A flexible sensor and its preparation method and application

By combining titanium dioxide-modified SBS fiber membrane and Ecoflex-CNTs composite membrane with a variety of electrode designs, the problem of signal crosstalk and complex structure of flexible sensors in multi-functional sensing is solved, achieving high-sensitivity detection of pressure, stretch and humidity, and simplifying The preparation process reduces costs and is suitable for a variety of applications.

CN115266855BActive Publication Date: 2024-10-01UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211039773.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-29
Publication Date
2024-10-01
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

Existing flexible sensors have problems with signal crosstalk and complex structures in terms of multi-functional sensing. It is difficult to collect different types of external signals at the same time, and the complex electrode design makes the preparation process difficult.

Method used

Using titanium dioxide modified SBS fiber membrane and Ecoflex-CNTs composite elastic membrane combined with various electrode designs, the SBS electrospun film was prepared by electrospinning method, and interdigital electrodes were deposited by DC magnetron sputtering method to achieve pressure, stretching and Highly sensitive detection of humidity, electrode reuse solves wiring problems.

Benefits of technology

It achieves crosstalk-free sensing of three different stimuli and integrates multiple sensing functions into the same flexible device, simplifying the preparation process and reducing costs. It is suitable for fields such as electronic skin equipment, medical detection systems, and environmental monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115266855B_ABST
    Figure CN115266855B_ABST
Patent Text Reader

Abstract

The present invention discloses a flexible sensor and a preparation method and application, belonging to the field of sensor technology; including titanium dioxide modified SBS fiber membrane, Ecoflex-CNTs composite elastic membrane, first plane electrode, second plane electrode and interdigital electrode; titanium dioxide modified SBS fiber membrane is arranged above Ecoflex-CNTs composite elastic membrane, first plane electrode and second plane electrode are respectively arranged at two ends of titanium dioxide modified fiber membrane along thickness direction, second plane electrode and interdigital electrode are respectively arranged at two ends of Ecoflex-CNTs composite elastic membrane along length direction, located between titanium dioxide modified SBS fiber membrane and Ecoflex-CNTs composite elastic membrane. It can realize high-precision measurement of stretching, pressure and humidity, has simple preparation process, realizes crosstalk-free sensing of multiple signals under the premise of reducing the number of electrodes; solves the problems existing in the prior art such as "signal is difficult to decouple; large area, it is difficult to collect different types of signals at the same position at the same time; too many electrodes, and the manufacturing process is more troublesome".
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sensor technology, and in particular to a flexible sensor and a preparation method thereof. Background Art

[0002] The statements in this section merely mention background technology related to the present application and do not necessarily constitute prior art.

[0003] Electronic skin has been widely studied due to its good flexibility, easy conformability and adhesion. Flexible sensors are an important part of the electronic skin system that can accurately convert stimuli into electrical signals while being comfortable to wear. Although common flexible sensors have certain advantages in performance, they have relatively simple functions compared to human skin. The common solution at present is to use nano-conductive materials that can sense multiple stimuli or to assemble different sensors into arrays, but this still has problems of signal crosstalk and complex structure.

[0004] Common flexible sensors detect physical signals such as pressure, stretching, temperature, and chemical signals such as pH, humidity, and gas by combining flexible polymers and dielectric materials. The properties of the dielectric material itself play a decisive role: First, conductive dielectric materials can be made into resistive sensors because conductive materials change resistance when stimulated. Materials with high relative dielectric constants can be used as capacitive sensors; in addition, dielectric materials play a decisive role in sensing performance (sensitivity, response recovery time, stability). At present, common dielectric materials mainly include carbon-based materials, oxides, etc. Oxides are often used in capacitive sensors, but their synthesis is usually difficult and cannot be adapted to flexible substrates; carbon-based materials have attracted attention due to their superior conductivity, thermal stability, and low toxicity, and have been proven to be able to sense multiple stimuli simultaneously under long-term wear conditions, but the response selectivity is poor and different external stimuli cannot be distinguished.

[0005] In order to solve the problem of crosstalk in multifunctional sensors, researchers have made special structural designs for sensors, such as assembling different sensors into arrays on a flexible substrate, and sensing pressure, touch, and temperature through different structural designs and electrode designs. This separate testing method can avoid the phenomenon that multiple signals are difficult to decouple. However, this type of sensor has a large area and it is difficult to collect different types of signals at the same location. Some researchers make full use of the vertical space, design an upper and lower structure, and integrate the two modules into a single structural sensor. However, the complex production process and the large number of electrodes do not make use of integration and packaging. Summary of the invention

[0006] In order to address the deficiencies of the prior art, the present application provides a flexible sensor and a preparation method and application, which can achieve crosstalk-free sensing of three different stimuli, integrate multiple sensing functions into the same flexible sensor, and solve the problem of difficulty in wiring due to too many electrodes during the preparation process through electrode multiplexing.

[0007] In a first aspect, the present application provides a flexible sensor, comprising a titanium dioxide modified SBS fiber membrane, an Ecoflex-CNTs composite elastic membrane, a first planar electrode, a second planar electrode and an interdigital electrode;

[0008] The titanium dioxide modified SBS fiber membrane is arranged above the Ecoflex-CNTs composite elastic membrane, the first planar electrode and the second planar electrode are respectively arranged at the two ends of the titanium dioxide modified fiber membrane along the thickness direction, and the second planar electrode and the interdigital electrode are respectively arranged at the two ends of the Ecoflex-CNTs composite elastic membrane along the length direction and are located between the titanium dioxide modified SBS fiber membrane and the Ecoflex-CNTs composite elastic membrane.

[0009] In a second aspect, the present application provides a method for preparing the flexible sensor, comprising the following steps:

[0010] The SBS electrospinning film is prepared by an electrospinning method, and the SBS electrospinning film is immersed in a prepared DA dispersion to form a PDA-SBS fiber membrane; the PDA-SBS fiber membrane is subjected to a hydrothermal reaction with the prepared precursor solution to obtain a titanium dioxide-modified SBS fiber membrane;

[0011] A cross-finger electrode was sputtered on one end of the titanium dioxide modified SBS fiber membrane along the length direction by direct current magnetron sputtering.

[0012] The Ecoflex solution is evenly applied on the glass surface, and the solution is heated and cured to form an Ecoflex film. The multi-walled carbon nanotube dispersion is applied on the Ecoflex film and dried to obtain an Ecoflex-CNTs composite elastic film.

[0013] The titanium dioxide modified SBS fiber membrane is placed on top of the Ecoflex-CNTs composite elastic membrane, and the interdigitated electrodes are in contact with the Ecoflex-CNTs composite elastic membrane; a conductive tape is attached to the other end of the titanium dioxide modified SBS fiber membrane along the length direction, and the conductive tape is located at both ends of the titanium dioxide modified SBS fiber membrane along the thickness direction;

[0014] The flexible sensor is packaged as a whole.

[0015] In a third aspect, the present application provides applications of the flexible sensor in electronic skin devices, medical detection systems, environmental monitoring and biotechnology fields.

[0016] Compared with the prior art, the beneficial effects of this application are:

[0017] 1. This application adopts a three-electrode multiplexing design, using different electrode combinations, and cooperates with each other to complete high-sensitivity detection of pressure, stretching and humidity. During the detection process, due to the use of different electrode combinations, different external stimuli will only cause changes in specific electrical signals, thereby achieving crosstalk-free sensing of three different stimuli;

[0018] 2. This application integrates multiple sensing functions into the same flexible device instead of simply superimposing them, and solves the problem of too many electrodes and difficult wiring during the preparation process by multiplexing electrodes;

[0019] 3. The SBS electrospinning film obtained by the electrospinning technology in the present application has a large specific surface area, which provides numerous sites for the subsequent growth of humidity-sensitive materials through hydrothermal reaction, thereby improving the sensitivity;

[0020] 4. The flexible sensor proposed in this application is simple to prepare, low-cost, and miniaturized, and can be widely used in electronic skin devices, medical detection systems, environmental monitoring, biotechnology and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.

[0022] Figure 1 A schematic diagram of the structure of a flexible sensor provided in an embodiment of the present application;

[0023] Figure 2 A schematic diagram of the preparation process of the flexible sensor provided in the embodiment of the present application;

[0024] Figure 3 This is a field emission scanning electron microscope image of the titanium dioxide modified SBS fiber membrane provided in the examples of the present application;

[0025] Figure 4 An enlarged structural schematic diagram of the interdigital electrode and an electron transfer schematic diagram provided in an embodiment of the present application;

[0026] Figure 5 A schematic diagram of the stretch response principle of the flexible sensor provided in an embodiment of the present application;

[0027] Figure 6 A schematic diagram of the humidity response principle of the flexible sensor provided in an embodiment of the present application;

[0028] Figure 7A schematic diagram of a stretch response curve of a flexible sensor provided in an embodiment of the present application;

[0029] Figure 8 A schematic diagram of a humidity response curve of a flexible sensor provided in an embodiment of the present application;

[0030] Fig. 9 A schematic diagram of a pressure response curve of a flexible sensor provided in an embodiment of the present application;

[0031] In the figure: 1. first planar electrode; 2. second planar electrode; 3. interdigitated electrode; 4. titanium dioxide modified SBS fiber membrane; 5. Ecoflex-CNTs composite elastic membrane; 6. first interdigitated finger; 7. second interdigitated finger; l is the length of the finger electrode, w is the width of the finger electrode, and d is the distance between the finger electrodes. DETAILED DESCRIPTION

[0032] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used in the present application have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0033] In the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0034] like Figure 1-9 As shown, in the first aspect, the present invention provides a flexible sensor, which is an upper and lower structure, including a titanium dioxide modified SBS fiber membrane 4, an Ecoflex-CNTs composite elastic membrane 5, a first planar electrode 1, a second planar electrode 2 and a forked electrode 3; the titanium dioxide modified SBS fiber membrane 4 is arranged above the Ecoflex-CNTs composite elastic membrane 5, the first planar electrode 1 and the second planar electrode 2 are respectively arranged at the two ends of the titanium dioxide modified fiber membrane along the thickness direction, the first planar electrode 1 is located above the titanium dioxide modified fiber membrane, and the second planar electrode 2 is located below the titanium dioxide modified fiber membrane; the second planar electrode 2 and the forked electrode 3 are respectively arranged at the two ends of the Ecoflex-CNTs composite elastic membrane 5 along the length direction and between the titanium dioxide modified SBS fiber membrane 4 and the Ecoflex-CNTs composite elastic membrane 5.

[0035] The interdigitated electrode 3 is composed of a first interdigitated finger 6 and a second interdigitated finger 7. The end of the first interdigitated finger 6 close to the Ecoflex-CNTs composite elastic membrane 5 along the length direction is a planar electrode structure. The Ecoflex-CNTs composite elastic membrane 5 is only in contact with the planar electrode structure. The planar electrode structure with a larger size can increase the contact area between the first interdigitated finger 6 and the Ecoflex-CNTs composite elastic membrane 5, ensuring good ohmic contact and smooth passage of electrons. The first interdigitated finger 6 and the second interdigitated finger 7 are respectively composed of a comb-like structure composed of a plurality of finger-shaped electrodes. The finger-shaped electrodes of the first interdigitated finger 6 and the finger-shaped electrodes of the second interdigitated finger 7 are interlaced and not conductive.

[0036] In some embodiments, the first planar electrode 1 and the second planar electrode 2 are both flexible planar electrodes made of conductive tape.

[0037] The first planar electrode 1, the second planar electrode 2 and the titanium dioxide modified SBS fiber membrane 4 form a parallel plate capacitor to form a pressure sensor, which can detect the capacitance response under different pressures. The response size depends on the capacitance value:

[0038]

[0039] Wherein, ε is the relative dielectric constant of the titanium dioxide modified SBS fiber membrane 4, A is the effective area of ​​the first planar electrode 1 and the second planar electrode 2, d is the distance between the first planar electrode 1 and the second planar electrode 2, and k is the electrostatic force constant.

[0040] Under the condition that A does not change significantly, applying pressure can not only change the distance between the first planar electrode 1 and the second planar electrode 2, but also change the effective dielectric constant of the titanium dioxide modified SBS fiber membrane 4 by squeezing out air.

[0041] The effective dielectric constant is defined as:

[0042]

[0043] Among them, ε air and ε S are the dielectric constants of air and titanium dioxide modified SBS fiber membrane 4, V air and V S are the volume fractions of air and titanium dioxide modified SBS fiber membrane 4 respectively; α is the determining parameter of the mixing rule type.

[0044] When the device is subjected to pressure, the air is squeezed out, so the volume fraction V of the titanium dioxide modified SBS fiber membrane 4 S has been improved. S Much larger than ε air , V SSlight changes will also increase the overall capacitance of the titanium dioxide modified SBS fiber membrane 4, resulting in ultra-high response.

[0045] The second planar electrode 2, the first interdigitated finger 6 and the Ecoflex-CNTs composite elastic membrane 5 together constitute a stretching sensor. In the initial stage, the multi-walled carbon nanotubes on the surface of the Ecoflex-CNTs composite elastic membrane 5 are interconnected to form numerous conductive pathways. As the Ecoflex-CNTs composite elastic membrane 5 is continuously stretched, the distance between the multi-walled carbon nanotubes becomes larger and larger, and the multi-walled carbon nanotubes are no longer interconnected, thereby reducing conductivity and increasing resistance. The second planar electrode 2 and the first interdigitated finger 6 are used to measure the resistance change of the Ecoflex-CNTs composite elastic membrane 5 to achieve a response to stretching.

[0046] The flexible sensor of the present application realizes high sensitivity sensing of humidity through the interdigital electrode 3 composed of the first interdigital 6 and the second interdigital 7. The interdigital electrode 3 is used to detect the capacitance change of the titanium dioxide modified SBS fiber membrane 4. The high sensitivity depends on the capacitance value C0 between the first interdigital 6 and the second interdigital 7:

[0047]

[0048] Wherein, ε is the relative dielectric constant of the titanium dioxide modified SBS fiber membrane 4, n is the number of finger electrodes, l is the length of the finger electrodes, w is the width of the finger electrodes, and d is the distance between the finger electrodes.

[0049] Electrons will charge and discharge between two opposing electrodes, so there will be (n-1) charge fields. The relative humidity will have a certain effect on the capacitance between the interdigital electrodes 3. The adsorption of water molecules will increase the dielectric constant of the titanium dioxide modified SBS fiber membrane 4, thereby increasing the capacitance value to achieve humidity sensing performance.

[0050] In a second aspect, the present invention provides a method for preparing the flexible sensor, comprising the following steps:

[0051] The SBS electrospinning film is prepared by an electrospinning method, and the SBS electrospinning film is immersed in a prepared DA dispersion to form a PDA-SBS fiber membrane; the PDA-SBS fiber membrane is subjected to a hydrothermal reaction with the prepared precursor solution to obtain a titanium dioxide-modified SBS fiber membrane 4;

[0052] Sputtering an interdigital electrode 3 on one end of a titanium dioxide modified SBS fiber membrane 4 along the length direction by a DC magnetron sputtering method;

[0053] The Ecoflex solution is evenly dropped on the glass surface, and the solution is heated and cured to form an Ecoflex film. The multi-walled carbon nanotube dispersion is dropped on the Ecoflex film and dried to obtain an Ecoflex-CNTs composite elastic film 5.

[0054] The titanium dioxide modified SBS fiber membrane 4 is placed above the Ecoflex-CNTs composite elastic membrane 5, and the interdigital electrode 3 is in contact with the Ecoflex-CNTs composite elastic membrane 5; a conductive tape is attached to the other end of the titanium dioxide modified SBS fiber membrane 4 along the length direction, and the conductive tape is located at both ends of the titanium dioxide modified SBS fiber membrane 4 along the thickness direction;

[0055] The flexible sensor is packaged as a whole.

[0056] In some embodiments, the steps of preparing the SBS electrospinning film by electrospinning method include:

[0057] The SBS polymer solid is fully mixed with the two solvents to obtain a uniform SBS solution;

[0058] The mixed SBS solution is electrospun through a needle tube, a collector and a high-voltage power supply. Under the action of high voltage electricity, the SBS is stretched into filaments and forms an SBS electrospinning film.

[0059] Furthermore, the two solvents are a mixture of N,N-dimethylformamide and tetrahydrofuran and a mixture of N,N-dimethylformamide and acetone.

[0060] Furthermore, the mass ratio of N,N-dimethylformamide to tetrahydrofuran is 1:3, and the mass ratio of N,N-dimethylformamide to acetone is 1:3; the SBS electrospinning film obtained under this ratio has more uniform and slender fibers.

[0061] Furthermore, the concentration of the SBS solution is 9%-14%.

[0062] SBS solutions with different concentration ratios have different viscosities, and the diameters of the electrospun fibers obtained during the spinning process are different, which prepares for the subsequent TiO2 modification.

[0063] In some embodiments, the DA dispersion is prepared by adding DA powder into a Tris-HCl buffer solution and stirring until the DA powder is fully dissolved.

[0064] Furthermore, the pH value of the Tris-HCl buffer solution is 8.5.

[0065] Furthermore, the stirring time is two hours.

[0066] In some embodiments, the SBS electrospun film is immersed in the prepared DA dispersion for 4 hours, and then taken out and dried after immersion for 4 hours. DA (dopamine) forms a PDA coating on the surface of the SBS electrospun film and self-polymerizes to form a PDA-SBS fiber membrane, providing binding sites for subsequent modification of TiO2.

[0067] In some embodiments, the precursor solution is prepared by mixing tetrabutyl titanate, water, acetic acid and ethanol in proportion and stirring the mixture sufficiently.

[0068] Further, the precursor solution and the PDA-SBS fiber membrane were placed in a reactor liner and subjected to a hydrothermal reaction at 110° C. for 4 hours. After the reaction was completed, the PDA-SBS fiber membrane was taken out and dried at 60° C. to obtain a titanium dioxide-modified SBS fiber membrane 4.

[0069] In some embodiments, the sputtering deposition parameters of the DC magnetron sputtering method are as follows:

[0070] The reference pressure is 8.0×10-3Pa-2.0×10 -3 Pa, working pressure is 0.8Pa-1.0Pa, sputtering temperature is 20℃-30℃, gas flow rate is 40sccm-50sccm, sputtering energy is 40W-50W, pre-sputtering time is 60s-120s, and sputtering time is 10min-15min. Compared with common electrode materials such as graphene, silver nanowires, carbon nanotubes and carbon black, the method of magnetron sputtering deposition of silver has low cost, high precision and good stability, and can realize the fine preparation of interdigital electrodes 3 with simple preparation process.

[0071] Furthermore, only one end of the first interdigital finger 6 of the interdigital electrode 3 is in contact with the Ecoflex-CNTs composite elastic membrane 5 , and the contact end between the first interdigital finger 6 and the Ecoflex-CNTs composite elastic membrane 5 is sputtered into a planar structure.

[0072] In some embodiments, the preparation step of the multi-walled carbon nanotube dispersion is to add deionized water to a high-concentration multi-walled carbon nanotube solution for dilution, and perform ultrasound and stirring.

[0073] In some embodiments, the preparation step of the Ecoflex solution is to mix and stir the Ecoflex A agent and the Ecoflex B agent, and then perform a vacuum defoaming treatment on the mixed solution.

[0074] Furthermore, the mass ratio of Ecoflex A agent to Ecoflex B agent is 1:1.

[0075] Furthermore, the Ecoflex film is subjected to an oxygen ion hydrophilic treatment, so that the Ecoflex film is no longer hydrophobic and is easy to evenly drip the carbon nanotube solution in the later stage.

[0076] In some embodiments, the Ecoflex membrane may be replaced with a polydimethylsiloxane (PDMS) elastomer.

[0077] In some embodiments, the planar structure end of the first interdigitated finger 6 contacts the Ecoflex-CNTs composite elastic membrane 5, and a conductive tape is inserted between the titanium dioxide modified SBS fiber membrane 4 and the Ecoflex-CNTs composite elastic membrane 5 to form a second planar electrode 2, and the second planar electrode 2 is located at one end of the titanium dioxide modified SBS fiber membrane 4 away from the interdigitated electrode 3 along the length direction. A conductive tape is attached to the top of the titanium dioxide modified SBS fiber membrane 4 to form a second planar electrode 2, and the second planar electrode 2 is located at one end of the titanium dioxide modified SBS fiber membrane 4 away from the interdigitated electrode 3 along the length direction.

[0078] In a third aspect, the present invention provides applications of the flexible sensor in electronic skin devices, medical detection systems, environmental monitoring and biotechnology fields.

[0079] Example 1

[0080] (1) Preparation of titanium dioxide modified SBS fiber membrane 4, the specific steps are as follows:

[0081] (101) Take 2 g of SBS solid and dissolve it in a mixed solution of DMF and THF; the DMF solution in the mixed solution of DMF and THF is 5.05 g and the THF solution is 15.15 g. Stir at 80°C for 6 hours to obtain a 9 wt% SBS solution.

[0082] (102) The SBS solution is electrospun through a needle tube, a collector, and a high-voltage power supply, and the SBS is stretched into filaments under the action of high voltage electricity to form an SBS electrospun film; the obtained SBS electrospun film is dried and cut into 2CM*1CM films;

[0083] (103) Preparation of DA dispersion: 50 mg of DA powder was added to 25 ml of Tris-HCl (pH = 8.5) buffer solution and stirred for 2 h until fully mixed. The SBS electrospun film was then immersed in the DA dispersion for 4 h to form a PDA-SBS fiber membrane, which was then removed and dried.

[0084] (104) The precursor solution was prepared by thoroughly mixing 0.2 ml of tetrabutyl titanate, 0.1 ml of deionized water, 5 ml of acetic acid, and 15 ml of ethanol and ultrasonicating to obtain a homogeneous precursor solution;

[0085] The precursor solution and the PDA-SBS fiber membrane were placed in a reaction kettle and hydrothermally heated at 110° C. for 4 hours. After the hydrothermal treatment, the resulting titanium dioxide-modified SBS fiber membrane 4 was naturally cooled to room temperature and then heated and dried.

[0086] (104) A special silver interdigital electrode 3 was deposited on one end of the titanium dioxide modified SBS fiber membrane 4 by direct current magnetron sputtering. The sputtering deposition parameters were as follows: a. base pressure was 5.2×10-3Pa; b. working pressure was 1Pa; c. sputtering temperature was 24°C; d. argon gas flow rate was 22sccm; e. sputtering energy was 50W; f. pre-sputtering time was 120s; g. sputtering time was 15min, and a silver interdigital electrode 3 was obtained.

[0087] (2) Preparation of Ecoflex-CNTs composite elastic film 5, the specific steps are as follows:

[0088] (201) 2 g of Ecoflex A and B were mixed and stirred for 20 min. The mixture was placed in a vacuum drying oven for defoaming for 30 min, and then evenly coated on a glass slide and cured at 80 °C for 2 h to obtain an Ecoflex film.

[0089] (202) The Ecoflex film was then subjected to an oxygen plasma hydrophilic treatment for 2 min.

[0090] (203) Take 1 ml of the multi-walled carbon nanotube aqueous dispersion and add 9 ml of deionized water to dilute it. Take 3 ml of the diluted multi-walled carbon nanotube aqueous dispersion and evenly drop it onto the Ecoflex film after the oxygen ion hydrophilic treatment, and dry it at 50 °C for 1 h to obtain the Ecoflex-CNTs composite elastic film 5, which is then cut into 1.5 cm*1 cm;

[0091] (3) The titanium dioxide modified SBS fiber membrane 4 is placed on top of the Ecoflex-CNTs composite elastic membrane 5, and a conductive tape is attached to the other end without the silver interdigital electrode 3; conductive tapes of appropriate sizes are attached on top of the Ecoflex-CNTs composite elastic membrane 5 and on top of the titanium dioxide modified SBS fiber membrane 4, respectively, to assemble a flexible sensor.

[0092] (4) The flexible sensor is packaged as a whole, and its structure is as follows Figure 1 shown.

[0093] Example 2

[0094] (1) Preparation of titanium dioxide modified SBS fiber membrane 4, the specific steps are as follows:

[0095] (101) Take 2 g of SBS solid and dissolve it in a mixed solution of DMF and THF; the DMF solution in the mixed solution is 3.1 g and the THF solution is 9.3 g. Stir at 80 °C for 6 hours to obtain 14.3 g of SBS solution.

[0096] (102) The SBS solution is electrospun through a needle tube, a collector, and a high-voltage power supply, and the SBS is stretched into filaments under the action of high voltage electricity to form an SBS electrospun film; the obtained SBS electrospun film is dried and cut into films of appropriate sizes;

[0097] (103) Preparation of DA dispersion: 70 mg of DA powder was added to 25 ml of Tris-HCl (pH = 8.5) buffer solution and stirred for 2 h until fully mixed. The SBS electrospun film was then immersed in the DA dispersion for 4 h to form a PDA-SBS fiber membrane, which was then removed and dried.

[0098] (104) The precursor solution was prepared by thoroughly mixing 0.2 ml of tetrabutyl titanate, 0.1 ml of deionized water, 5 ml of acetic acid, and 15 ml of ethanol and ultrasonicating to obtain a homogeneous precursor solution;

[0099] The precursor solution and the PDA-SBS fiber membrane were placed in a reaction kettle and hydrothermally heated at 110° C. for 4 hours. After the hydrothermal treatment, the resulting titanium dioxide-modified SBS fiber membrane 4 was naturally cooled to room temperature and then heated and dried.

[0100] (104) A special silver interdigital electrode 3 was deposited on one end of the titanium dioxide modified SBS fiber membrane 4 by direct current magnetron sputtering. The sputtering deposition parameters were as follows: the base pressure was 3.8×10 -3 Pa; b, working pressure is 1Pa; c, sputtering temperature is 24℃; d, argon gas flow rate is 20sccm; e, sputtering energy is 40W; f, pre-sputtering time is 120s; g, sputtering time is 8min, and silver interdigital electrode 3 is obtained.

[0101] (2) Preparation of Ecoflex-CNTs composite elastic film 5, the specific steps are as follows:

[0102] (201) 2 g of Ecoflex A and B were mixed and stirred for 20 min. The mixture was placed in a vacuum drying oven for defoaming for 30 min, and then evenly coated on a glass slide and cured at 80 °C for 2 h to obtain an Ecoflex film.

[0103] (202) The Ecoflex film was then subjected to an oxygen plasma hydrophilic treatment for 2 min.

[0104] (203) Take 1 ml of the multi-walled carbon nanotube aqueous dispersion and add 9 ml of deionized water to dilute it. Take the diluted multi-walled carbon nanotube aqueous dispersion and evenly drop it onto the Ecoflex film after the oxygen ion hydrophilic treatment, and dry it at 50 °C for 1 h to obtain the Ecoflex-CNTs composite elastic film 5, which is then cut into 1.5 cm*1.5 cm;

[0105] (3) The titanium dioxide modified SBS fiber membrane 4 is placed on top of the Ecoflex-CNTs composite elastic membrane 5, and a conductive tape is attached to the other end without the silver interdigital electrode 3; conductive tapes of appropriate sizes are attached on top of the Ecoflex-CNTs composite elastic membrane 5 and on top of the titanium dioxide modified SBS fiber membrane 4, respectively, to assemble a flexible sensor.

[0106] (4) The flexible sensor is packaged as a whole.

[0107] Example 3

[0108] (1) Preparation of titanium dioxide modified SBS fiber membrane 4, the specific steps are as follows:

[0109] (101) 1.5 g of SBS solid was dissolved in a mixed solution of DMF and THF, wherein the DMF solution contained 3.03 g and the THF solution contained 9.09 g. The mixture was stirred at 80 °C for 6 hours to obtain an SBS solution.

[0110] (102) The SBS solution is electrospun through a needle tube, a collector, and a high-voltage power supply, and the SBS is stretched into filaments under the action of high voltage electricity to form an SBS electrospun film; the obtained SBS electrospun film is dried and cut into films of appropriate sizes;

[0111] (103) Preparation of DA dispersion: 80 mg of DA powder was added to 50 ml of Tris-HCl (pH = 8.5) buffer solution and stirred for 2 h until fully mixed. The SBS electrospun film was then immersed in the DA dispersion for 4 h to form a PDA-SBS fiber membrane, which was then removed and dried.

[0112] (104) The precursor solution was prepared by thoroughly mixing 0.2 ml of tetrabutyl titanate, 0.1 ml of deionized water, 5 ml of acetic acid, and 15 ml of ethanol and ultrasonicating to obtain a homogeneous precursor solution;

[0113] The precursor solution and the PDA-SBS fiber membrane were placed in a reaction kettle and hydrothermaled at 110° C. for 5 hours. After the hydrothermal treatment, the resulting titanium dioxide-modified SBS fiber membrane 4 was naturally cooled to room temperature and then heated and dried.

[0114] (104) A special silver interdigital electrode 3 was deposited on one end of the titanium dioxide modified SBS fiber membrane 4 by direct current magnetron sputtering. The sputtering deposition parameters were as follows: the base pressure was 4.3×10 -3 Pa; b. working pressure is 0.98Pa; c. sputtering temperature is 24°C; d. argon gas flow rate is 22sccm; e. sputtering energy is 60W; f. pre-sputtering time is 60s; g. sputtering time is 12min, and a silver interdigital electrode 3 is obtained.

[0115] (2) Preparation of Ecoflex-CNTs composite elastic film 5, the specific steps are as follows:

[0116] (201) 1.5 g of Ecoflex A and B were mixed and stirred for 20 min. The mixture was placed in a vacuum drying oven for defoaming for 30 min. The mixture was then evenly coated on a glass sheet and cured at 100 °C for 1.5 h to obtain an Ecoflex film.

[0117] (202) The Ecoflex film was then subjected to an oxygen plasma hydrophilic treatment for 2 min.

[0118] (203) Take 1.2 ml of the multi-walled carbon nanotube aqueous dispersion and add 10.8 deionized water to dilute it. Take the diluted multi-walled carbon nanotube aqueous dispersion and evenly drop it onto the Ecoflex film after the oxygen ion hydrophilic treatment, and dry it at 50 °C for 1 h to obtain the Ecoflex-CNTs composite elastic film 5, and cut it into 1.5 cm*1 cm;

[0119] (3) The titanium dioxide modified SBS fiber membrane 4 is placed on top of the Ecoflex-CNTs composite elastic membrane 5, and a conductive tape is attached to the other end without the silver interdigital electrode 3; conductive tapes of appropriate sizes are attached on top of the Ecoflex-CNTs composite elastic membrane 5 and on top of the titanium dioxide modified SBS fiber membrane 4, respectively, to assemble a flexible sensor.

[0120] (4) The flexible sensor is packaged as a whole.

[0121] The description of each embodiment in the above embodiments has different emphases. For parts not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0122] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A flexible sensor, characterized in that: It includes a titanium dioxide modified SBS fiber membrane, an Ecoflex-CNTs composite elastic membrane, a first plane electrode, a second plane electrode and an interdigital electrode; The titanium dioxide modified SBS fiber membrane is arranged above the Ecoflex-CNTs composite elastic membrane, the first plane electrode and the second plane electrode are respectively arranged at two ends of the titanium dioxide modified SBS fiber membrane along the thickness direction, and the second plane electrode and the interdigital electrode are respectively arranged at two ends of the Ecoflex-CNTs composite elastic membrane along the length direction, and are located between the titanium dioxide modified SBS fiber membrane and the Ecoflex-CNTs composite elastic membrane; The preparation method of the titanium dioxide modified SBS fiber membrane comprises: preparing an SBS electrospinning film by an electrospinning method, immersing the SBS electrospinning film in a prepared DA dispersion to form a PDA-SBS fiber membrane; and subjecting the PDA-SBS fiber membrane to a hydrothermal reaction with a prepared precursor solution to prepare a titanium dioxide modified SBS fiber membrane.

2. The flexible sensor according to claim 1, characterized in that: The interdigitated electrode is composed of a first interdigitated finger and a second interdigitated finger, and one end of the first interdigitated finger close to the Ecoflex-CNTs composite elastic membrane along the length direction is a planar electrode structure.

3. The flexible sensor according to claim 1, characterized in that: The first planar electrode and the second planar electrode are both flexible planar electrodes made of conductive tape.

4. The flexible sensor according to claim 1, wherein: The first planar electrode and the second planar electrode are used to detect capacitance responses under different pressures, the second planar electrode and the first interdigital electrode are used to measure the resistance change of the Ecoflex-CNTs composite elastic membrane, and the interdigital electrode is used to measure the capacitance value of the titanium dioxide modified SBS fiber membrane.

5. The method for preparing the flexible sensor according to any one of claims 1 to 4, characterized in that: The steps include: The SBS electrospinning film is prepared by an electrospinning method, and the SBS electrospinning film is immersed in a prepared DA dispersion to form a PDA-SBS fiber membrane; the PDA-SBS fiber membrane is subjected to a hydrothermal reaction with the prepared precursor solution to obtain a titanium dioxide-modified SBS fiber membrane; A cross-finger electrode was sputtered on one end of the titanium dioxide modified SBS fiber membrane along the length direction by direct current magnetron sputtering. The Ecoflex solution is evenly applied on the glass surface, and the solution is heated and cured to form an Ecoflex film. The multi-walled carbon nanotube dispersion is applied on the Ecoflex film and dried to obtain an Ecoflex-CNTs composite elastic film. The titanium dioxide modified SBS fiber membrane is placed on top of the Ecoflex-CNTs composite elastic membrane, and the interdigitated electrode is in contact with the Ecoflex-CNTs composite elastic membrane; a conductive tape is attached to the other end of the titanium dioxide modified SBS fiber membrane along the length direction, and the conductive tape is located at both ends of the titanium dioxide modified SBS fiber membrane along the thickness direction; The flexible sensor is packaged as a whole.

6. The preparation method according to claim 5, characterized in that: The sputtering deposition parameters of DC magnetron sputtering include: The reference pressure is 8.0×10-3 Pa-2.0×10-3 Pa, the working pressure is 0.8 Pa -1.0 Pa, the sputtering temperature is 20℃-30℃, the gas flow rate is 40 sccm-50 sccm, the sputtering energy is 40 W-50 W, the pre-sputtering time is 60 s-120 s, and the sputtering time is 10 min-15 min; or, The first interdigital fingers of the interdigital electrodes are in contact with the Ecoflex-CNTs composite elastic film, and the contact ends of the first interdigital fingers and the Ecoflex-CNTs composite elastic film are sputtered into a planar structure.

7. The preparation method according to claim 5, characterized in that: The steps of preparing SBS electrospinning film by electrospinning method include: The SBS polymer solid is fully mixed with the two solvents to obtain a uniform SBS solution; The mixed SBS solution is electrospun through a needle tube, a collector and a high-voltage power supply. Under the action of high voltage electricity, the SBS is stretched into filaments and forms an SBS electrospinning film.

8. The preparation method according to claim 7, characterized in that: The two solvents are a mixture of N,N-dimethylformamide and tetrahydrofuran and a mixture of N,N-dimethylformamide and acetone.

9. The preparation method according to claim 8, characterized in that: The mass ratio of the N,N-dimethylformamide to tetrahydrofuran is 1:3, and the mass ratio of the N,N-dimethylformamide to acetone is 1:

3.

10. The preparation method according to claim 7, characterized in that: The concentration of the SBS solution is 9%-14%.

11. The preparation method according to claim 5, characterized in that: The DA dispersion is prepared by adding DA powder into a Tris-HCl buffer solution and stirring until the DA powder is fully dissolved.

12. The preparation method according to claim 11, characterized in that: The pH value of the Tris-HCl buffer solution is 8.

5.

13. The preparation method according to claim 11, characterized in that: The stirring time is two hours.

14. The preparation method according to claim 5, characterized in that: The soaking time is 4 hours.

15. The preparation method according to claim 5, characterized in that: The precursor solution is prepared by mixing tetrabutyl titanate, water, acetic acid and ethanol in proportion and stirring them fully.

16. The preparation method according to claim 5, characterized in that: The preparation steps of the multi-walled carbon nanotube dispersion are as follows: adding deionized water to a high-concentration multi-walled carbon nanotube solution for dilution, and performing ultrasonication and stirring.

17. The preparation method according to claim 5, characterized in that: The preparation steps of the Ecoflex solution are as follows: mixing Ecoflex A agent and Ecoflex B agent and stirring the mixture, and performing vacuum defoaming treatment on the mixed solution.

18. The preparation method according to claim 17, characterized in that: The mass ratio of the Ecoflex A agent to the Ecoflex B agent is 1:

1.

19. Application of the flexible sensor according to any one of claims 1 to 4 in the fields of electronic skin devices, medical detection systems, environmental monitoring and biotechnology.