop functional substances and powders suitable for cosmetics, and thus designed a method for preparing propolis-treated powder, so as to perform propolis surface treatment on the powder, and add the obtained treated powder to the cosmetic formula, so as to achieve antioxidant, anti-wrinkle and anti-corrosion effects while making the cosmetic products more skin-adherent and more durable. The technical solution of the preparation method of propolis-treated powder is:

[0041] Step 1: Mix a certain proportion of propolis and a solvent to prepare a propolis solution;

[0042] Step 2: Add the base powder into the mixer and mix;

[0043] Step 3: Spray the propolis solution obtained in step 1 while mixing the base powder and mix well;

[0044] Step 4: Drying the treated powder obtained in step 3;

[0045] Step 5: Crush the dried powder from step 4 with a crusher to obtain a finished product.

[0046] Wherein, when the propolis solution is configured in step 1, it is stirred by a stirrer and the temperature is maintained at 25 to 90° C. by heating. In step 1, the ratio of propolis to the solvent is 1:1 to 1:100 (mass ratio). Wherein, the ratio of propolis to the solvent is preferably 1:10 to 1:100, 1:20 to 1:100, 1:30 to 1:100, 1:40 to 1:100, 1:50 to 1:100, 1:60 to 1:100, 1:70 to 1:100, 1:80 to 1:100, 1:90 to 1:100, 1:1 to 1:90, 1:1 to 1:80, 1:1 to 1:70, 1:1 to 1:60, 1:1 to 1:50, 1:1 to 1:40, 1:1 to 1:30, 1:1 to 1:20, 1:1 to 1:10. More preferably, the ratio of propolis to solvent is 1:5 to 1:30.

[0047] In more detail, in one embodiment of the present invention, the solvent in step 1 is at least one of alcohol, chloroform and ether, and the base powder in step 2 is a powder treated with triethoxycaprylylsiloxane. That is, the powder treated with triethoxycaprylylsiloxane is then wrapped with propolis, and the specific wrapping method is:

[0048] 1. Use a blender to dissolve propolis in a solvent;

[0049] 2. Put the powder treated with triethoxycaprylylsiloxane into the mixer and mix;

[0050] 3. Spray the evenly dissolved propolis solution while mixing the powder to ensure that the material is fully mixed;

[0051] 4. Dry the powder;

[0052] 5. Crush the dry powder with a crusher;

[0053] In the above process 1, a mixing and stirring machine is used to stir and dissolve it uniformly. In order to increase the dissolution rate, it can be appropriately heated to 30-70°C. The solvents used in this embodiment are mainly alcohol, chloroform, and ether. The present invention mainly uses alcohol as a solvent. The powder treated with triethoxycaprylylsiloxane in process 2 is obtained by purchase.

[0054] In step 3, after 1 is dissolved evenly, it is sprayed on the powder of the mixer, and then mixed and sprayed. The powder used is not particularly limited, and is preferably selected from one or more powders of inorganic or organic powders treated with triethoxycaprylylsiloxane. For example, as the minerals and metal oxides used, mica, talc, silica, calcium carbonate, titanium oxide, zinc oxide and iron oxide (FeO, Fe2O3, Fe3O4 and mixtures thereof) treated with triethoxycaprylylsiloxane can be exemplified, and one or more of these powders can be used as needed. It should be noted that the ratio of solvent to propolis needs to be specifically limited. It is recommended that the ratio of propolis to alcohol is =1:1 to 1:100 (mass ratio), and the preferred ratio is 1:5-1:30, but the mass ratio of propolis, solvent mixture and powder is not particularly limited.

[0055] In the above step 4, the mixture in step 3 can be mixed while removing the solvent under a vacuum state, and taken out when it becomes powder. The vacuum state can be, for example, 0.03Mpa to 0.08Mpa. If the mixer does not have a vacuum device, the mixture is taken out and heated and dried. The heating temperature in this process is 20-160°C; preferably, the temperature is 30-120°C. In the above step 5, the powder coated with propolis is further dried, and the solid obtained is crushed with a crusher (crusher), thereby obtaining the propolis-treated triethoxycaprylylsiloxane-treated powder of the present invention.

[0056] In another embodiment of the present invention, the solvent in step 1 is at least one of alcohol, chloroform and ether; or a mixture of alcohol and a silicon coupling agent.

[0057] In the above embodiment, the silicon coupling agent is triethoxyoctylsiloxane, wherein the ratio of alcohol to triethoxyoctylsiloxane is 1:1-50:1 (mass ratio); further, the preferred ratio is preferably 5:1-50:1, 10:1-50:1, 20:1-50:1, 30:1-50:1, 40:1-50:1, 1:1-10:1, 1:1-20:1, 1:1-30:1, 1:1-40:1, and the more preferred ratio is 10:1-30:1. It can be understood that in the embodiment of the present invention, the ratio of solvent to propolis needs to be limited, but the mass ratio of propolis, solvent mixture and powder is not particularly limited.

[0058] In step 2 of the technical solution of the present invention: the base powder is at least one of inorganic powder, pearl powder, organic powder, organic pigment powder, and composite powder. In the embodiment of the present invention, the powder (base powder) to be surface treated is usually a powder commonly used in cosmetics, which is not subject to special restrictions such as spherical, flaky, needle-shaped shapes, nanometer or micrometer particle sizes, or porous, non-porous particle structures.

[0059] In the technical solution of the present invention, the surface-treated powder (base powder) is preferably inorganic powder such as inorganic powder, pearlescent inorganic powder and composite inorganic powder, and more preferably inorganic plate-like powder and metal oxide pigments such as titanium oxide, zinc oxide and iron oxide.

[0060] Among them, the above-mentioned inorganic powders can be one or more selected from titanium oxide, ultramarine, red iron oxide, yellow iron oxide, black iron oxide, zinc oxide, aluminum oxide, silicon dioxide, magnesium oxide, zirconium oxide, magnesium carbonate, calcium carbonate, chromium oxide, chromium hydroxide, carbon black, aluminum silicate, magnesium silicate, magnesium aluminum silicate, mica, synthetic mica, talc, kaolin, barium sulfate, bentonite, montmorillonite and boron nitride.

[0061] As the pearly inorganic powder, one or more selected from bismuth oxychloride, mica or synthetic mica coated with inorganic or organic colorants or pigments, glass powder coated with inorganic or organic colorants or pigments, and metal pearl powder can be used.

[0062] Among them, as the above-mentioned organic powder, one or more selected from nylon powder, polymethyl methacrylate powder, acrylonitrile-methacrylic acid copolymer powder, vinylidene chloride-methacrylic acid copolymer powder, PET resin powder, polyethylene powder, polystyrene powder, organic polysiloxane elastomer powder, polymethyl silsesquioxane powder, polyurethane powder, wool powder, silk powder, crystalline cellulose powder, etc. can be used.

[0063] As the pigment powders, one or more selected from organic tar pigments, lake pigments of organic pigments, and the like can be used.

[0064] In the technical solution of the present invention, the base powder also includes one or more of inorganic plate-like powder and metal oxide, the inorganic plate-like powder also includes mica, talc, calcium carbonate, and the metal oxide includes titanium oxide, zinc oxide, and iron oxide. Further, the iron oxide is one or more of FeO, Fe2O3, and Fe3O4.

[0065] In the above-mentioned embodiments, the powders to be surface treated are particularly suitable for plate-like inorganic powders such as talc and mica, and metal oxide pigments such as titanium oxide, zinc oxide, and iron oxide. For example, in the case of iron oxide, especially in the case of fine particles, it is easy to aggregate due to magnetism in the untreated state, but if the above-mentioned propolis is used as a surface treatment agent, the dispersibility of the surface-treated iron oxide becomes better, so it can effectively reduce or solve the risk of color banding that often occurs in cosmetics.

[0066] In the technical solution of the present invention, the method for treating the powder obtained by drying step 3 in step 4 comprises:

[0067] Under vacuum, the treated powder mixture obtained in step 3 is mixed while removing the solvent, and taken out immediately when it becomes powder; or,

[0068] Under non-vacuum conditions, the treated powder mixture obtained in step 3 is heated and dried, and taken out immediately when it is dried into powder.

[0069] That is, the technical solution of the present invention realizes heating and drying of the treated powder mixture obtained in step 3 by designing a drying method in a vacuum state and a non-vacuum state without a vacuum device. Wherein, the vacuum value in the vacuum drying state is 0.05Mpa to 0.08Mpa; in the non-vacuum state, the heating and drying temperature is 20-160°C; preferably, the temperature is 30-120°C.

[0070] The embodiment of the present invention also relates to the use of propolis treated powder in the preparation of cosmetics, wherein the cosmetics include any one of pressed powder, loose powder, foundation, lipstick, lip cream, eyebrow pencil, eyebrow powder and skin care lotion.

[0071] Among them, the preparation method of loose powder is: mix the weighed raw materials together according to a certain formula, then crush them with a powder grinder, and then mix the powders evenly to obtain; the preparation method of pressed powder is: mix the weighed raw materials together according to a certain formula, then crush them with a powder grinder, and then press them after mixing evenly to obtain.

[0072] Hereinafter, the present invention will be specifically described by way of Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0073] The technical solution of the present invention provides multiple embodiments of a method for preparing propolis treated powder in treatment mode 1 (the ratio not specifically stated in this embodiment is the mass ratio), which specifically includes the following:

[0074] Embodiment 1:

[0075] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0076] (2) Add 95 g of red iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0077] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0078] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0079] Embodiment 2:

[0080] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0081] (2) Add 95 g of yellow iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0082] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0083] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0084] Embodiment 3:

[0085] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0086] (2) Add 95 g of black iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes;

[0087] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0088] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0089] Embodiment 4:

[0090] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0091] (2) Add 95 g of titanium dioxide color powder into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolving solution. The spraying takes about 5 minutes.

[0092] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0093] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0094] Embodiment 5:

[0095] (1) Heat 2 g of propolis and 20 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0096] (2) Add 98 g of talcum powder into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0097] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0098] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, heating the powder to 100° C. to dry the powder; after drying for 5 hours, cooling the powder to 30° C. to obtain propolis-treated talc powder.

[0099] Embodiment 6:

[0100] (1) Heat 3 g of propolis and 17 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed solution, and put it into an oil tank with a spray device;

[0101] (2) Add 97 g of silica into the mixer, maintain the vacuum degree in the mixer at 0.05 MPa, stir at 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0102] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0103] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the powder; after drying for 4.5 hours, lowering the temperature to 30° C. to obtain propolis-treated silica powder.

[0104] The technical solution of the present invention provides multiple embodiments of a method for preparing propolis treated powder obtained by treatment method 2, which specifically include the following:

[0105] Embodiment 7:

[0106] (1) 5 g of propolis, 10 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed evenly to form a uniformly dissolved mixed liquid, which is then put into an oil tank with a spraying device;

[0107] (2) Add 95 g of red iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0108] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0109] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0110] Embodiment 8:

[0111] (1) 5 g of propolis, 10 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed evenly to form a uniformly dissolved mixed liquid, which is then put into an oil tank with a spraying device;

[0112] (2) Add 95 g of yellow iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0113] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0114] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0115] Embodiment 9:

[0116] (1) 5 g of propolis, 10 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed evenly to form a uniformly dissolved mixed liquid, which is then put into an oil tank with a spraying device;

[0117] (2) Add 95 g of black iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes;

[0118] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0119] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0120] Embodiment 10:

[0121] (1) 5 g of propolis, 10 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed evenly to form a uniformly dissolved mixed liquid, which is then put into an oil tank with a spraying device;

[0122] (2) Add 95 g of titanium dioxide color powder into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolving solution. The spraying takes about 5 minutes.

[0123] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0124] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0125] Embodiment 11:

[0126] (1) 2 g of propolis, 15 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed to obtain a uniformly dissolved mixed solution, which is then poured into an oil tank equipped with a spraying device;

[0127] (2) Add 98 g of talcum powder into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0128] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0129] (4) maintaining a vacuum degree of 0.05 MPa, stirring at a speed of 300 rpm, heating to 100° C. to dry the powder, and after drying for 5 hours, cooling to 30° C. to obtain propolis-treated talc;

[0130] (5) Sampling and testing: Propolis treated talcum powder and deionized water were mixed in a ratio of 1:99, and shaken at 25°C and 240 rpm for three minutes using a high-speed constant temperature incubator shaker. After 30 minutes, the color powder did not sink to the bottom and the phases were clear. The product was judged to be qualified as C.

[0131] Embodiment 12:

[0132] (1) 3 g of propolis, 12 g of alcohol and 5 g of triethoxycaprylylsiloxane are heated to 30-50° C. and mixed to obtain a uniformly dissolved mixed solution, which is then put into an oil tank equipped with a spraying device;

[0133] (2) Add 97 g of silica into the mixer, maintain the vacuum degree in the mixer at 0.05 MPa, stir at 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0134] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0135] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the powder; after drying for 4.5 hours, lowering the temperature to 30° C. to obtain propolis-treated silica powder.

[0136] Embodiment 13

[0137] (1) Mix 5 g of propolis and 15 g of alcohol and heat at 30-50°C to make a uniformly dissolved mixed solution, and put it into an oil tank with a spray device;

[0138] (2) Add 95 g of triethoxycaprylylsiloxane-treated red iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0139] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0140] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0141] Embodiment 14:

[0142] (1) Mix 5 g of propolis and 15 g of alcohol and heat at 30-50°C to make a uniformly dissolved mixed solution, and put it into an oil tank with a spray device;

[0143] (2) Add 95 g of triethoxycaprylylsiloxane-treated yellow iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0144] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0145] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0146] Embodiment 15:

[0147] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0148] (2) Add 95 g of triethoxycaprylylsiloxane-treated black iron oxide into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0149] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0150] (4) maintaining a vacuum degree of 0.05 MPa, stirring at a speed of 300 rpm, heating to 100° C. to dry the toner, and then cooling to 30° C. after drying for 4 hours to obtain propolis treated toner

[0151] Embodiment 16:

[0152] (1) Heat 5 g of propolis and 15 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0153] (2) Add 95 g of triethoxycaprylylsiloxane titanium dioxide toner into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0154] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 20 minutes;

[0155] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the color powder; after drying for 4 hours, lowering the temperature to 30° C. to obtain the propolis-treated color powder.

[0156] Embodiment 17:

[0157] (1) Heat 2 g of propolis and 20 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed liquid, and put it into an oil tank with a spray device;

[0158] (2) Add 98 g of triethoxycaprylylsiloxane talc into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0159] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0160] (4) maintaining a vacuum degree of 0.05 MPa, stirring at a speed of 300 rpm, heating to 100° C. to dry the powder, and after drying for 5 hours, cooling to 30° C. to obtain propolis-treated talc;

[0161] Embodiment 18:

[0162] (1) Heat 3 g of propolis and 17 g of alcohol at 30-50°C and mix them evenly to make a uniformly dissolved mixed solution, and put it into an oil tank with a spray device;

[0163] (2) Add 97 g of triethoxyoctylsiloxane-treated silica into the mixer, maintain a vacuum degree of 0.05 MPa in the mixer, stir at a speed of 150 rpm, and slowly spray the dissolved solution. The spraying takes about 5 minutes.

[0164] (3) After the solution is sprayed, maintain the vacuum degree at 0.05 MPa, increase the stirring speed to 300 rpm, and continue stirring for 30 minutes;

[0165] (4) maintaining a vacuum degree of 0.05 MPa and a stirring speed of 300 rpm, raising the temperature to 100° C. to dry the powder; after drying for 4.5 hours, lowering the temperature to 30° C. to obtain propolis-treated silica powder.

[0166] Under the same other conditions, the propolis-treated powders obtained in Examples 1-6, Examples 7 to 12, and Examples 13-18 and the silicon-treated powders commonly found in the market are applied to water-free cosmetic powder blocks, and after simultaneous proofing, they are distributed to consumers for use. For details, see the following examples.

[0167] The silicon-treated powder used in the embodiment of the present invention is the surface-treated powder of Shanghai Yirong Yumei Biotechnology Co., Ltd., and the iron oxide red is YRIOR 4001AS / the iron oxide yellow is YRIOY 4002AS / the iron oxide black is YRIOB 4001AS / the titanium dioxide is YRTI 4001AS / the talc is YRTA2001AS / the silica is YRSI 3001AS.

[0168] Embodiment 19:

[0169] Itemization name Ratio (mass percentage) A1 Propolis treated iron oxide red 0.1 A2 Propolis treated iron oxide yellow 0.05 A3 Propolis treated iron oxide black 0.45 A4 Propolis treated with titanium dioxide 5 A5 Propolis treated talc 83.7 A6 Propolis treated silica 3 B1 Dimethicone 4 B2 Diisostearyl Malate 3 B3 Polyhydroxystearic acid 0.3 C Phenoxyethanol 0.4 total 100

[0170] Table 1 Application of propolis treated powder to water-free cosmetic powder block formula Example 20:

[0171]

[0172]

[0173] Table 2 Triethoxycaprylylsiloxane treated powder applied to water-free makeup powder block formula Example 21:

[0174]

[0175]

[0176] Table 3 Application of propolis and triethoxycaprylylsiloxane treated powder to water-free makeup powder block formula Example 22

[0177] Itemization name Ratio (mass percentage) A1 Propolis, triethoxycaprylylsiloxane treated with red iron oxide 0.1 A2 Propolis, triethoxycaprylylsiloxane treated iron oxide yellow 0.05 A3 Propolis, triethoxycaprylylsiloxane treated with black iron oxide 0.45 A4 Propolis, triethoxycaprylylsiloxane treated titanium dioxide 5 A5 Propolis, triethoxycaprylylsiloxane treated talc 83.7 A6 Propolis, Silica Treated with Triethoxycaprylylsiloxane 3 B1 Dimethicone 4 B2 Diisostearyl Malate 3 B3 Polyhydroxystearic acid 0.3 C Phenoxyethanol 0.4 total 100

[0178] Table 4 Application of propolis-treated triethoxycaprylylsiloxane-treated powder to water-free makeup powder block formula

[0179] The method for obtaining a water-free makeup powder block formula according to the formula of each ingredient in each table in Examples 19 to 22 comprises:

[0180] 1. First, mix and grind phase A (0.1% of treated iron oxide red, 0.05% of treated iron oxide yellow, 0.45% of treated iron oxide black, 5% of treated titanium dioxide, 83.7% of treated talc, and 3% of treated silica) using a powder grinder;

[0181] 2. Mix the BC phase (4% dimethicone, 3% diisostearyl malate, 0.3% polyhydroxystearic acid and 0.4% phenoxyethanol) evenly, and spray it in a mixer to mix evenly;

[0182] 3. Pass through 80 mesh sieve;

[0183] 4. The sieved material is placed in an aluminum pan and pressed at a pressure of 20 kg to obtain a water-free makeup powder block.

[0184] The products obtained by the above method in Example 19, Example 20, Example 21 and Example 22 were distributed to 25 female consumers for use, and smear tests and instrument tests were performed during use.

[0185] In this example, all the above consumers use the product according to the same specifications, cooperate with the staff to complete the evaluation work as required, have certain expression ability, and can truly reflect their feelings after use.

[0186] 25 professional cosmetics evaluation panel members were selected to conduct the test, and consumers were asked to rate the smoothness, spreadability, skin adhesion and durability of the products according to the evaluation criteria in the table below (the highest is 10 points and the lowest is 1). The average score of each indicator from all panel members was then calculated and judged based on the excellent, good, fair, and poor criteria.

[0187] index Embodiment 19 Embodiment 20 Embodiment 21 Embodiment 22 Smoothness 7 points 7 points 8 points 8 points Ductility 8 points 7 points 9 points 9 points Skin-friendly 7 points 6 points 9 points 9 points Persistence 8 points 5 points 9 points 9 points evaluate good medium excellent excellent

[0188] Table 5 Product test index scores and evaluation criteria

[0189] According to Table 5, it can be seen that from the perspective of performance, the powder treated with propolis and triethoxycaprylylsiloxane has the best effect.

[0190] The products obtained in Examples 19, 20, 21 and 22 were subjected to an impact resistance test. The aforementioned impact resistance verification mainly tests the falling property of the powder blocks. The relevant operation steps include: dropping the products in Examples 19, 20, 21 and 22 on a PVC board at a distance of 50 cm to observe whether the impact resistance of the powder blocks is OK. It was found that the product in Example 19 broke after 15 impacts, while the product in Example 20 broke after 5 impacts, and the products in Examples 21 and 22 broke after more than 25 impacts. The above content indicates that the impact resistance of the powder blocks treated with propolis is also improved, and the effect of treating with propolis and triethoxycaprylylsiloxane is better.

[0191] Since anti-oxidation is related to skin aging, two testers were selected to conduct aging tests on the products of Example 19, Example 20, and Examples 21 and 22. The relevant process was as follows: before the test, facial wrinkles were observed and recorded using a facial graphic analyzer. At the same time, after using the product for 1 month, the facial wrinkles were observed and recorded again using a facial image analyzer. The testers were compared to see whether their facial wrinkles were alleviated before and after using the product. Figures 1 to 4 It can be seen that the product of Example 20 has the least obvious wrinkle improvement effect.

[0192] The products of Example 19, Example 20, Example 21 and Example 22 were tested for antibacterial properties. The relevant steps included: conducting an antiseptic challenge test on the powder by inoculating the powder with the bacterial solution. Figures 5 to 8 The product test results of Example 19, Example 20 and Example 21 are shown in FIG. Figures 5 to 8 It can be seen that the products of Examples 19 and 21 passed the anti-corrosion challenge, but Example 20 failed the anti-corrosion challenge. At the same time, the anti-corrosion effects of Examples 21 and 22 were Figures 5 to 8 It can be seen that the effect is best.

[0193] More specifically, according to Figures 5 to 8 It can be seen that: when the inoculation amount is constant, on the 7th day, all the bacteria inoculated in Examples 21 and 22 are gone, and the bacteria in Example 19 also decreases significantly, but although there is a decrease in Example 20, the decrease is relatively low. This can be reflected from another aspect: the powder treated with propolis has an antibacterial effect, but the effect of using propolis and triethoxycaprylylsiloxane is better; it can be understood that under the same conditions, the amount of preservatives in the product can be reduced.

[0194] The embodiment of the present invention also relates to the use of propolis treated powder in the preparation of cosmetics.

[0195] The powder obtained in the aforementioned embodiments treated with propolis or propolis and triethoxycaprylylsiloxane can be used in pressed powders as well as in formulations of loose powder, foundation, lipstick, skin care lotion, etc. However, it can be understood that the application of the propolis treated powder is not limited to the aforementioned products.

[0196] This paper adopts propolis treated powder and propolis and triethoxyoctylsiloxane treated powder. The obtained propolis treated powder has the following advantages compared with the powder in the prior art:

[0197] (1) Silky or smooth skin feel;

[0198] (2) Water-resistant, oil-resistant or friction-resistant;

[0199] (3) It has the effect of improving skin adhesion;

[0200] (4) It has good powder aggregation effect;

[0201] (5) It has good antioxidant and antibacterial effects;

[0202] Studies have found that powder treated with propolis and triethoxycaprylylsiloxane has stronger characteristics than powder treated with propolis alone, that is, the powder treated with the combination of propolis and triethoxycaprylylsiloxane has more obvious antioxidant and antibacterial effects.

[0203] Furthermore, the present invention uses a uniformly dissolved solution liquid obtained by mixing propolis with a solvent, and then uses the solution liquid to treat the powder to obtain the following beneficial effects:

[0204] 1. Propolis can be evenly distributed on the surface of the color powder under the carrier of the solvent to obtain a surface-coated powder with uniform properties and high quality. The time required for coating can be shortened through vacuum drying. At the same time, the obtained propolis-treated color powder has excellent hydrophobicity and can achieve a long-lasting color retention effect.

[0205] 2. The propolis treated powder obtained by the present invention has good adhesion and ductility on the skin, and has a softer and more advanced skin feel when used;

[0206] 3. Because propolis is coated on the surface of the color powder, it can meet the basic functions of the color powder while adding better effects such as anti-oxidation and anti-inflammatory.

[0207] In summary, the embodiments of the present invention utilize the multifunctional characteristics of propolis and design a processing method to make propolis dispersed more evenly to cover the surface of the powder. The obtained propolis-treated powder has obvious skin-nourishing, anti-oxidation and anti-inflammatory effects. Long-term use can achieve the characteristics of firming the skin and reducing wrinkles.

[0208] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing propolis treated powder, characterized in that: It includes the following steps: Step 1: Mix a certain proportion of propolis and a solvent to prepare a propolis solution; Step 2: Add the base powder into the mixer and mix; Step 3: Spray the propolis solution obtained in step 1 while mixing the base powder and mix well; Step 4: Drying the treated powder obtained in step 3; Step 5: crush the dry powder obtained in step 4 with a crusher to obtain a finished product; Wherein, when the propolis solution is prepared in step 1, it is stirred by a stirrer and the temperature is maintained at 25°C to 90°C by heating; the mixing in step 3 is carried out under reduced pressure conditions; the solvent in step 1 is at least one of alcohol, chloroform and ether, and the ratio of propolis to the solvent is 1:1 to 1:100; the base powder in step 2 is a powder treated with triethoxyoctylsiloxane.

2. The method for preparing propolis treated powder according to claim 1, characterized in that: The solvent in step 1 is a mixture of alcohol and a silicon coupling agent.

3. The method for preparing propolis treated powder according to claim 2, characterized in that: The silicon coupling agent is triethoxyoctylsiloxane, wherein the ratio of the alcohol to the triethoxyoctylsiloxane is 1:1 to 50:

1.

4. The method for preparing propolis treated powder according to claim 3, characterized in that: In step 2, the base powder is at least one of inorganic powder, organic powder and composite powder.

5. The method for preparing propolis treated powder according to claim 1, characterized in that: The method for treating the powder obtained by drying step 3 in step 4 comprises: Under vacuum, the treated powder mixture obtained in step 3 is mixed while removing the solvent, and taken out immediately when it becomes powder; Alternatively, the treated powder mixture obtained in step 3 is heated and dried under non-vacuum conditions, and taken out immediately when it is dried into powder.

6. The method for preparing propolis treated powder according to claim 5, characterized in that: The vacuum value under vacuum drying state is 0.03Mpa-0.08Mpa; under non-vacuum state, the heating drying temperature is 20-160℃.

7. Use of the propolis-treated powder obtained by the preparation method according to any one of claims 1 to 6 in the preparation of cosmetics, wherein the cosmetics comprise: Any of pressed powder, loose powder, foundation, lipstick, lip cream, eyebrow pencil, eyebrow powder, and skin care lotion.

Citation Information

Patent Citations

  • Brazilian green propolis powder and its preparation method

    CN109260234A

  • Cosmetic composition containing propolis extract

    CN110251448A

  • Cosmetic composition comprising cosmetic capsules into which water-soluble extract is absorbed

    CN113286574A

  • Modified powder and preparation method thereof, and cosmetic containing modified powder

    CN114224747A

  • Method for extracting propolis and water soluble dry propolis powder obtained thereby and cosmetic and pharmaceutical preparations containing same

    EP0109993A1