Method for manufacturing steel parts having local softened portions
By applying strain to the steel plate and controlling the processing conditions, the problem of difficulty in achieving local softening by local temperature control in the existing technology was solved, and high-strength steel parts that were softened only in specific parts were successfully manufactured.
Patent Information
- Application Number
- CN202180019095.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-13
- Filing Date
- 2021-01-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-01-15
Smart Images

Figure CN115279927B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a steel part having a local softened portion. Background Art
[0002] In recent years, in order to protect passengers in the event of a car collision, a technology that allows specific parts to be deformed preferentially in the event of a collision while maintaining high strength as a whole is required for the car frame parts. To this end, a high-strength steel part with a locally softened specific part and / or a manufacturing method thereof that can be used in this technology is required.
[0003] Patent Document 1 discloses a method of applying a heat shield to a portion to be softened when a steel plate is heated to an austenite single-phase temperature region. Thus, the portion to which the heat shield is applied is lower than the austenite single-phase temperature region even during heating, and the martensitic transformation of this portion after rapid cooling is suppressed, so that this portion softens compared to the portion to which the heat shield is not applied.
[0004] Patent Document 2 discloses a method in which a portion where the steel sheet and the die are poorly contacted is provided when the steel sheet is brought into contact with the die and rapidly cooled from the austenite single phase temperature region, thereby analyzing a soft structure (ferrite and / or pearlite) in the portion and softening the portion.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-78189
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 2011-179028 Summary of the invention
[0009] Problems to be solved by the invention
[0010] In Patent Documents 1 and 2, it is not possible to soften only the desired portion by the influence of heat transfer in the steel plate. For example, in Patent Document 1, when only the portion to which the heat shield is applied is softened below the austenite single-phase temperature region, heat is transferred from the adjacent portion to which the heat shield is not applied to the end of the portion to which the heat shield is applied, and as a result, the end of the portion to which the heat shield is applied cannot be fully softened. In Patent Document 2, when only the portion that is poorly in contact with the mold is softened without rapid cooling, heat is transferred from the portion to the adjacent portion that is in good contact with the mold, and as a result, the adjacent portion adjacent to the mold can also obtain a softening effect. Therefore, it is difficult to locally soften only the desired portion by a method of softening by local temperature control as in Patent Documents 1 and 2.
[0011] The embodiments of the present invention have been proposed in view of such circumstances, and one of the objects thereof is to provide a method for manufacturing a locally softened high-strength steel part without performing local temperature control.
[0012] Means of solving the problem
[0013] A first aspect of the present invention is a method for manufacturing a steel part, comprising the following steps:
[0014] A process for preparing a steel plate having the following chemical composition,
[0015] C: 0.05 to 0.40 mass %,
[0016] Si: 0-2.0 mass %,
[0017] Mn: 1.0 to 3.0 mass %,
[0018] Al: 0.010 to 1.0 mass %,
[0019] P: more than 0 mass % and less than 0.100 mass %,
[0020] S: more than 0 mass % and less than 0.010 mass %,
[0021] N: more than 0 mass % and less than 0.010 mass %,
[0022] B: 0.0005 to 0.010 mass %, and
[0023] Balance: Iron and unavoidable impurities;
[0024] The step of heating the steel plate to a temperature not less than the Ac1 point (°C) and not less than the Ac3 point (°C) + 10°C;
[0025] After the heating step, a processing step of applying a strain of 0.5% or more at a processing temperature of 675°C or more and lower than Ac3 point (°C) + 10°C;
[0026] After the processing step, a step of maintaining the processing temperature for 1 second to 120 seconds or slowly cooling the processing temperature for 1 second to 120 seconds at an average cooling rate higher than 0°C / second and less than 15°C / second;
[0027] After the holding or slow cooling step, the step of cooling to Ms point (°C) - 50°C is performed.
[0028] The average cooling rate from the temperature in the heating step to Ms point (° C.)-50° C. is controlled to be 10° C. / sec or more.
[0029] A second aspect of the present invention is a method for manufacturing a steel part, comprising the following steps:
[0030] A process for preparing a steel plate having the following chemical composition,
[0031] C: 0.05 to 0.40 mass %,
[0032] Si: 0-2.0 mass %,
[0033] Mn: 1.0 to 3.0 mass %,
[0034] Al: 0.010 to 1.0 mass %,
[0035] P: more than 0 mass % and less than 0.100 mass %,
[0036] S: more than 0 mass % and less than 0.010 mass %,
[0037] N: more than 0 mass % and less than 0.010 mass %,
[0038] B: 0.0005 to 0.010 mass %, and
[0039] Balance: Iron and unavoidable impurities;
[0040] The step of heating the steel plate to a temperature of Ac3 point (°C)+10°C or higher and 1100°C or lower;
[0041] After the heating step, a processing step of applying a strain of 10% or more at a processing temperature of Ms point (°C) + 50°C or more and lower than Ac3 point (°C) + 10°C;
[0042] After the processing step, a step of maintaining the processing temperature for 1 second to 120 seconds or slowly cooling the processing temperature for 1 second to 120 seconds at an average cooling rate higher than 0°C / second and less than 15°C / second;
[0043] After the holding or slow cooling step, the step of cooling to Ms point (°C) - 50°C is performed.
[0044] The average cooling rate from the temperature in the heating step to Ms point (° C.)-50° C. is controlled to be 10° C. / sec or more.
[0045] A third aspect of the present invention is the manufacturing method according to aspect 1 or 2, wherein the steel sheet further comprises
[0046] Cu: more than 0 mass% and less than 0.50 mass%, and
[0047] Ni: one or more selected from the group consisting of more than 0 mass % and 0.50 mass % or less.
[0048] A fourth aspect of the present invention is the manufacturing method according to any one of aspects 1 to 3, wherein the steel plate further comprises
[0049] Ti: more than 0 mass% and less than 0.10 mass%,
[0050] Cr: more than 0 mass% and less than 3.0 mass%, and
[0051] Nb: one or more selected from the group consisting of higher than 0 mass % and 0.10 mass % or less.
[0052] A fifth aspect of the present invention is the production method according to any one of aspects 1 to 4, comprising applying the strain by bulging.
[0053] Aspect 6 of the present invention is the manufacturing method according to any one of aspects 1 to 4, comprising applying the strain by forging.
[0054] A seventh aspect of the present invention is the production method according to any one of aspects 1 to 4, comprising applying the strain by bending back during draw forming.
[0055] An eighth aspect of the present invention is the production method according to any one of aspects 1 to 4, comprising applying the strain by shearing.
[0056] Aspect 9 of the present invention is the production method according to any one of aspects 1 to 8, comprising applying the strain by a plurality of processes.
[0057] A tenth aspect of the present invention is the manufacturing method according to the ninth aspect, wherein the plurality of processes include a process of imparting deformation and a process of restoring the deformation.
[0058] Effects of the Invention
[0059] According to an embodiment of the present invention, a method for manufacturing a locally softened high-strength steel part without performing local temperature control can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a graph showing the relationship between temperature and displacement when a steel plate is heated from a low temperature in a hot working simulation test.
[0061] Figure 2 It means that except Figure 1 In addition to the relationship, this is a graph showing the relationship between temperature and displacement when a steel plate is cooled from a high temperature in a hot working simulation test.
[0062] Figure 3 It is a schematic diagram which shows the extraction position of the sample for evaluation in Example.
[0063] Figure 4 yes Figure 3 Schematic diagram of the X-X line cross section shown. DETAILED DESCRIPTION
[0064] The inventors of the present application have studied from various perspectives in order to realize a method for manufacturing a high-strength steel part that can be locally softened without performing local temperature control.
[0065] As a result, a manufacturing method (hereinafter referred to as embodiment 1 of the present invention) was discovered, in which a steel plate having a predetermined chemical composition is heated to a state where austenite is relatively unstable, such as a two-phase region of austenite and ferrite, and a certain strain is applied to a portion to be softened, thereby promoting nucleation of soft tissue (ferrite and / or pearlite) only in the portion to be softened, and the soft tissue is grown from the portion by holding or slowly cooling for a certain period of time.
[0066] It was also simultaneously discovered (hereinafter referred to as embodiment 2 of the present invention) that, during the above-mentioned heating, even when the austenite is heated to a relatively stable state such as the austenite single-phase region, by applying a larger strain to the portion to be softened, it is possible to promote the nucleation of soft tissue only in the portion to be softened, as in embodiment 1 of the present invention.
[0067] The following describes the details of each requirement specified in Embodiments 1 and 2 of the present invention.
[0068] In this specification, the term "steel part" refers to a steel plate processed into a predetermined shape through the processing steps of the first and second embodiments of the present invention.
[0069] <Embodiment 1 of the present invention>
[0070] The manufacturing method according to the first embodiment of the present invention comprises:
[0071] (a) Process of preparing steel plates;
[0072] (b) after step (a), a step of heating;
[0073] (c) a step of performing processing after step (b);
[0074] (d) after step (c), a step of holding or slow cooling;
[0075] (e) A step of cooling after step (d).
[0076] Hereinafter, each step will be described.
[0077] (a) Process of preparing steel plates
[0078] The chemical composition of the steel plate according to the first embodiment of the present invention is as follows: C: 0.05-0.40 mass%, Si: 0-2.0 mass%, Mn: 1.0-3.0 mass%, Al: 0.010-1.0 mass%, P: higher than 0 mass% and less than 0.100 mass%, S: higher than 0 mass% and less than 0.010 mass%, N: higher than 0 mass% and less than 0.010 mass%, B: 0.0005-0.010 mass%, and the balance: iron and unavoidable impurities.
[0079] Each element is described below in detail.
[0080] (C: 0.05 to 0.40 mass %)
[0081] The strength of the steel part is determined by the C content. In order to obtain sufficient strength of the steel part, the C content is 0.05 mass % or more, preferably 0.10 mass % or more, and more preferably 0.20 mass % or more.
[0082] On the other hand, if the C content becomes excessive, the toughness of the steel part is significantly reduced, and delayed fracture of the steel part is also likely to occur. Therefore, the C content is 0.40 mass% or less, preferably 0.38 mass% or less, and more preferably 0.36 mass% or less.
[0083] (Si: 0-2.0 mass %)
[0084] Si is an element optionally contained in the steel sheet. Since Si improves temper softening resistance, it contributes to the hardness stability of the steel sheet. Therefore, it is preferable that Si is contained in the steel sheet in an amount higher than 0 mass %.
[0085] On the other hand, Si easily forms retained austenite (γ), and promotes a decrease in yield strength (YS) and segregation of Mn. Therefore, the Si content is 2.0 mass % or less, preferably 1.8 mass % or less.
[0086] (Mn: 1.0 to 3.0 mass %)
[0087] Mn contributes to the high strength of steel parts by improving the hardenability of the steel sheet. In order to exert this effect, the Mn content is 1.0 mass % or more, preferably 1.2 mass % or more, and more preferably 1.4 mass % or more.
[0088] On the other hand, if the Mn content becomes excessive, coarse carbides may precipitate in the steel parts. Therefore, the Mn content is 3.0 mass % or less, preferably 2.8 mass % or less, and more preferably 2.6 mass % or less.
[0089] (Al: 0.010 to 1.0 mass%)
[0090] Al is an element that acts as a deoxidizer. In order to exert such an effect, the Al amount is 0.010 mass % or more. The Al amount is preferably 0.020 mass % or more, and more preferably 0.025 mass % or more. However, if Al is contained in excess, the manufacturing cost will increase, and the Ac3 point will be significantly improved, causing the deterioration of the surface quality (decarburization or thickness loss) caused by the high temperature of the raw material heating temperature. Therefore, the Al amount is 1.0 mass % or less. The Al amount is preferably 0.80 mass % or less, and more preferably 0.70 mass % or less.
[0091] (P: higher than 0 mass % and not more than 0.100 mass %)
[0092] P is an element that is inevitably contained and is an element that deteriorates the weldability of the steel plate, but it is also an element that contributes to the solid solution strengthening effect of the ferrite phase. In order to exert this effect without deteriorating the weldability of the steel plate, the P amount is 0.100 mass% or less. The P amount is preferably 0.050 mass% or less, and more preferably 0.020 mass% or less. In addition, P is an impurity that is inevitably mixed into the steel, and its amount cannot be reduced to 0 mass% in industrial production, and is usually higher than 0 mass%. In addition, it can contain 0.00050 mass% or more.
[0093] (S: higher than 0 mass % and not more than 0.010 mass %)
[0094] S is an element that is inevitably contained and deteriorates the weldability of the steel plate. Therefore, the S content is 0.010 mass % or less. The S content is preferably 0.0080 mass % or less, and more preferably 0.0050 mass % or less. Since the S content is preferably as small as possible, the lower limit is not particularly limited, but in industrial production, it is impossible to make the content reach 0 mass %, and it is usually higher than 0 mass %, and it can be contained at 0.00010 mass % or more.
[0095] (N: higher than 0 mass % and not more than 0.010 mass %)
[0096] N is an element that is inevitably contained. If it is contained excessively, AlN is generated, which reduces the deoxidation effect from Al. Therefore, the amount of N is 0.010 mass% or less. The amount of N is preferably 0.0080 mass% or less, and more preferably 0.0050 mass% or less. Since the amount of N is preferably as small as possible, the lower limit is not particularly limited, but in industrial production, it is impossible to make it reach 0 mass%, usually higher than 0 mass, and it can contain 0.00010 mass% or more.
[0097] (B: 0.0005 to 0.010 mass %)
[0098] B contributes to the high strength of steel parts by improving the hardenability of the steel sheet. In order to exert this effect, the B content is 0.0005 mass % or more, preferably 0.0010 mass % or more, and more preferably 0.0015 mass % or more.
[0099] On the other hand, if the B content becomes excessive, coarse iron-boron compounds precipitate and the toughness of the steel parts decreases. Therefore, the B content is 0.010 mass % or less, preferably 0.0080 mass % or less, and more preferably 0.0060 mass % or less.
[0100] (Remainder: Iron and inevitable impurities)
[0101] In a preferred embodiment, the balance is iron and inevitable impurities. Inevitable impurities are elements mixed in from the state of raw materials, materials, manufacturing equipment, etc.
[0102] In addition, for example, P, S, and N are usually unavoidable impurities, the smaller the content, the better, but their composition ranges are separately specified as described above. Therefore, in this specification, the term "unavoidable impurities" that constitute the balance is a concept that excludes elements whose composition ranges are separately specified.
[0103] Furthermore, the steel sheet according to the first embodiment of the present invention may selectively contain the following arbitrary elements as necessary, and the characteristics of the steel parts can be further improved according to the contained components.
[0104] (One or more selected from the group consisting of Cu: higher than 0 mass % and lower than 0.50 mass % and Ni: higher than 0 mass % and lower than 0.50 mass %)
[0105] By containing Cu, the corrosion resistance of the steel sheet itself is improved, so the generation of hydrogen caused by corrosion of the steel sheet can be suppressed, and the delayed fracture resistance is improved. In addition, Cu also has the effect of promoting the generation of thermodynamically stable protective iron oxide: α-FeOOH among the rust generated in the atmosphere. By achieving the promotion of the generation of this rust, the intrusion of the generated hydrogen into the steel sheet can be suppressed, and hydrogen-assisted cracking can be suppressed in a harsh corrosive environment. Therefore, it is preferred that the Cu content is higher than 0 mass%, more preferably 0.05 mass% or more, and further preferably 0.10 mass% or more. On the other hand, if the Cu content becomes excessive, the plating properties of the plating process during the manufacture of the steel sheet and the chemical treatment properties after hot stamping deteriorate. Therefore, it is preferred that the Cu content is 0.50 mass% or less.
[0106] It is known that Ni has the same effect as Cu. Therefore, the Ni content is also preferably higher than 0 mass%, more preferably 0.05 mass% or more, and further preferably 0.10 mass% or more. On the other hand, the Ni content is preferably 0.50 mass% or less.
[0107] (One or more selected from the group consisting of Ti: higher than 0 mass% and lower than 0.10 mass%, Cr: higher than 0 mass% and lower than 3.0 mass%, and Nb: higher than 0 mass% and lower than 0.10 mass%)
[0108] Ti reduces the amount of BN generated in the steel sheet by generating TiN. As a result, the amount of solid-solution B in the steel sheet can be increased, and the hardenability improvement effect from B can be enhanced. In order to exert this effect, the Ti content is preferably higher than 0 mass%, more preferably 0.0050 mass% or more, further preferably 0.0250 mass% or more, 0.050 mass% or more.
[0109] On the other hand, if the steel sheet contains excessive Ti, carbides will precipitate at the grain boundaries, and the hardenability of the steel sheet will deteriorate. Therefore, the Ti content is preferably 0.10 mass % or less, more preferably 0.080 mass % or less, and further preferably 0.070 mass % or less.
[0110] Cr helps to ensure hardness and helps to suppress the precipitation of coarse carbides during cooling. In order to exert these effects, the Cr content is preferably higher than 0 mass %.
[0111] On the other hand, if Cr is excessively contained in the steel sheet, cracks may occur in the steel sheet, and the Cr content is preferably 3.0 mass % or less, more preferably 2.5 mass % or less, and even more preferably 2.0 mass % or less.
[0112] Nb is a carbide-forming element and contributes to the refinement of the structure of the steel sheet. Therefore, the Nb content is preferably higher than 0 mass %, and more preferably 0.0050 mass % or more.
[0113] On the other hand, although the reverse phase transformation during heat treatment can be promoted by refining the structure of the steel sheet, it will promote the formation of ferrite during cooling, resulting in a decrease in the strength of the steel parts. This effect becomes greater as its content increases. In addition, the problem of deterioration of cold rolling properties may also occur. From this point of view, it is preferred to contain 0.10% by mass or less of Nb. Preferably, it is 0.070% by mass or less, and more preferably, it is 0.050% by mass or less.
[0114] (b) Heating process
[0115] In the first embodiment of the present invention, the steel sheet is heated to a temperature not lower than the Ac1 point (°C) and lower than the Ac3 point (°C) + 10°C.
[0116] If the temperature is lower than the Ac1 point, austenite transformation does not occur, and it is difficult to form a high-strength steel part after the cooling step (e) described later. On the other hand, by lowering the temperature to Ac3 point + 10°C in advance, the nucleation of ferrite and / or pearlite as soft structures is easily promoted in the processing step (c) described later.
[0117] The Ac1 point and the Ac3 point can be obtained by investigating the temperature during heating and the displacement history caused by the expansion and contraction of the steel accompanying the heating in a hot working simulation test. Figure 1 This is a graph showing the relationship between temperature and displacement when a steel plate is heated from a low temperature in a hot working simulation test. In the low temperature region, as the temperature rises, the steel can expand linearly with an expansion coefficient corresponding to the crystal structure (bcc) of ferrite. If the temperature is further increased, austenite with a denser crystal structure (fcc) can be generated and begins to shrink. The temperature at which the deviation from the straight line begins can be defined as the Ac1 point. In the high temperature region where the temperature is further increased, all ferrite transforms into austenite and can expand linearly again with an expansion coefficient corresponding to the crystal structure of austenite. The temperature at which linear expansion begins can be defined as the Ac3 point.
[0118] (c) Processing steps
[0119] After the above-mentioned heating step (b), processing is performed to apply a strain of 0.5% or more at a temperature of 675° C. or higher and lower than Ac3 point+10° C.
[0120] At the above temperature, a large number of crystal grain boundaries serving as nucleation sites of ferrite and / or pearlite as soft structures can exist in the steel plate. By applying a certain amount of strain (i.e., 0.5% or more) in such an unstable state, the nucleation of ferrite and / or pearlite as soft structures can be significantly promoted in the portion where the strain is applied. It is more preferable to apply a strain of 5.0% or more, and even more preferable to apply a strain of 9.0% or more.
[0121] In addition, the strain can be calculated by the following formula (1).
[0122] Strain (%) = |(d0-d1) / d0×100|…(1)
[0123] d0 is the thickness of the steel plate before processing or the thickness of the non-processed portion of the steel plate after processing, and d1 is the thickness of the processed portion of the steel plate after processing. The units are all mm.
[0124] The strain may be, for example, an equivalent plastic strain obtained by FEM analysis. That is, if the equivalent plastic strain obtained by FEM analysis is 0.5% or more, softening can be achieved in the same manner.
[0125] The Ms point can be obtained by examining the temperature during cooling and the displacement history due to expansion and contraction of steel during cooling in a hot working simulation test. Figure 2 Except Figure 1 In addition to the temperature-displacement relationship during heating, this diagram also shows the relationship between temperature and displacement when the steel plate is cooled at a faster cooling rate after heating. In the medium and high temperature range, as the temperature drops, the steel can shrink linearly at a shrinkage rate corresponding to the crystal structure of austenite. If the temperature is further lowered, it will transform into martensite and begin to expand. The temperature at which it starts to deviate from the straight line can be regarded as the Ms point.
[0126] On the basis of setting the heating temperature of the above-mentioned (b) heating step to be above the Ac1 point (°C) and below the Ac3 point (°C) + 10°C, if the processing temperature is set to be lower than 675°C, the phase transformation to the soft structure is active, so the softening of the non-processed part is also significant, making it difficult to manufacture steel parts in which only the processed part is locally softened.
[0127] On the basis of setting the heating temperature of the above-mentioned (b) heating step to be above Ac1 point (°C) and below Ac3 point (°C) + 10°C, if the processing temperature is set to be above Ac3 point + 10°C, the number of crystal grain boundaries serving as nucleation sites for the soft tissue will decrease, and only applying a certain strain will not promote the nucleation of the soft tissue.
[0128] The processing temperature may be the same as or different from the heating temperature of the heating step (b). If different, a supplementary heating step and / or cooling step may be included between the steps (b) and (c). In addition, a step of maintaining the temperature at a certain temperature may be included after the step (b) and before the step (c).
[0129] The above-mentioned processing may be any processing, and for example, press processing, bulging forming, forging, bending back during drawing, shearing, etc. can be used appropriately.
[0130] (d) Holding or slow cooling process
[0131] After the above-mentioned processing step (c), the steel is held or slowly cooled at an average cooling rate of 0 to 15°C / sec for 1 second or longer and 120 seconds or shorter. That is, the above-mentioned processing temperature is held for 1 second or longer and 120 seconds or shorter, or slowly cooled at an average cooling rate higher than 0°C / sec and less than 15°C / sec for 1 second or longer and 120 seconds or shorter. Thus, the ferrite and / or pearlite as the soft structure nucleated in the above-mentioned processing step (c) can be grown.
[0132] When the average cooling rate is higher than 15°C / second, or when the holding time or slow cooling time is lower than 1 second, ferrite and / or pearlite as soft structures cannot be fully precipitated and grown. The holding time or slow cooling time is preferably higher than 1 second, more preferably 3 seconds or more, and even more preferably 6 seconds or more.
[0133] On the other hand, if the holding or slow cooling time exceeds 120 seconds, ferrite and / or pearlite, which are soft structures, will also precipitate and grow in the non-processed portion, and high-strength steel parts cannot be obtained.
[0134] (e) Cooling process
[0135] After the above-mentioned (d) holding or slow cooling process, cool to Ms point (℃) - 50℃. At this time, the average cooling rate from the heating temperature of the above-mentioned (b) heating process (i.e., above Ac1 point (℃) and below Ac3 point (℃) + 10℃) to Ms point (℃) - 50℃ is controlled to be above 10℃ / second. As a result, at least in the non-processed part, martensitic transformation can be induced, and the strength of the non-processed part can be fully maintained. If the cooling with an average cooling rate of more than 10℃ / second ends at a temperature higher than Ms point (℃) - 50℃, martensitic transformation cannot be fully induced in the non-processed part. In addition, even if the average cooling rate is lower than 10℃ / second, martensitic transformation cannot be fully induced in the non-processed part.
[0136] After the cooling step (e) described above, the material may be cooled to room temperature, for example. The cooling rate from Ms point (° C.)-50° C. to room temperature is not particularly limited.
[0137] <Embodiment 2 of the present invention>
[0138] The manufacturing method of the second embodiment of the present invention is different from the manufacturing method of the first embodiment of the present invention in the conditions of the (b) heating step and the (c) processing step. These steps different from the first embodiment of the present invention are described below as the (b') heating step and the (c') processing step.
[0139] (b') Heating process
[0140] In the second embodiment of the present invention, the steel plate is heated to a temperature above Ac3 point (°C) + 10°C and below 1100°C. Unlike the first embodiment of the present invention, even if the steel plate is heated to above Ac3 point + 10°C in the heating process, if a relatively large strain is applied in the processing process (c') described later, the nucleation of ferrite and / or pearlite as soft structures can be significantly promoted, as in the first embodiment of the present invention. On the other hand, if the temperature is higher than 1100°C, the decarburization of the steel surface is significant and the target strength cannot be ensured. In addition, oxidation may also progress and cause thickness loss. If it is a plated material, oxidation or alloying proceeds, and the hardness of the plating becomes too high, resulting in problems such as peeling (oxidation and scratches of the steel plate) in subsequent processing steps.
[0141] (c') Processing steps
[0142] After the above-mentioned (b') heating process, a process of applying a strain of 10% or more is performed at a temperature of more than Ms point (℃) + 50℃ and less than Ac3 point (℃) + 10℃. When the temperature is more than Ms point (℃) + 50℃ and less than Ac3 point (℃) + 10℃, austenite is in a relatively unstable state. Therefore, by applying a relatively large (more than 10%) strain, the nucleation of ferrite and / or pearlite as soft tissue can be significantly promoted in the part where the strain is applied. It is more preferable to apply a strain of more than 15%, and it is further preferable to apply a strain of more than 40%. In addition, the strain can be calculated by the above formula (1). In addition, the strain can also be taken as an equivalent plastic strain obtained, for example, by FEM analysis. That is, if the equivalent plastic strain obtained by FEM analysis is more than 10%, it can also be softened.
[0143] At temperatures above Ac3 point + 10°C, austenite is in a relatively stable state, and even if a relatively large strain is applied, it is difficult to promote the nucleation of ferrite and / or pearlite as soft structures. On the other hand, if the temperature is lower than Ms point (°C) + 50°C, there is a possibility of causing martensitic transformation, and it is difficult to promote the nucleation of ferrite and / or pearlite as soft structures.
[0144] There is no particular limitation on the cooling from the temperature after the (b') heating step (above Ac3 point (℃) + 10℃ and below 1100℃) to the temperature of the (c') processing step (above Ms point (℃) + 50℃ and below Ac3 point (℃) + 10℃), and any average cooling rate may be used. In addition, a step of maintaining the temperature at a certain temperature may be included after the (b') step and before the (c') step.
[0145] The processing in the processing step (c') may be any processing, and for example, extrusion processing, bulging forming, forging, bending back during drawing, shearing, etc. can be used appropriately.
[0146] In the first and second embodiments of the present invention, the strains in the processing steps (c) and (c′) described above may be applied by multiple processing.
[0147] When the strain in the processing steps (c) and (c′) is applied by multiple processing, the strain of the multiple processing can be calculated as shown in the following formula (2).
[0148] [Formula 1]
[0149]
[0150] d n It is the thickness of the processed part of the steel plate after the nth processing, in mm.
[0151] The strain in the above formula (2) may be, for example, the sum of equivalent plastic strains obtained by FEM analysis after each processing.
[0152] For example, when the processing steps (c) and (c') are a single process, it may be difficult to apply a predetermined strain (0.5% or more in Embodiment 1, and 10% or more in Embodiment 2). In this case, it is advantageous to perform the processing steps (c) and (c') multiple times to accumulate the strain, thereby making it easier to make the strain reach a predetermined value or more.
[0153] In addition, when the processing steps (c) and (c') are a single process, the transport time from the steps (c) and (c') to the cooling step (e) is less than 1 second, and it may be difficult to ensure the time (1 second or more) for the holding or slow cooling step (d). In this case, it is advantageous to perform the steps (c) and (c') by multiple processing so that the transport time between the multiple processing steps can be used as the holding or slow cooling time for the step (d).
[0154] In addition, the above-mentioned multiple processing may include processing to apply deformation and processing to restore the deformation. In this way, the above-mentioned strain can be applied to the initial shape of the steel plate without changing the final shape of the steel part.
[0155] When the above-mentioned (c) and (c') processing steps include multiple processing, the above-mentioned (d) holding or slow cooling step can be performed after each processing. For example, when it includes two processings, the first holding or slow cooling step can be performed after the first processing, and then the second holding or slow cooling step can be performed after the second processing. In this case, the total time of the first holding or slow cooling step and the time of the second holding or slow cooling step is the time specified in the (d) step of embodiments 1 and 2 of the present invention, that is, more than 1 second and less than 120 seconds.
[0156] The temperatures in the above-mentioned steps (a) to (e), (b') and (c') are the surface temperatures of the steel plates (or steel parts) and can be measured using a thermocouple or a radiation thermometer. Alternatively, the corresponding relationship between the atmospheric temperature of the heating production line and the surface temperature of the steel plates (or steel parts) measured by the thermocouple may be investigated in advance, and the surface temperature of the steel plates (or steel parts) may be read from the atmospheric temperature of the heating production line.
[0157] According to the first and second embodiments of the present invention, it is possible to provide a method for manufacturing a high-strength steel part in which only a portion to which a predetermined strain or more is applied by processing is locally softened without performing local temperature control.
[0158] Example
[0159] The following examples are given to more specifically illustrate the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and can be appropriately modified within the scope of the above and below-mentioned purposes, which are all included in the technical scope of the embodiments of the present invention.
[0160] Example 1
[0161] Using the steel with the chemical composition shown in steel type No. A in Table 1 (Ac1 point: 778°C, Ac3 point: 875°C, Ms point: 385°C), a steel plate with a thickness of 1.6 mm and an area of 100 mm×100 mm was prepared, and the steel plate was heated to 880°C. After that, it was cooled to 750°C at a rate of about 12°C / sec, and bulging was performed at 750°C. The bulging was performed by pressing the central part of the 100 mm×100 mm steel plate from the back. The bulging height is 3.0 mm. After bulging, the bulging is slowly cooled at an average cooling rate of 10.8°C / sec for 6 seconds. Thereafter, water-cooled to Ms point (°C) - 50°C (i.e. 335°C), and the average cooling rate from 880°C to 335°C is 39.5°C / sec. Then, cooled to room temperature. The above is manufacturing example 1-2.
[0162] The Ac1 point, Ac3 point and Ms point are obtained by a hot working simulation test. The hot working simulation test is performed under the following conditions.
[0163] Thermal processing simulation (Formaster) testing machine: Fuji Denpako FTM-10
[0164] Test piece size: Thickness 2.0mm x Width 3.0mm x Length 10mm (two holes of Φ0.7mm x Depth 2.0mm are provided for inserting thermocouples)
[0165] Number of tests: 7 times (only the cooling speed was changed, and other conditions were constant)
[0166] Heating speed: 10℃ / s (room temperature ~ heating temperature)
[0167] Heating temperature: 950℃
[0168] Holding time at heating temperature: 180 seconds
[0169] Cooling rate: 2, 5, 10, 15, 20, 30 and 40℃ / s (heating temperature ~ room temperature)
[0170] In addition, in Table 1, the Cu content of steel type No. A is an unavoidable impurity level (less than 0.01 mass %), and therefore is described as "-".
[0171]
Table 1
[0172]
[0173] In order to evaluate the strain and hardness of the steel parts obtained in Manufacturing Example 1-2, the evaluation samples were extracted. The extraction positions of the evaluation samples are shown in Figure 3 In. Figure 3 As shown, a bulge formed portion A (25 mm in length and 5 mm in width) at the center of the steel part and a non-processed portion B (10 mm in length and 5 mm in width) at a position away from the bulge formed portion A in the longitudinal direction are extracted.
[0174] In order to evaluate the strain of the sample, the cross section was observed using an optical microscope to determine the plate thickness.
[0175] The plate thickness of the bulging forming portion A is obtained at the center of the steel part, a position 3.75 mm away from the center in the longitudinal direction (referred to as the middle portion), and a position 7.5 mm away from the center in the longitudinal direction (referred to as the edge portion). Then, using the above formula (1), the plate thickness of the center, middle, and edge of the steel part is set as the plate thickness d1 of the processed part, and the plate thickness of the non-processed portion B is set as the plate thickness d0 of the steel plate before processing, and the strain of the center, middle, and edge of the steel part is obtained.
[0176] The Vickers hardness was measured at three locations (central, middle, and edge) of the bulge forming portion A and the non-processed portion B. The measurement was performed using a Vickers hardness tester under the conditions of a load of 1 kg and a holding time of 10 seconds. When the plate thickness is d, the measurement position is measured at three points at a distance of d / 4 from the surface of the steel part in the plate thickness direction. Figure 4 yes Figure 3 The schematic cross-sectional view along the line X-X shown in the figure indicates the hardness measurement position of the bulging forming portion A.
[0177] The hardness measurement positions of the non-processed portion B are not shown in the figure, but the hardness is measured at three points: substantially the center of the non-processed portion B in the longitudinal and lateral directions and at a position d / 4 away from the surface of the steel part in the plate thickness direction.
[0178] The average value of the Vickers hardness at three locations (central portion, middle portion, and edge portion) of the bulge-formed portion A and three points of the unprocessed portion B was adopted as the respective Vickers hardnesses.
[0179] The temperature (°C) (referred to as forming temperature), bulging height (mm), cooling rate (°C / second) during slow cooling, slow cooling time (seconds), and average cooling rate (°C / second) from heating temperature to Ms point-50°C were changed in Manufacturing Example 1-2 to manufacture steel parts (referred to as Manufacturing Examples 1-1 and 1-3 to 1-8). Then, similarly to the steel parts obtained in Manufacturing Example 1-2, strain and Vickers hardness were evaluated for each steel part. The results are shown in Table 2.
[0180] In Table 2, underlined numerical values indicate values outside the range of Embodiment 1 of the present invention.
[0181]
Table 2
[0182]
[0183] Among manufacturing examples 1-1 to 1-8, when the Vickers hardness of at least one of the central portion, the middle portion, and the edge portion is compared with the Vickers hardness of the non-processed portion, the Vickers hardness is reduced by more than 20 HV, and the hardness of the non-processed portion is more than 310 HV. It is judged that the manufacturing example meets the standard of "locally softened high-strength steel parts".
[0184] In addition, as a "locally softened" steel part, a more preferred manufacturing example is that the Vickers hardness of at least one of the central part, the middle part and the edge part is reduced by 40 HV or more compared with the Vickers hardness of the non-processed part, and a further preferred manufacturing example is that the Vickers hardness is reduced by 100 HV or more.
[0185] In addition, as a "high-strength steel part", a more preferable manufacturing example is one in which the Vickers hardness of the non-processed portion is 400 HV or more, and a further preferable manufacturing example is one in which the Vickers hardness is 500 HV or more.
[0186] The same determination is made in Examples 2 and 3 described later.
[0187] The following observations can be made from the results in Table 2. Manufacturing Examples 1-1 to 1-4 in Table 2 are all examples that satisfy all the requirements specified in Embodiment 1 of the present invention, and can manufacture high-strength steel parts in which only portions subjected to a predetermined strain or more (0.5% or more in Embodiment 1 of the present invention) are locally softened without performing local temperature control.
[0188] On the other hand, Manufacturing Examples 1-5 to 1-8 in Table 2 do not satisfy the requirements specified in Embodiment 1 of the present invention, and cannot manufacture high-strength steel parts that are locally softened in portions where a specified strain or more (0.5% or more in Embodiment 1 of the present invention) is applied by processing.
[0189] In Manufacturing Examples 1-5 to 1-8, since the forming temperature is 650° C. or 550° C., which is lower than 675° C., the entire steel part including the non-processed portion is softened, and a locally softened high-strength steel part cannot be manufactured.
[0190] Example 2
[0191] A steel plate with a thickness of 1.6 mm and an area of 100 mm × 100 mm was prepared using the steel of the chemical composition shown in steel grade No. A in Table 1. The steel plate was heated to 880°C. Thereafter, the steel plate was cooled to 750°C at a rate of about 12°C / sec. The first bulging process was performed at 750°C. The first bulging process was performed by pressing the central portion of the 100 mm × 100 mm steel plate from the back. The bulging height is 3.0 mm. After the first bulging process, the bulging is slow-cooled at an average cooling rate of 10.8°C / second for 6 seconds. After the first slow cooling process, the second bulging process is performed. The second bulging process is performed by pressing the area where the first bulging process was performed from the opposite direction of the first bulging process (i.e., from the surface). The 2nd expansion process was followed by slow cooling at an average cooling rate of 6.7°C / sec for 6 seconds. After the second slow cooling process, the 2nd expansion process was followed by water cooling to Ms point (°C) -50°C (i.e., 335°C), with an average cooling rate of 26.2°C / sec from 880°C to 335°C. The 2nd expansion process was followed by slow cooling at an average cooling rate of 6.7°C / sec from 335°C to 880°C. The 2nd expansion process was followed by slow cooling at an average cooling rate of 26.2°C / sec from 335°C to 880°C. The 2nd expansion process was followed by slow cooling at an average cooling rate of 6.7°C / sec from 335°C to 880°C. The 2nd expansion process was followed by slow cooling at an average cooling rate of 26.2°C / sec from 335
[0192] For the steel parts obtained from Manufacturing Example 2-1, the strain and Vickers hardness were evaluated in the same manner as in Example 1. The strain was calculated using the above formula (2). In addition, the first bulging forming was performed in the same manner as Manufacturing Example 1-2, and the plate thickness after the first bulging forming was assumed to be the same as that of Manufacturing Example 1-2, thereby calculating the strain. The results are shown in Table 3. In addition, the second bulging forming was performed in the opposite direction to the first bulging forming, so the bulging height of the second bulging forming was a negative value.
[0193]
Table 3
[0194]
[0195] The following observations can be made from the results of Table 3. Manufacturing Example 2-1 in Table 3 is an example that satisfies all the requirements specified in Embodiment 1 of the present invention, and can manufacture a high-strength steel part in which only a portion subjected to a predetermined strain or more (0.5% or more in Embodiment 1 of the present invention) is locally softened without performing local temperature control.
[0196] Example 3
[0197] Using the steel with the chemical composition shown in Steel No. A in Table 1, a steel plate with a thickness of 1.6 mm and an area of 100 mm × 100 mm was prepared. The steel plate was heated to 950°C and held for 60 seconds. Thereafter, it was cooled to 550°C at a rate of about 12°C / second and bulging was performed at 550°C. The bulging was performed by pressing the central portion of the 100 mm × 100 mm steel plate from the back. The bulging height is 0.1 mm. After bulging, the bulging is slowly cooled at an average cooling rate of 4.7°C / sec for 6 seconds. Thereafter, water-cooling is performed to Ms point (°C) - 50°C (i.e. 335°C), and the average cooling rate from 950°C to 335°C is 12.5°C / sec. Thereafter, cooling is performed to room temperature. The above is Manufacturing Example 3-1.
[0198] The steel parts obtained in Manufacturing Example 3-1 were evaluated for strain and Vickers hardness in the same manner as in Example 1.
[0199] From Manufacturing Example 3-1, steel parts (referred to as Manufacturing Examples 3-2 to 3-19) were manufactured by changing the steel type, the temperature (°C) for bulging forming (referred to as forming temperature), the bulging height (mm), the cooling rate during slow cooling (°C / second), the slow cooling time (seconds), and the average cooling rate (°C / second) from the heating temperature to the Ms point-50°C. Then, as in Manufacturing Example 3-1, the strain and Vickers hardness were evaluated for each steel part. The results are shown in Tables 4 and 5. In addition, the steel with the chemical composition shown in Steel Type No. B in Table 1 has an Ac1 point of 778°C, an Ac3 point of 875°C, and an Ms point of 385°C.
[0200] In Tables 4 and 5, underlined numerical values indicate values outside the range of Embodiment 2 of the present invention.
[0201]
Table 4
[0202]
[0203]
Table 5
[0204]
[0205] The following observations can be made from the results of Tables 4 and 5. Manufacturing Examples 3-4 to 3-6, 3-9, 3-11, and 3-14 to 3-16 in Table 4 and Manufacturing Examples 3-20 to 3-27, 3-30 to 3-32, and 3-34 to 3-38 in Table 5 are all examples that satisfy all the requirements specified in Embodiment 2 of the present invention, and can manufacture high-strength steel parts in which only a portion to which a predetermined strain or more (10% or more in Embodiment 2 of the present invention) is applied by processing is locally softened without performing local temperature control.
[0206] On the other hand, manufacturing examples No. 3-1 to 3-3, 3-7 to 3-8, 3-10, 3-12 to 3-13, 3-17 and 3-19 in Table 4, and manufacturing examples 3-28, 3-29 and 3-33 in Table 5 are examples that do not satisfy the requirements specified in the second embodiment of the present invention, and high-strength steel parts that are locally softened in portions where a strain exceeding a specified value (10% or more in the second embodiment of the present invention) is applied by processing cannot be manufactured.
[0207] In Manufacturing Examples 3-1 to 3-3, 3-8, 3-10, 3-13 and 3-19 in Table 4 and Manufacturing Example 3-33 in Table 5, strains in the center, middle and edge portions were all less than 10%, and thus local softened high-strength steel parts could not be manufactured.
[0208] In manufacturing examples 3-7 of Table 4, the slow cooling rate in the (d) holding or slow cooling process is higher than 15°C / second (i.e., the slow cooling time is less than 1 second), and the strains in the central part, middle part, and edge part are all less than 10%, so it is impossible to manufacture high-strength steel parts that are locally softened.
[0209] In manufacturing examples 3-12 and 3-17 of Table 4 and manufacturing examples 3-28 and 3-29 of Table 5, since the cooling rate in the (d) holding or slow cooling step is higher than 15°C / second (i.e., the slow cooling time is less than 1 second), it is impossible to manufacture locally softened high-strength steel parts.
[0210] In addition, in manufacturing example 3-18 in Table 4, the strain applied by processing in the central part is 8%, which does not meet the strain of 10% or more specified in embodiment 2 of the present invention, but the hardness difference with the non-processed part is 20HV or more. This may be because in the central part of part No. 3-18, the manufacturing conditions other than the strain (heating temperature, cooling rate, slow cooling time, etc.) are preferred conditions, but the details are unclear.
[0211] Example 4
[0212] A steel plate with a thickness of 1.6 mm and an area of 100 mm × 100 mm was prepared using the steel of the chemical composition shown in steel grade No. A in Table 1. The steel plate was heated to 950°C. Thereafter, the steel plate was cooled to 750°C at a rate of about 12°C / sec and the first bulging was performed at 750°C. The first bulging was performed by pressing the central portion of the 100 mm × 100 mm steel plate from the back. The bulging height is 4.0 mm. After the first bulging process, the bulging is slow-cooled at an average cooling rate of 9.7°C / s for 6 seconds. After the first slow cooling process, the second bulging process is performed. The second bulging process is performed by pressing the area where the first bulging process was performed from the opposite direction of the first bulging process (i.e., from the surface). The 2nd expansion process was followed by slow cooling at an average cooling rate of 5.3°C / sec for 6 seconds. After the 2nd slow cooling process, the 2nd expansion process was followed by water cooling to Ms point (°C) -50°C (i.e., 335°C), and the average cooling rate from 950°C to 335°C was 16.6°C / sec. The 2nd expansion process was followed by slow cooling at an average cooling rate of 5.3°C / sec for 6 seconds. The 2nd expansion process was followed by water cooling to Ms point (°C) -50°C (i.e., 335°C), and the average cooling rate from 950°C to 335°C was 16.6°C / sec. The 2nd expansion process was followed by water cooling at an average cooling rate of ...
[0213] For the steel parts obtained by Manufacturing Example 4-1, the strain and Vickers hardness were evaluated in the same manner as in Example 1. The strain was calculated using the above formula (2). In addition, since it was separately confirmed that the plate thickness of the central portion when the second bulging forming was not performed in Manufacturing Example 4-1 was 1.39 mm, the plate thickness of the middle portion was 1.22 mm, and the plate thickness of the edge portion was 1.58 mm, these plate thicknesses were used as the plate thickness after the first bulging forming of Manufacturing Example 4-1, and the strain was calculated. The results are shown in Table 6. In addition, since the second bulging forming was performed in the opposite direction to the first bulging forming, the second bulging height was a negative value.
[0214]
Table 6
[0215]
[0216] The results of Table 6 allow the following considerations. Manufacturing Example 4-1 in Table 6 satisfies all the requirements specified in Embodiment 2 of the present invention, and can manufacture a high-strength steel part in which only a portion subjected to a predetermined strain or more (10% or more in Embodiment 2 of the present invention) is locally softened without performing local temperature control.
[0217] Possibility of Industrial Application
[0218] According to an embodiment of the present invention, a method for manufacturing a locally softened high-strength steel part without performing local temperature control can be provided. Such a high-strength steel part is suitable for automobile frame raw materials, for example.
[0219] Explanation of symbols
[0220] 1 Steel parts
[0221] 2 Hardness measurement of the center part 1st position
[0222] 3. Second position for measuring hardness in the center
[0223] 4 Hardness measurement of the center part (3rd position)
[0224] 5. Hardness measurement of the middle part, first position
[0225] 6 Middle part hardness measurement second position
[0226] 7 Hardness measurement of the middle part 3rd position
[0227] 8 Edge hardness measurement position 1
[0228] 9 Edge hardness measurement second position
[0229] 10 Edge hardness measurement position 3
[0230] A Bulging forming part
[0231] B Non-processing department
[0232] The present application claims priority based on Japanese Patent Application No. 2020-042274 filed on March 11, 2020 and Japanese Patent Application No. 2020-172764 filed on October 13, 2020. Japanese Patent Application No. 2020-042274 and Japanese Patent Application No. 2020-172764 are incorporated herein by reference.
Claims
1. A method for manufacturing a steel part, wherein: Including the following processes: A process for preparing a steel plate having a chemical composition comprising: C: 0.05 to 0.40 mass %, Si: 0-2.0 mass %, Mn: 1.0 to 3.0 mass %, Al: 0.010 to 1.0 mass %, P: more than 0 mass % and less than 0.100 mass %, S: more than 0 mass % and less than 0.010 mass %, N: more than 0 mass % and less than 0.010 mass %, B: 0.0005 to 0.010 mass %, At least one of the following (a) and (b): (a) one or more selected from the group consisting of Cu: higher than 0 mass % and lower than 0.50 mass % and Ni: higher than 0 mass % and lower than 0.50 mass %, (b) one or more selected from the group consisting of Ti: higher than 0 mass % and lower than 0.10 mass %, Cr: higher than 0 mass % and lower than 3.0 mass %, and Nb: higher than 0 mass % and lower than 0.10 mass %, and Balance: Iron and unavoidable impurities; A heating step of heating the steel plate to a temperature that is higher than the Ac1 point and lower than the Ac3 point + 10°C; After the heating step, a processing step of applying a strain of 0.5% or more to a portion of the steel plate to be softened at a processing temperature of 675° C. or more and lower than Ac3 point+10° C.; After the processing step, a holding or slow cooling step of holding the processing temperature for 1 second to 120 seconds, or slow cooling at an average cooling rate higher than 0°C / second and less than 15°C / second for 1 second to 120 seconds; After the holding or slow cooling step, a step of cooling to Ms point - 50°C is performed. The average cooling rate from the temperature in the heating step to Ms point - 50°C is controlled to be 10°C / sec or more, The units of the Ac1 point, Ac3 point and Ms point are °C.
2. A method for manufacturing a steel part, wherein: Including the following processes: A process for preparing a steel plate having a chemical composition comprising: C: 0.05 to 0.40 mass %, Si: 0-2.0 mass %, Mn: 1.0 to 3.0 mass %, Al: 0.010 to 1.0 mass %, P: more than 0 mass % and less than 0.100 mass %, S: more than 0 mass % and less than 0.010 mass %, N: more than 0 mass % and less than 0.010 mass %, B: 0.0005 to 0.010 mass %, At least one of the following (a) and (b): (a) one or more selected from the group consisting of Cu: higher than 0 mass % and lower than 0.50 mass % and Ni: higher than 0 mass % and lower than 0.50 mass %, (b) one or more selected from the group consisting of Ti: higher than 0 mass % and lower than 0.10 mass %, Cr: higher than 0 mass % and lower than 3.0 mass %, and Nb: higher than 0 mass % and lower than 0.10 mass %, and Balance: Iron and unavoidable impurities; A heating step of heating the steel plate to a temperature of Ac3 point+10°C or higher and 1100°C or lower; After the heating step, a processing step of applying a strain of 10% or more to a portion of the steel plate to be softened at a processing temperature of Ms point + 50°C or more and lower than Ac3 point + 10°C; After the processing step, a holding or slow cooling step of holding at the processing temperature for 1 second to 120 seconds, or slow cooling at an average cooling rate higher than 0°C / second and less than 15°C / second for 1 second to 120 seconds; After the holding or slow cooling step, the step of cooling to Ms point - 50°C is performed. The average cooling rate from the temperature in the heating step to Ms point - 50°C is controlled to be 10°C / sec or more, The units of the Ac3 point and the Ms point are °C.
3. The manufacturing method according to claim 1 or 2, wherein: This includes applying the strain by bulging.
4. The manufacturing method according to claim 1 or 2, wherein: Including applying the strain by forging.
5. The manufacturing method according to claim 1 or 2, wherein: This includes applying the strain by bending back during drawing.
6. The manufacturing method according to claim 1 or 2, wherein: Including applying the strain by shearing.
7. The manufacturing method according to claim 1 or 2, wherein: This includes applying the strain through multiple processes.
8. The manufacturing method according to claim 7, wherein: The multiple processing includes processing for applying deformation and processing for recovering the deformation.