A UV detector based on FTO / α-Ga2O3 / MgZnO crystal matching heterojunction and its preparation method

By using SiO2/FTO substrate and α-Ga2O3 nanowire composite MgZnO nanomaterial in ultraviolet photodetectors, the problem of improving performance of traditional single material is solved and high responsiveness and The ultraviolet detection effect of high light current is suitable for large-scale production.

CN115274932BActive Publication Date: 2024-11-01JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210954059.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-10
Publication Date
2024-11-01
Estimated Expiration
2042-08-10

AI Technical Summary

Technical Problem

Traditional single wide bandgap semiconductor material UV photodetectors encounter problems of performance reduction in performance improvement, especially low carrier mobility, short exciton lifetime, and many traps and defects in the body of oxide materials, resulting in low photocurrent. , low responsiveness.

Method used

The FTO/α-Ga2O3/MgZnO crystal form matching heterojunction was constructed using SiO2/FTO substrate and α-Ga2O3 nanowire composite MgZnO nanomaterial. The α-Ga2O3/MgZnO heterojunction photosensitive layer was prepared by hydrothermal method, and the photosensitive layer of α-Ga2O3/MgZnO heterojunction was prepared in the same way as the On it, an Ag electrode is prepared to form an ultraviolet detector based on FTO/α-Ga2O3/MgZnO heterojunction.

Benefits of technology

It improves the responsiveness and photocurrent of the ultraviolet photodetector, reduces the dark current, enhances the light-to-dark current ratio, is suitable for large-scale production, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115274932B_ABST
    Figure CN115274932B_ABST
Patent Text Reader

Abstract

A UV detector based on FTO / α-Ga2O3 / MgZnO crystal-matched heterojunction and a preparation method thereof, a UV photodetector and a preparation method thereof, belong to the field of UV photodetection technology. From bottom to top, it is composed of a SiO2 / FTO substrate, a Ga2O3 nanowire grown on FTO, a Ga2O3 / MgZnO heterojunction photosensitive layer formed by filling MgZnO nanomaterials in the gaps of the Ga2O3 nanowires, and an Ag electrode prepared on the photosensitive layer; the UV light to be measured is incident from one side of the SiO2 / FTO substrate, wherein the thickness of the SiO2 / FTO substrate is 2 to 3 mm, the thickness of the Ga2O3 / MgZnO heterojunction photosensitive layer is 2 to 3 μm, and the thickness of the Ag electrode is 1 to 3 mm. The hydrothermal method of the present invention is simple and easy, low in cost, and has low requirements on equipment. The prepared device has a high response to UV light and is suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of ultraviolet photoelectric detection, and specifically relates to an ultraviolet detector based on FTO / α-Ga2O3 / MgZnO crystal matching heterojunction, which uses SiO2 / FTO (silicon dioxide / fluorine-doped tin oxide) as a substrate, α-Ga2O3 nanowire composite MgZnO nanomaterial as a photosensitive layer, and Ag (silver) as an electrode, and a preparation method thereof. The ultraviolet photoelectric detector and its preparation method. Background Art

[0002] Ultraviolet photodetectors are detectors that convert ultraviolet light into electrical signals. When exposed to ultraviolet electromagnetic waves with a frequency higher than a certain frequency, the electrons in the detector's photosensitive layer absorb photon energy and transition, forming a quantitatively detectable current under the action of the electric field, thereby realizing the detection of ultraviolet signals.

[0003] High-performance ultraviolet detectors are widely used in the fields of environment, medicine, astronomy, military, etc. They can be used for ultraviolet intensity detection, optical communication, missile tail flame detection, fire alarm, etc. With the development of science and technology, people are committed to studying ultraviolet photodetectors with high responsiveness, high detection sensitivity, high selectivity, and ultrafast response speed. However, ultraviolet photodetectors based on traditional single wide bandgap semiconductor materials, especially wide bandgap semiconductor materials, are currently difficult to further improve various performance parameters. In addition, some inherent deficiencies of wide bandgap semiconductor materials, such as low carrier mobility, short exciton lifetime, and many traps and defects in oxide materials, lead to problems such as low device photocurrent and low responsiveness. Therefore, improving traditional single materials to achieve the improvement of overall device performance is the research focus and hotspot in the field of ultraviolet detectors in the future. The main methods currently used are doping, modification, and construction of heterojunctions. Among them, the preparation of heterogeneous composite materials to construct heterostructures has been proven by a large number of experiments and theories to be a simple and extremely effective method, that is, to improve the shortcomings of single material devices by synergizing the advantages of two materials and the different working mechanisms of multiple heterostructures to achieve an overall improvement in device performance.

[0004] However, in the process of preparing ultraviolet photodetectors with heterojunctions, the performance of the device is often reduced due to mismatched crystal forms. By selecting two semiconductor materials with similar crystal structures, atomic spacing and thermal expansion coefficients but different energy band gaps, the advantages of the two materials can be combined to stimulate better photoelectric performance. Summary of the invention

[0005] The purpose of the present invention is to provide a UV detector based on FTO / α-Ga2O3 / MgZnO crystal matching heterojunction and a preparation method thereof in view of the above-mentioned heterogeneous crystal type matching problem. The method uses α-Ga2O3 nanowires as a substrate, fills MgZnO nanomaterials, and composites an α-Ga2O3 / MgZnO heterojunction photosensitive layer. The hydrothermal method used is simple and easy, low in cost, and has low equipment requirements. Moreover, the materials constituting the device are all inorganic semiconductor materials, which are non-toxic and environmentally friendly. The prepared device has a high response to ultraviolet light, is suitable for mass production, and has good development prospects and important application value.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] A UV detector based on FTO / α-Ga2O3 / MgZnO heterojunction, which consists of a SiO2 / FTO substrate, an α-Ga2O3 / MgZnO heterojunction photosensitive layer grown on FTO, and an Ag electrode prepared on the heterojunction photosensitive layer from bottom to top. The UV light to be measured is incident from the SiO2 side of the SiO2 / FTO substrate; the α-Ga2O3 / MgZnO heterojunction photosensitive layer consists of α-Ga2O3 nanorods and MgZnO filled in the gaps of the α-Ga2O3 nanorods;

[0008] The method for preparing a UV detector based on FTO / α-Ga2O3 / MgZnO heterojunction described in the present invention comprises the following steps:

[0009] (1) Substrate processing

[0010] The SiO2 / FTO substrate with a thickness of 2-3 mm (wherein the thickness of FTO is 250-350 nm) is immersed in acetone, ethanol, and deionized water for ultrasonic treatment for 10-20 minutes, blown dry with nitrogen, and then placed in an ultraviolet ozone environment for treatment for 10-20 minutes to obtain a clean SiO2 / FTO substrate;

[0011] (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction

[0012] First, prepare an α-Ga2O3 seed layer precursor solution: add 4.20~8.40g of gallium nitrate nonahydrate, 20~40µL of polyoxyethylene lauryl ether, and 0.015~0.030g of D-(-)-tartaric acid into 20~40mL of deionized water, stir in a 70~80℃ water bath for 20~40 minutes, and finally place the obtained solution in a dark place for 18~30 hours to obtain an α-Ga2O3 seed layer precursor solution;

[0013] An α-Ga2O3 seed layer is prepared on the surface of the substrate cleaned in step (1): an α-Ga2O3 seed layer precursor solution is spin-coated on the FTO surface of the SiO2 / FTO substrate to form a thin film, the spin-coating speed is 2000-3500 rpm, and the spin-coating time is 20-30 seconds; the substrate is dried at 100-120°C for 10-15 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps are repeated 4-5 times, and finally the SiO2 / FTO substrate is sintered at 400-500°C for 30-60 minutes, thereby obtaining an α-Ga2O3 seed layer on the surface of the SiO2 / FTO substrate;

[0014] Preparation of the hydrothermal solution: add 0.76-1.26 g of gallium nitrate nonahydrate and 0.042-0.070 g of hexamethylenetetramine to 60-100 mL of deionized water, and stir for 30-60 minutes to obtain a hydrothermal solution;

[0015] Then, the SiO2 / FTO substrate with the α-Ga2O3 seed layer is immersed in the hydrothermal solution with the seed layer facing downward, sealed and subjected to hydrothermal reaction at 170-190°C for 10-14 hours, and after cooling to room temperature, the SiO2 / FTO substrate is taken out and the seed layer is facing upward, rinsed with deionized water, dried, and sintered at 450-550°C for 3-5 hours to obtain α-Ga2O3 nanorods on the SiO2 / FTO substrate;

[0016] (3) Preparation of MgZnO precursor solution

[0017] 0.26-0.52 g of magnesium acetate tetrahydrate and 1.05-2.11 g of zinc acetate dihydrate are added to 20-40 mL of isopropanol, and the mixture is stirred in a water bath at 70-80° C. for 30-60 minutes. Then, 0.36-0.72 mL of monoethanolamine and 0.009-0.019 g of hexamethylenetetramine are added, and the mixture is stirred in a water bath at 70-80° C. for 1-3 hours. Finally, the obtained solution is placed in a dark place for aging for 18-30 hours to obtain a MgZnO precursor solution.

[0018] (4) Preparation of α-Ga2O3 / MgZnO heterojunction photosensitive layer

[0019] Spin coating the surface of α-Ga2O3 nanorods on SiO2 / FTO substrate with MgZnO precursor solution to form a thin film, the spin coating speed is 2000-3500 rpm, and the spin coating time is 20-30 seconds; after drying at 170-190°C for 8-12 minutes, the substrate is cooled to room temperature; the above spin coating, drying, and substrate cooling steps are repeated 3-9 times, and finally the SiO2 / FTO substrate is sintered at 450-550°C for 1-3 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction photosensitive layer on the surface of the SiO2 / FTO substrate with a thickness of 2-3 μm;

[0020] (5) Preparation of Ag electrode

[0021] Using a mask with a hollow circular pattern, Ag conductive glue is drop-coated on the α-Ga2O3 / MgZnO heterojunction photosensitive layer and Ag wires are led out, and the mixture is dried at 80-120°C for 8-20 minutes to obtain two circular Ag electrodes with a thickness of 1-3 mm on the α-Ga2O3 / MgZnO heterojunction layer, thereby preparing the ultraviolet light detector based on the FTO / α-Ga2O3 / MgZnO heterojunction described in the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 : A schematic diagram of the structure of the ultraviolet photodetector prepared by the present invention;

[0024] Figure 2 : SEM image of α-Ga2O3 nanowires prepared in step 2) of Example 2 of the present invention;

[0025] Figure 3 : SEM image of the α-Ga2O3 / MgZnO heterojunction photosensitive layer composite material prepared in step 4) of Example 2 of the present invention;

[0026] Figure 4 : XRD patterns of α-Ga2O3 nanowires, MgZnO, and α-Ga2O3 / MgZnO heterojunction photosensitive layer composite materials (α-Ga2O3-MgZnO) prepared by the present invention;

[0027] Figure 5 : Current-voltage characteristic curve of the device prepared in Example 1 of the present invention;

[0028] Figure 6 : Current-voltage characteristic curve of the device prepared in Example 2 of the present invention;

[0029] Figure 7 : Current-voltage characteristic curve of the device prepared in Example 3 of the present invention;

[0030] Figure 8 : Current-voltage characteristic curve of the device prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work, any modifications, equivalent substitutions, improvements, etc., should be included in the protection scope of the present invention.

[0032] Embodiment 1:

[0033] (1) Substrate processing

[0034] A 3 mm thick SiO2 / FTO substrate (wherein the thickness of FTO is 300 nm) was immersed in acetone, ethanol, and deionized water for ultrasonic treatment for 15 minutes, dried with nitrogen, and then placed in an ultraviolet ozone environment for treatment for 15 minutes to obtain a clean SiO2 / FTO substrate;

[0035] (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction

[0036] First, prepare the α-Ga2O3 seed layer precursor solution: add 6.30 g of gallium nitrate nonahydrate, 30 µL of polyoxyethylene lauryl ether, and 0.023 g of D-(-)-tartaric acid into 30 mL of deionized water, stir in a 75°C water bath for 30 minutes, and finally place the obtained solution in a dark place for 24 hours to obtain the α-Ga2O3 seed layer precursor solution;

[0037] An α-Ga2O3 seed layer is prepared on the surface of the substrate cleaned in step (1): an α-Ga2O3 seed layer precursor solution is spin-coated on the FTO surface of the SiO2 / FTO substrate to form a thin film, the spin-coating speed is 3000 rpm, and the spin-coating time is 30 seconds; the substrate is dried at 110° C. for 10 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps are repeated 5 times, and finally the SiO2 / FTO substrate is sintered at 450° C. for 30 minutes, thereby obtaining an α-Ga2O3 seed layer on the surface of the SiO2 / FTO substrate;

[0038] Preparation of hydrothermal solution: Add 1.01 g of gallium nitrate nonahydrate and 0.056 g of hexamethylenetetramine to 80 mL of deionized water and stir for 30 minutes to obtain a hydrothermal solution;

[0039] The SiO2 / FTO substrate with the α-Ga2O3 seed layer was immersed in the hydrothermal solution with the seed layer facing downward and completely tilted and fixed with tweezers, sealed and subjected to hydrothermal reaction at 180°C for 12 hours, and after cooling to room temperature, the SiO2 / FTO substrate was taken out and the seed layer was facing upward, rinsed with deionized water, dried, and sintered in a muffle furnace at 500°C for 4 hours to obtain α-Ga2O3 nanorods on the SiO2 / FTO substrate;

[0040] (3) Preparation of MgZnO precursor solution

[0041] 0.39 g of magnesium acetate tetrahydrate and 1.58 g of zinc acetate dihydrate were added to 30 mL of isopropanol, and the mixture was stirred in a water bath at 75° C. for 30 minutes. Then, 0.54 mL of monoethanolamine and 0.014 g of hexamethylenetetramine were added, and the mixture was stirred in a water bath at 75° C. for 2 hours. Finally, the obtained solution was placed in a dark place for aging for 24 hours to obtain a MgZnO precursor solution.

[0042] (4) Preparation of α-Ga2O3 / MgZnO heterojunction photosensitive layer

[0043] The MgZnO precursor solution was spin-coated on the surface of the α-Ga2O3 nanorods on the SiO2 / FTO substrate to form a thin film, the spin-coating speed was 3000 rpm, and the spin-coating time was 30 seconds; then the substrate was dried at 180°C for 10 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps were repeated 3 times, and finally the SiO2 / FTO substrate was sintered at 500°C for 2 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction photosensitive layer on the surface of the SiO2 / FTO substrate with a thickness of 2 μm;

[0044] (5) Preparation of Ag electrode

[0045] Using a mask with a hollow circular pattern, Ag conductive glue was drop-coated on the α-Ga2O3 / MgZnO heterojunction photosensitive layer and Ag wires were led out. After drying at 100°C for 15 minutes, two circular Ag electrodes with a thickness of 2.5 mm were obtained on the α-Ga2O3 / MgZnO heterojunction photosensitive layer, thereby preparing an ultraviolet light detector based on FTO / α-Ga2O3 / MgZnO heterojunction.

[0046] Embodiment 2:

[0047] (1) Substrate processing: The specific implementation is the same as Example 1.

[0048] (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction: The specific implementation is the same as Example 1.

[0049] (3) Preparation of MgZnO precursor solution: The specific implementation is the same as Example 1.

[0050] (4) Preparation of α-Ga2O3 / MgZnO heterojunction photosensitive layer

[0051] The MgZnO precursor solution was spin-coated on the surface of the α-Ga2O3 nanorods on the SiO2 / FTO substrate to form a thin film, the spin-coating speed was 3000 rpm, and the spin-coating time was 30 seconds; then the substrate was dried at 180°C for 10 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps were repeated 5 times, and finally the SiO2 / FTO substrate was sintered at 500°C for 2 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction on the surface of the SiO2 / FTO substrate with a thickness of 2.3 μm;

[0052] (5) Preparation of Ag electrode: The specific implementation is the same as Example 1.

[0053] Embodiment 3:

[0054] (1) Substrate processing: The specific implementation is the same as Example 1.

[0055] (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction: The specific implementation is the same as Example 1.

[0056] (3) Preparation of MgZnO precursor solution: The specific implementation is the same as Example 1.

[0057] (4) Preparation of α-Ga2O3 / MgZnO heterojunction

[0058] The MgZnO precursor solution was spin-coated on the surface of the α-Ga2O3 nanorods on the SiO2 / FTO substrate to form a thin film, the spin-coating speed was 3000 rpm, and the spin-coating time was 30 seconds; then the substrate was dried at 180°C for 10 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps were repeated 7 times, and finally the SiO2 / FTO substrate was sintered at 500°C for 2 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction on the surface of the SiO2 / FTO substrate with a thickness of 2.6 μm;

[0059] (5) Preparation of Ag electrode: The specific implementation is the same as Example 1.

[0060] Embodiment 4:

[0061] (1) Substrate processing: The specific implementation is the same as Example 1.

[0062] (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction: The specific implementation is the same as Example 1.

[0063] (3) Preparation of MgZnO precursor solution: The specific implementation is the same as Example 1.

[0064] (4) Preparation of α-Ga2O3 / MgZnO heterojunction

[0065] The MgZnO precursor solution was spin-coated on the surface of the α-Ga2O3 nanorods on the SiO2 / FTO substrate to form a thin film, the spin-coating speed was 3000 rpm, and the spin-coating time was 30 seconds; then the substrate was dried at 180°C for 10 minutes and then cooled to room temperature; the above spin-coating, drying, and substrate cooling steps were repeated 9 times, and finally the SiO2 / FTO substrate was sintered at 500°C for 2 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction on the surface of the SiO2 / FTO substrate with a thickness of 3.0 μm;

[0066] (5) Preparation of Ag electrode: The specific implementation is the same as Example 1.

[0067] After the ultraviolet photodetector was prepared, its ultraviolet photodetection performance was tested.

[0068] like Figure 1 As shown, the ultraviolet photodetector of the present invention is composed of SiO21 / FTO2 substrate, α-Ga2O3 nanorods 3 grown on FTO, MgZnO filled in the gaps of the nanorods to form an α-Ga2O3 / MgZnO heterojunction photosensitive layer 4, and Ag electrode 5 prepared on the photosensitive layer, and a silver wire 6 is led out as a wire for device connection. The ultraviolet light to be measured is incident from one side of the SiO2 / FTO substrate.

[0069] like Figure 2 As shown, it can be seen from the figure that the α-Ga2O3 nanowires are neatly arranged, and the diameter of the nanowires is about 300nm;

[0070] like Figure 3 As shown in the figure, it can be seen that the α-Ga2O3 nanowires are in close contact with the MgZnO nanomaterials, and the MgZnO nanomaterials are effectively filled into the gaps in the α-Ga2O3 nanowires;

[0071] like Figure 4 As shown, when the number of MgZnO spin-coated layers in the device is 3, under a bias of 1V, the photocurrent of the device is 65.1nA, the dark current is 0.4nA, and the light-to-dark current ratio is 162.75;

[0072] like Figure 5 As shown, when the number of MgZnO spin-coated layers in the device is 5, under a bias of 1V, the photocurrent of the device is 5.12µA, the dark current is 1.39nA, and the light-to-dark current ratio is 3683.45;

[0073] like Figure 6As shown, when the number of MgZnO spin-coated layers in the device is 7, under a bias of 1V, the photocurrent of the device is 5.21µA, the dark current is 1.14nA, and the light-to-dark current ratio is 4570.18;

[0074] like Figure 7 As shown, when the number of MgZnO spin-coated layers in the device is 9, under a bias of 1V, the photocurrent of the device is 10.7µA, the dark current is 13.2nA, and the light-to-dark current ratio is 810.

[0075] As can be seen from the above figure, the ultraviolet photodetector of the present invention uses α-Ga2O3 nanorods composited with MgZnO nanomaterials as the photosensitive layer. Figure 3 As shown in the SEM image, there is no obvious stratification between α-Ga2O3 nanorods and MgZnO nanomaterials. Figure 4 As shown, the α-Ga2O3 prepared by the present invention is a hexagonal crystal, and MgZnO belongs to a triangular crystal, and the hexagonal crystal belongs to a special type of triangular crystal. Due to the similarity of the crystal forms, the α-Ga2O3 nanorods and the MgZnO nanomaterials have a tighter combination when forming a heterojunction. At the same time, the lattice mismatch rate of α-Ga2O3 and MgZnO is very low, which can reduce a large number of defects at the heterojunction interface caused by lattice mismatch, thereby constructing a higher quality built-in electric field. In addition, the α-Ga2O3 nanowire, with its special structure, has a large number of gaps, and filling MgZnO therein can form a large amount of heterojunction area, thereby effectively improving the photoelectric performance of the device.

[0076] Therefore, the ultraviolet photodetector based on the FTO / α-Ga2O3 / MgZnO heterojunction prepared by the present invention has extremely low dark current and high light-dark suppression ratio, and can effectively detect ultraviolet rays.

[0077] At the same time, the process of the invention is simple, the ultraviolet photodetector prepared is small in size, suitable for mass production, and thus has important application value. The preparation method of the invention has the characteristics of simple preparation method, low cost, high light response, and promising large-scale production, and has good detection performance for ultraviolet light.

[0078] The above-described contents are only specific implementation modes of the present invention and cannot be used to limit the scope of implementation of the present invention. All equivalent changes and improvements made according to the scope of the patent application of the present invention should still fall within the scope covered by the patent of the present invention.

Claims

1. A method for preparing an ultraviolet detector based on FTO / α-Ga2O3 / MgZnO heterojunction, the steps of which are as follows: (1) Substrate processing The SiO2 / FTO substrate is sequentially immersed in acetone, ethanol, and deionized water for ultrasonic treatment for 10 to 20 minutes, blown dry with nitrogen, and then placed in an ultraviolet ozone environment for treatment for 10 to 20 minutes to obtain a clean SiO2 / FTO substrate; (2) Preparation of FTO / α-Ga2O3 nanowire heterojunction First, prepare an α-Ga2O3 seed layer precursor solution: add 4.20-8.40 g of gallium nitrate nonahydrate, 20-40 μL of polyoxyethylene lauryl ether, and 0.015-0.030 g of D-(-)-tartaric acid to 20-40 mL of deionized water, stir in a water bath at 70-80° C. for 20-40 minutes, and finally place the obtained solution in a dark place and let it stand for 18-30 hours to obtain an α-Ga2O3 seed layer precursor solution; An α-Ga2O3 seed layer is prepared on the surface of the substrate cleaned in step (1): an α-Ga2O3 seed layer precursor solution is spin-coated on the FTO surface of the SiO2 / FTO substrate to form a thin film, and then the substrate is dried at 100-120°C for 10-15 minutes and then cooled to room temperature; the above spin coating, drying, and substrate cooling steps are repeated 4-5 times, and finally the SiO2 / FTO substrate is sintered at 400-500°C for 30-60 minutes, thereby obtaining an α-Ga2O3 seed layer on the surface of the SiO2 / FTO substrate; Preparation of the hydrothermal solution: add 0.76-1.26 g of gallium nitrate nonahydrate and 0.042-0.070 g of hexamethylenetetramine to 60-100 mL of deionized water, and stir for 30-60 minutes to obtain a hydrothermal solution; Then, the SiO2 / FTO substrate with the α-Ga2O3 seed layer is immersed in a hydrothermal solution with the seed layer facing downward, sealed and subjected to hydrothermal reaction at 170-190° C. for 10-14 hours, and after cooling to room temperature, the SiO2 / FTO substrate is taken out, and the seed layer is faced upward, rinsed with deionized water, dried, and sintered at 450-550° C. for 3-5 hours to obtain α-Ga2O3 nanorods on the SiO2 / FTO substrate; (3) Preparation of MgZnO precursor solution 0.26-0.52 g of magnesium acetate tetrahydrate and 1.05-2.11 g of zinc acetate dihydrate are added to 20-40 mL of isopropanol, and the mixture is stirred in a water bath at 70-80° C. for 30-60 minutes. Then, 0.36-0.72 mL of monoethanolamine and 0.009-0.019 g of hexamethylenetetramine are added, and the mixture is stirred in a water bath at 70-80° C. for 1-3 hours. Finally, the obtained solution is placed in a dark place for aging for 18-30 hours to obtain a MgZnO precursor solution. (4) Preparation of α-Ga2O3 / MgZnO heterojunction photosensitive layer The MgZnO precursor solution is spin-coated on the surface of the α-Ga2O3 nanorods of the SiO2 / FTO substrate to form a thin film, and then the substrate is dried at 170-190°C for 8-12 minutes and then cooled to room temperature; the spin coating, drying, and substrate cooling steps are repeated 3-9 times, and finally the SiO2 / FTO substrate is sintered at 450-550°C for 1-3 hours, thereby obtaining an α-Ga2O3 / MgZnO heterojunction photosensitive layer on the surface of the SiO2 / FTO substrate; (5) Preparation of Ag electrode Using a mask with a hollow circular pattern, Ag conductive glue is drop-coated on the α-Ga2O3 / MgZnO heterojunction photosensitive layer and Ag wires are led out. The mixture is dried at 80-120°C for 8-20 minutes to obtain two circular Ag electrodes on the α-Ga2O3 / MgZnO heterojunction layer, thereby preparing an ultraviolet light detector based on FTO / α-Ga2O3 / MgZnO heterojunction.

2. A UV detector based on FTO / α-Ga2O3 / MgZnO heterojunction, characterized in that: It is prepared by the method described in claim 1.

3. The ultraviolet detector based on FTO / α-Ga2O3 / MgZnO heterojunction according to claim 2, characterized in that: The thickness of the SiO2 / FTO substrate is 2-3 mm, wherein the thickness of the FTO is 250-350 nm; the thickness of the α-Ga2O3 / MgZnO heterojunction photosensitive layer is 2-3 μm, and the thickness of the Ag electrode is 1-3 mm.