A nickel-iron-based electrocatalyst for alkaline high current oxygen evolution and a preparation method thereof

By using foam nickel hydrothermal solution in electrochemical water decomposition technology to prepare nickel hydrated molybdate and perform impregnation and cyclic voltammetry treatment, a nickel-iron-based electrocatalyst is formed, which solves the high energy consumption of oxygen evolution reaction and catalyst self-reconstruction in the prior art. The problem of incompleteness has achieved efficient and low-cost electrolysis of water and hydrogen production.

CN115261920BActive Publication Date: 2024-11-08TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210845144.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-19
Publication Date
2024-11-08
Estimated Expiration
2042-07-19

AI Technical Summary

Technical Problem

In the existing electrochemical water decomposition technology, the high energy consumption of oxygen evolution reaction (OER) limits the efficiency and cost of hydrogen production by electrolyzing water. Especially under high current density, the incomplete self-reconstitution of NiFe-based catalysts leads to insufficient catalytic activity. .

Method used

Using nickel foam as the base material to prepare nickel molybdate hydrated by one step hydrothermal, then impregnation treatment forms a nickel-iron-based precatalyst, and a nickel-iron-based electrocatalyst is obtained through cyclic voltammetry treatment, retaining the rod-like structure and active sites, achieving rapid Completely self-reconstructed.

Benefits of technology

Highly active sites and excellent oxygen evolution activity are obtained, which can stably drive the oxygen evolution reaction with a high current density for a long time at low overpotentials, reducing the preparation cost and improving the efficiency of hydrogen production by electrolyzing water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115261920B_ABST
    Figure CN115261920B_ABST
Patent Text Reader

Abstract

The present invention discloses a nickel-iron-based electrocatalyst for alkaline high current oxygen evolution. The nickel-iron-based electrocatalyst uses foamed nickel as a base material, obtains hydrated nickel molybdate through a one-step hydrothermal treatment, obtains a nickel-iron-based precatalyst through an impregnation treatment, and finally obtains the nickel-iron-based electrocatalyst through 20 cycles of cyclic voltammetry treatment. The present invention provides a design concept for a low-cost, high-activity oxygen evolution electrocatalyst. The nickel-iron-based electrocatalyst prepared by the present invention has abundant active sites and excellent oxygen evolution activity, and exhibits good durability and low oxygen evolution overpotential under long-term alkaline high current conditions. The preparation method can introduce different anions, and has great potential application value and broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electrocatalytic material and belongs to the technical field of preparation of oxygen evolution electrocatalysts, in particular to a nickel-iron based electrocatalyst for alkaline large current oxygen evolution and a preparation method thereof. Background Art

[0002] Hydrogen energy is considered a promising renewable energy carrier and alternative to fossil fuels due to its high energy density (142MJ / kg) and zero emissions during combustion. Using green electricity such as solar energy and wind energy to produce hydrogen by electrolysis of water is a very promising green hydrogen production method. Among the many water electrolysis technologies, alkaline water electrolysis technology has been commercialized for more than 100 years and is the most mature and economical technology. However, due to the high energy consumption of the oxygen evolution reaction (OER), today's electrochemical water splitting can only meet 4% of the world's hydrogen. Therefore, efficient OER catalysts play an important role in improving hydrogen production efficiency and reducing costs.

[0003] Among many catalysts, precious metal oxides have good OER catalytic activity, but their limited storage, high price and poor stability lead to very limited practical application prospects. At present, iron-based metal catalysts, especially NiFe-based catalysts, are expected to replace them due to their high intrinsic activity, including sulfide selenides, phosphides, borides, (hydr)oxides, etc. Although NiFe-based electrocatalysts have made great progress in recent years, most of these catalysts can only drive the OER process at a small current density, and large-scale production requires the catalyst to be at 500mA / cm 2 , even 1000mA / cm 2 Therefore, developing and designing catalysts with good OER performance at high current density to achieve cheap and efficient hydrogen production by water electrolysis is a problem that needs to be solved urgently in the field of water electrolysis hydrogen production.

[0004] In recent years, a series of studies have shown that NiFe-based metal (hydride) oxides, chalcogenides, phosphides and borides are not the real oxygen evolution active phases, but NiFeOOH converted in situ during the oxygen evolution process is the real active substance. However, most of the current OER precatalysts undergo slow or incomplete self-reconstruction to produce real active sites. Therefore, by designing a precatalyst that can quickly and completely self-reconstruct, thereby obtaining the real catalyst NiFeOOH enriched with exposed active sites, it will help to achieve high current density oxygen evolution and the development of cheap and efficient water electrolysis hydrogen production technology. Summary of the invention

[0005] In view of the deficiencies in the prior art and the needs of research and application in this field, the present invention aims to provide a nickel-iron based electrocatalyst for alkaline large current oxygen evolution.

[0006] The present invention is achieved by adopting the following technical solutions:

[0007] A nickel-iron based electrocatalyst for alkaline large current oxygen evolution, wherein the nickel-iron based electrocatalyst uses foamed nickel as a base material, undergoes a one-step hydrothermal treatment to obtain hydrated nickel molybdate, undergoes an impregnation treatment to obtain a nickel-iron based precatalyst, and finally undergoes 20 cycles of cyclic voltammetry treatment to obtain the nickel-iron based electrocatalyst.

[0008] The method for preparing the nickel-iron-based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0009] (1) Dissolve nickel nitrate and ammonium molybdate in deionized water, then add ammonia water to adjust the pH to ≤5.2, then transfer to a polytetrafluoroethylene autoclave and add the treated nickel foam, and perform hydrothermal reaction at 150°C for 6-7 hours; after naturally cooling to room temperature, wash with deionized water and ethanol several times, and vacuum dry to obtain a hydrated nickel molybdate precatalyst;

[0010] (2) immersing the hydrated nickel molybdate obtained in step (1) in a mixed solution containing iron ions and different anions, or alternately immersing it in solutions containing iron ions and different anions, or immersing it in a ferric chloride solution, repeating the process several times, taking it out and drying it at 80° C. for 1 to 2 hours, washing it with deionized water and ethanol several times, and vacuum drying it to obtain a nickel-iron-based precatalyst;

[0011] (3) The nickel-iron-based precatalyst obtained in step (2) was subjected to cyclic voltammetry treatment 20 times in 1 mol / L potassium hydroxide to obtain a nickel-iron-based electrocatalyst.

[0012] Further preferably, the ammonium molybdate is ammonium heptamolybdate, and the pH is 5.2. The rod-shaped hydrated nickel molybdate structure is formed by larger molybdate oxyanions. In a reaction system with a pH of 5.2, the larger heptamolybdate is more stable, while in a 1 mol / L potassium hydroxide, larger molybdates such as heptamolybdate anions are unstable and more easily leached, forming larger vacancies, thereby enabling rapid deep reconstruction.

[0013] Further preferably, the molar ratio of the nickel nitrate to ammonium molybdate is 4:1.

[0014] Further preferably, the iron source may be any soluble iron salt.

[0015] Further preferably, the solubility of the solution containing iron ions is 0.05-0.5 mol / L.

[0016] Further preferably, the different anion sources are sodium borohydride, potassium dihydrogen phosphate, sodium thiosulfate or selenious acid.

[0017] Further preferably, the range of the cyclic voltammetry scan is 0.1-1.9 V (V vs. Hg / HgO).

[0018] In addition, the nickel-iron based electrocatalyst of the present invention is applied to the alkaline high current density anode oxygen evolution reaction.

[0019] The present invention provides a method for designing a low-cost, high-activity oxygen evolution electrocatalyst. The nickel-iron-based electrocatalyst prepared by the method has abundant active sites and excellent oxygen evolution activity, and exhibits good durability and low oxygen evolution overpotential under long-term alkaline high current conditions.

[0020] Compared with the prior art, the present invention has the following main advantages and beneficial effects:

[0021] 1. The hydrated nickel molybdate of the present invention has a unique rod-like structure with a high aspect ratio and can be quickly and completely self-reconstructed into a truly active phase, and can be used as an excellent template for nickel-based catalysts. And by loading different iron-based materials, nickel-iron-based electrocatalysts modified with different anions can be finally obtained.

[0022] 2. The nickel-iron-based electrocatalyst described in the present invention is obtained by rapid reconstruction, retaining the three-dimensional rod-like structure of the pre-catalyst, and the surface morphology is further optimized, so that it has abundant exposed active sites and high intrinsic activity, and is conducive to the transfer of electrons and protons.

[0023] 3. The nickel-iron-based electrocatalyst described in the present invention has excellent oxygen evolution catalytic performance and can stably drive the oxygen evolution reaction with a large current density for a long time at a low overpotential.

[0024] 4. The preparation method of the electrocatalyst described in the present invention has simple process, convenient operation and is easy for large-scale production.

[0025] The invention has reasonable design, and the preparation method can introduce different anions, and has great potential application value and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The scanning electron microscope image of NiMoO obtained in Example 1 is shown.

[0027] Figure 2 This is a scanning electron microscope image of NiMoO / FeB obtained in Example 1.

[0028] Figure 3 This is a scanning electron microscope image of SR-NiMoO / FeB obtained in Example 1.

[0029] Figure 4 The X-ray diffraction spectrum of SR-NiMoO / FeB obtained in Example 1 is shown.

[0030] Figure 5The Raman spectrum of SR-NiMoO / FeB obtained in Example 1 is shown.

[0031] Figure 6 The linear voltammetric curve (1 mol / L potassium hydroxide) of the oxygen evolution performance test of SR-NiMoO / FeB obtained in Example 1 is shown.

[0032] Figure 7 The stability test curve of SR-NiMoO / FeB obtained in Example 1 is shown.

[0033] Figure 8 The linear voltammetric curve of SR-NiMoO / FeB obtained in Example 1 after the stability test is shown.

[0034] Fig. 9 The linear voltammetric curve (1 mol / L potassium hydroxide) of the oxygen evolution performance test of SR-NiMoO / FePO obtained in Example 2 is shown.

[0035] Fig.10 The figure shows the linear voltammetric curve (1 mol / L potassium hydroxide) of the oxygen evolution performance test of SR-NiMoO / FeSO obtained in Example 3.

[0036] Fig.11 The linear voltammetric curve (1 mol / L potassium hydroxide) of the oxygen evolution performance test of SR-NiMoO / FeSeO obtained in Example 4 is shown.

[0037] Fig.12 The linear voltammetric curve (1 mol / L potassium hydroxide) of the oxygen evolution performance test of SR-NiMoO / FeClO obtained in Example 5 is shown. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the present invention more clear, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, but are not limited thereto. The raw materials used in the embodiments are all common commercial products unless otherwise specified; the methods used are all commonly used methods in the art unless otherwise specified.

[0039] Example 1

[0040] A method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0041] (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium molybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.2. The mixture was then transferred to a 100 mL polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst (denoted as NiMoO).

[0042] (2) The NiMoO obtained in step (1) was alternately immersed in 15 mL of 0.5 mol / L ferric chloride solution and 15 mL of sodium hydroxide solution containing 1.5 mol / L sodium borohydride (wherein the concentration of sodium hydroxide was 0.25 mol / L to prevent hydrolysis of sodium borohydride) for 10 s each, and the mixture was repeated twice. The mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a nickel-iron based precatalyst (denoted as NiMoO / FeB).

[0043] (3) The NiMoO / FeB obtained in step (2) was subjected to 20 cyclic voltammetry treatments in 1 mol / L potassium hydroxide, with a voltage range of 0.1-1.9 V (V vs. Hg / HgO), and finally the corresponding genuine nickel-iron-based catalyst (denoted as SR-NiMoO / FeB) was obtained.

[0044] The scanning electron microscope photograph of the NiMoO precatalyst prepared in Example 1 is as follows Figure 1 As shown by Figure 1 It can be seen that the prepared NiMoO precatalyst has a unique rod-like structure with a high aspect ratio.

[0045] The scanning electron microscope photograph of the NiMoO / FeB precatalyst prepared in Example 1 is as follows Figure 2 As shown by Figure 2 It can be demonstrated that FeB nanoparticles are successfully loaded on the NiMoO surface.

[0046] The scanning electron microscope photograph of the SR-NiMoO / FeB electrocatalyst prepared in Example 1 is as follows Figure 3 As shown by Figure 3 It can be seen that the prepared SR-NiMoO / FeB electrocatalyst retains the rod-like structure and forms a nanoflower-like structure on the surface, which can provide a large electrochemically active surface area and is beneficial to the electron / proton transfer process.

[0047] The X-ray diffraction spectra of the NiMoO / FeB and SR-NiMoO / FeB electrocatalysts prepared in Example 1 are shown in Figure 4 As shown by Figure 4It can be seen that the characteristic peaks of NiMoO / FeB completely correspond to those of hydrated nickel molybdate, and the characteristic peaks of SR-NiMoO / FeB obtained by cyclic voltammetry treatment correspond to those of NiOOH (PDF#06-0075).

[0048] The Raman spectra of the NiMoO / FeB and SR-NiMoO / FeB electrocatalysts prepared in Example 1 are shown in Figure 5 As shown by Figure 5 It can be seen that the Raman peak of NiMoO / FeB completely corresponds to the characteristic peak of hydrated nickel molybdate. After cyclic voltammetry treatment, 473 cm -1 and 555cm -1 The peak at 680 cm-1 corresponds to the vibration of the Ni-O bond in NiOOH. -1 The corresponding position is Fe-O bond, 1054 cm -1 The position corresponds to the MO-O bond, which further illustrates that the cyclic voltammetry process completely reconstructs the NiFe-based pre-catalyst into a true NiFe-based electrocatalyst (NiFeOOH).

[0049] The oxygen evolution performance test curve of the SR-NiMoO / FeB electrocatalyst prepared in Example 1 is as follows: Figure 6 As shown by Figure 6 It can be seen that the prepared nickel-iron-based electrocatalyst only needs 166mV and 213mV to reach 10mA / cm 2 and 100mA / cm 2 The current density can be driven at 500 mA / cm at overpotentials of 277 mV and 315 mV. 2 and 1000mA / cm 2 of high current density.

[0050] The SR-NiMoO / FeB electrocatalyst prepared in Example 1 was 2 The stability test curve and the linear voltammetric curve after the test are as follows: Figure 7 and Figure 8 As shown by Figure 7 and Figure 8 It can be seen that the prepared nickel-iron-based electrocatalyst can stably drive the oxygen evolution reaction at a high current density for a long time.

[0051] Example 2

[0052] A method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0053] (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium molybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.2. The mixture was then transferred to a 100 mL polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst (denoted as NiMoO).

[0054] (2) The NiMoO obtained in step (1) was alternately immersed in 15 mL of a 0.1 mol / L ferric chloride solution and 15 mL of a 0.1 mol / L potassium dihydrogen phosphate solution for 10 s each, and the mixture was repeated 8 times. After being taken out, the mixture was dried at 80° C. for 1 h, washed with deionized water and ethanol several times, and vacuum dried to obtain a nickel-iron-based precatalyst (denoted as NiMoO / FePO).

[0055] (3) The NiMoO / FeB obtained in step (2) was subjected to cyclic voltammetry treatment 20 times in 1 mol / L potassium hydroxide, with a voltage range of 0.1-1.9 V (V vs. Hg / HgO), and finally the corresponding genuine nickel-iron-based catalyst (denoted as SR-NiMoO / FePO) was obtained.

[0056] The oxygen evolution performance test curve of the SR-NiMoO / FePO electrocatalyst prepared in Example 2 is as follows: Fig. 9 As shown by Fig. 9 It can be seen that the prepared nickel-iron-based electrocatalyst only needs an overpotential of 305mV to drive 1000mA / cm 2 of high current density.

[0057] Example 3

[0058] A method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0059] (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium molybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.2. The mixture was then transferred to a 100 mL polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst (denoted as NiMoO).

[0060] (2) 15 mL of a solution containing 0.1 mol / L ferric chloride and 15 mL of a solution containing 0.1 mol / L sodium thiosulfate were mixed and stirred for 10 min. The NiMoO obtained in step (1) was immersed in the mixed solution for 5 min. After being taken out, it was dried at 80° C. for 1 h, washed with deionized water and ethanol several times, and vacuum dried to obtain a nickel-iron based precatalyst (denoted as NiMoO / FeSO).

[0061] (3) The NiMoO / FeSO obtained in step (2) was subjected to 20 cyclic voltammetry treatments in 1 mol / L potassium hydroxide, with a voltage range of 0.1-1.9 V (V vs. Hg / HgO), and finally the corresponding genuine nickel-iron-based catalyst (denoted as SR-NiMoO / FeSO) was obtained.

[0062] The oxygen evolution performance test curve of the SR-NiMoO / FeSO electrocatalyst prepared in Example 3 is as follows: Fig.10 As shown by Fig.10 It can be seen that the prepared nickel-iron-based electrocatalyst only needs an overpotential of 305mV to drive 1000mA / cm 2 of high current density.

[0063] Example 4

[0064] A method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0065] (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium molybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.2. The mixture was then transferred to a 100 mL polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst (denoted as NiMoO).

[0066] (2) 15 mL of a solution containing 0.1 mol / L ferric chloride and 15 mL of a solution containing 0.1 mol / L selenious acid were mixed and stirred for 10 min. The NiMoO obtained in step (1) was immersed in the mixed solution for 5 min. After being taken out, it was dried at 80° C. for 1 h, washed with deionized water and ethanol several times, and vacuum dried to obtain a nickel-iron based precatalyst (denoted as NiMoO / FeSeO).

[0067] (3) The NiMoO / FeSeO obtained in step (2) was subjected to 20 cyclic voltammetry treatments in 1 mol / L potassium hydroxide, with a voltage range of 0.1-1.9 V (V vs. Hg / HgO), and finally the corresponding genuine nickel-iron-based catalyst (denoted as SR-NiMoO / FeSeO) was obtained.

[0068] The oxygen evolution performance test curve of the SR-NiMoO / FeSeO electrocatalyst prepared in Example 4 is as follows: Fig.11 As shown by Fig.11 It can be seen that the prepared nickel-iron-based electrocatalyst only needs an overpotential of 317 mV to drive 1000 mA / cm 2 of high current density.

[0069] Example 5

[0070] A method for preparing a nickel-iron-based electrocatalyst for alkaline high current oxygen evolution comprises the following steps:

[0071] (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium molybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.2. The mixture was then transferred to a 100 mL polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst (denoted as NiMoO).

[0072] (2) The NiMoO obtained in step (1) was immersed in 15 mL of a solution containing 0.25 mol / L ferric chloride for 30 s, taken out and dried at 80° C. for 1 h, washed with deionized water and ethanol several times, and vacuum dried to obtain a nickel-iron-based precatalyst (denoted as NiMoO / FeClO).

[0073] In Examples 1 to 4, Fe 3+ It reacts with other anions to form different compounds, thereby introducing different anions. 3 The solution is immersed, and finally FeClO compounds can be formed. - It is also one of the anions that can be introduced for regulation.

[0074] (3) The NiMoO / FeClO obtained in step (2) was subjected to 20 cyclic voltammetry treatments in 1 mol / L potassium hydroxide, with a voltage range of 0.1-1.9 V (V vs. Hg / HgO), and finally the corresponding genuine nickel-iron-based catalyst (denoted as SR-NiMoO / FeClO) was obtained.

[0075] The oxygen evolution performance test curve of the SR-NiMoO / FeClO electrocatalyst prepared in Example 5 is as follows: Fig.12 As shown by Fig.12 It can be seen that the prepared nickel-iron-based electrocatalyst only needs an overpotential of 320mV to drive 1000mA / cm 2 of high current density.

[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although detailed description is given with reference to the embodiments of the present invention, those skilled in the art should understand that modifications or equivalent substitutions of the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention, and should be covered by the protection scope of the claims of the present invention.

Claims

1. A method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution, characterized in that: The steps include: (1) 1.2 mmol nickel nitrate and 0.3 mmol ammonium heptamolybdate were dissolved in 30 mL deionized water, and then ammonia water was added to adjust the pH to 5.

2. The mixture was then transferred to a polytetrafluoroethylene autoclave and the treated nickel foam was added. The mixture was hydrothermally reacted at 150 °C for 6-7 h. After naturally cooling to room temperature, the mixture was washed with deionized water and ethanol for several times, and vacuum dried to obtain a hydrated nickel molybdate precatalyst. (2) impregnating the hydrated nickel molybdate obtained in step (1) alternately in a ferric chloride solution and a sodium hydroxide solution of sodium borohydride; or, impregnating alternately in a ferric chloride solution and a potassium dihydrogen phosphate solution; Alternatively, the hydrated nickel molybdate obtained in step (1) is immersed in a mixed solution of ferric chloride solution and sodium thiosulfate solution; or immersed in a mixed solution of ferric chloride solution and selenious acid solution; Alternatively, the hydrated nickel molybdate obtained in step (1) is immersed in a ferric chloride solution; After being taken out, the catalyst was dried at 80°C for 1-2 hours, washed with deionized water and ethanol for several times, and vacuum dried to obtain a nickel-iron based precatalyst; (3) The nickel-iron-based precatalyst obtained in step (2) was subjected to 20 cyclic voltammetry treatments in 1 mol / L potassium hydroxide, wherein the cyclic voltammetry scanning range was 0.1-1.9 V relative to Hg / HgO, to obtain a nickel-iron-based electrocatalyst.

2. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: In step (2), the alternating dipping is repeated several times.

3. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: When alternately immersed in the ferric chloride solution and the sodium borohydride sodium hydroxide solution, the concentration of the ferric chloride solution is 0.5 mol / L, and in the sodium borohydride sodium hydroxide solution: the concentration of sodium borohydride is 1.5 mol / L, and the concentration of sodium hydroxide is 0.25 mol / L.

4. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: When alternately immersed in the ferric chloride solution and the potassium dihydrogen phosphate solution, the concentration of the ferric chloride solution is 0.1 mol / L, and the concentration of the potassium dihydrogen phosphate solution is 0.1 mol / L.

5. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: When immersed in a mixed solution of ferric chloride solution and sodium thiosulfate solution, the concentration of the ferric chloride solution is 0.1 mol / L, and the concentration of the sodium thiosulfate solution is 0.1 mol / L.

6. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: When immersed in the mixed solution of ferric chloride solution and selenious acid solution, the concentration of ferric chloride solution is 0.1 mol / L, and the concentration of selenious acid solution is 0.1 mol / L.

7. The method for preparing a nickel-iron based electrocatalyst for alkaline high current oxygen evolution according to claim 1, characterized in that: The hydrated nickel molybdate is immersed in a ferric chloride solution, and the concentration of the ferric chloride solution is 0.25 mol / L.