A polyvinylidene fluoride submicron thin fiber membrane prepared by heating stretching method
By heating and stretching the PVDF film after electrospinning, combined with the use of SiC and GO, the problem of β crystalline content and fiber refinement in PVDF was solved, and its piezoelectric and mechanical properties were significantly improved, making it suitable for modern applications. electronic devices.
Patent Information
- Application Number
- CN202111600822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-24
AI Technical Summary
It is difficult to effectively increase the β crystalline content and fiber refinement in polyvinylidene fluoride (PVDF) with existing technology, resulting in its deficiencies in piezoelectric properties and mechanical properties and its inability to meet the high requirements of modern electronic devices for dielectric materials.
The heated stretching method is used to dissolve PVDF, silicon carbide (SiC) and graphene oxide (GO) in a specific solvent, electrospinning and then heated and stretched to increase the β crystal content and refine the fiber membrane, thereby improving its Thermal conductivity and mechanical properties.
It has improved the beta crystal content and fiber refinement of the PVDF film, improved its piezoelectric properties and mechanical properties, and is suitable for fields such as nano piezoelectric generators and battery separators.
Smart Images

Figure CN115287822B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electrostatic spinning nanofiber membranes, and in particular relates to a polyvinylidene fluoride submicron thin fiber membrane prepared based on a heating stretching method and a preparation method thereof. Background Art
[0002] In recent years, nonwovens have developed rapidly, among which electrospun nanofiber membranes have attracted more and more attention and have been applied in many fields, with a very fast growth rate. The application of electrospun nanofiber membranes in current life is ubiquitous, such as mask production, air purifier filter elements, mask cloths, nanofiber membrane water purifiers, anti-haze windows, etc., which have provided us with countless conveniences. With the development of science and technology, people have higher and higher requirements for dielectric materials. Traditional dielectric materials can no longer meet the requirements of environmental protection and performance. In today's increasingly miniaturized electronic devices, PVDF piezoelectric materials are widely used for their good piezoelectric properties, good flexibility, and fast response speed. However, most of the excellent properties of polyvinylidene fluoride come from its crystal structure. At present, PVDF has several different crystal forms such as α, β, γ and δ. These crystal forms can be transformed into each other, among which the β phase is the most piezoelectric crystal form. Therefore, improving piezoelectric performance is ultimately achieved by increasing the content of β crystal form in PVDF.
[0003] Electrospinning technology, namely polymer jet electrostatic stretching spinning, is a new fiber preparation technology that is completely different from conventional spinning. The basic principle is that when an external electric field acts on the surface of the capillary liquid, the polymer melt or solution carries a large amount of electrostatic charge. As the electric field force increases, the polymer melt or solution overcomes its surface tension to form a jet stream. During the jetting process, the solvent continues to evaporate and solidify, and finally forms a fine fiber aggregate on the receiving device. Due to its simple operation, wide applicability and low cost, electrospinning has become a research hotspot in the field of nanofiber spinning. Although in theory electrospinning is a method suitable for preparing ultrafine fibers, in actual operation most of them are micron or submicron fibers. Based on this, how to develop a method for thinning polyvinylidene fluoride fibers has become a research hotspot for polyvinylidene fluoride membranes. Summary of the invention
[0004] The purpose of the present invention is to provide a polyvinylidene fluoride submicron fine fiber membrane prepared based on a heating and stretching method. First, polyvinylidene fluoride (PVDF), silicon carbide (SiC) and graphene oxide (GO) are dissolved in N,N-dimethylformamide (DMF) and tetrahydrofuran (THF), and then put into a disposable syringe and placed on an electrospinning machine to spin a polyvinylidene fluoride submicron fiber membrane. By increasing the thermal conductivity, mechanical properties and β crystals, the polyvinylidene fluoride membrane is given more β crystals. By heating and stretching, on the one hand, the β crystal content of polyvinylidene fluoride can be increased, and on the other hand, a finer fiber membrane can be obtained, which can be used in the fields of nano piezoelectric generators, battery separators, etc.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A method for preparing a polyvinylidene fluoride submicron thin fiber membrane based on a heating and stretching method comprises the following steps:
[0007] (1) Dissolve a certain amount of PVDF, SiC and GO in DMF, heat to 70°C and stir for 6h-8h, then add THF and stir at room temperature for 18h-20h, and after sufficient stirring, obtain a PVDF solution;
[0008] (2) The PVDF solution is placed in a needle tube, and then placed on an electrospinning machine for electrospinning. The sprayed PVDF nanomembrane is received by a receiving roller, and the PVDF nanomembrane obtained by spinning is placed in an oven for drying to obtain a polyvinylidene fluoride submicron fiber membrane.
[0009] (3) The obtained polyvinylidene fluoride submicron fine fiber membrane is heated and stretched, so as to obtain the polyvinylidene fluoride submicron fine fiber membrane prepared by the heating and stretching method.
[0010] In the above technical solution, further, in step (1), PVDF, SiC and GO are added to DMF and THF in the PVDF solution so that the PVDF concentration is 6 wt%.
[0011] Furthermore, in step (1) the mass of DMF in the PVDF solution: the mass of THF = 1:1.
[0012] Furthermore, in step (1), the mass of SiC is 0.5wt%-0.7wt%, and the mass of GO is 0.1wt%-0.3wt%.
[0013] Furthermore, in step (2), the spinning voltage is 20 kV, the propulsion speed is 1 mL / h, and the receiving distance is 11 cm.
[0014] The drum speed is 80r / min.
[0015] Furthermore, in step (3), the stretching speed is 0.001-0.02 cm / sec, and the stretching temperature is 20°C-60°C.
[0016] The above technical solution has the following beneficial effects:
[0017] The present invention utilizes silicon carbide (SiC) as a filler to improve the dielectric properties of PVDF solution. The negative surface charge of the filler interacts with the -CH2 group of PVDF, and the positive charge interacts with the -CF2 of PVDF, thereby helping to induce a fully reverse polarity β crystal. Graphene oxide (GO) has good thermal conductivity, which is more conducive to later heating and stretching. In addition, it can effectively increase the sensitivity and mechanical properties of the PVDF film. At the same time, the PVDF film is stretched, on the one hand, an ultrafine nanofiber film can be obtained, and on the other hand, the number of β crystals can be increased again, and finally a PVDF ultrafine nanofiber film with good piezoelectric properties is obtained. The method of the present invention has a simple operation procedure, low equipment requirements, and is easy to promote and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings:
[0019] Figure 1 This is a scanning electron microscope image of the polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method obtained in Example 1;
[0020] Figure 2 is a scanning electron microscope image of the polyvinylidene fluoride submicron fiber membrane in Example 1;
[0021] Figure 3 The stress-strain diagram of the polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method at different speeds obtained in Example 1;
[0022] Figure 4 The stress-strain diagram of the polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method obtained in Example 1 at different temperatures;
[0023] Figure 5 This is the stress-strain diagram of the polyvinylidene fluoride submicron fiber membrane at different speeds in Example 1. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with embodiments:
[0025] In the following examples, unless otherwise specified, the reagents, materials and equipment used can be purchased from commercial sources or prepared by conventional methods.
[0026] Example 1
[0027] (1) PVDF, SiC and GO were dissolved in DMF, heated to 70 °C and stirred for 6 h, then THF was added and stirred at room temperature for 18 h (DMF:THF=1:1), and a 6 wt% PVDF solution was obtained by sufficient stirring, wherein the mass concentrations of the components were: PVDF 6 wt%, SiC 0.5 wt%, GO 0.1 wt%;
[0028] (2) placing the prepared PVDF solution into a disposable syringe, and then placing it on an electrospinning machine for electrospinning, using a voltage of 20 kV, a propulsion rate of 1 mL / h, a receiving distance of 11 cm, and a drum speed of 80 r / min for electrospinning, and placing the PVDF nanofilm obtained by spinning in an oven for drying;
[0029] (3) The obtained polyvinylidene fluoride submicron fiber membrane is uniaxially stretched at a temperature of 40° C. and a speed of 0.001 cm / sec, thereby obtaining a polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method.
[0030] According to tests, in the polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method, the proportion of 0-50nm is 1.67%, the proportion of 50-100nm is 40%, the proportion of 100-150nm is 35%, the proportion of 150-200nm is 16.67%, the proportion of 200-250nm is 5%, and the proportion of 250-300nm is 1.67%.
[0031] In addition, when SiC and GO are not added to the solution, the same process parameters are used, namely 20kV voltage, 1mL / h propulsion rate, 11cm receiving distance, and 80r / min drum speed. The diameters of the nanofiber membranes obtained after stretching under the same conditions are as follows: 0-50nm accounts for 0%, 50-100nm accounts for 1.67%, 100-150nm accounts for 11.67%, 150-200nm accounts for 26.67%, 200-250nm accounts for 30%, 250-300nm accounts for 16.67%, 300-350nm accounts for 11.67%, and 350-400 accounts for 1.67%. It is obvious that the fiber diameter without adding SiC and GO and using the same process parameters is much larger than the fiber diameter with SiC and GO added and the process parameters adjusted. This also verifies the correctness of our solution.
[0032] In addition, we Figure 3 and Figure 5 It can also be seen that under the same conditions, the one with added particles can be stretched to 70%, and the one without added particles can be stretched to about 50%; Figure 4It can be seen that under the same conditions, when the temperature is 20°C (without heating), it can be stretched to about 70%, but when the temperature is heated to 40°C, it can be stretched to about 90%. This also shows the advantages of adding particles and heating.
[0033] Example 2
[0034] (1) PVDF, SiC and GO were dissolved in DMF, heated to 70 °C and stirred for 6 h, then THF was added and stirred at room temperature for 18 h (DMF:THF=1:1), and fully stirred to obtain an 8 wt% PVDF solution, wherein the mass concentration of each component was: PVDF 8 wt%, SiC 0.7 wt%, GO 0.3 wt%;
[0035] (2) placing the prepared PVDF solution into a disposable syringe, and then placing it on an electrospinning machine for electrospinning, using a voltage of 20 kV, a propulsion rate of 1 mL / h, a receiving distance of 11 cm, and a drum speed of 80 r / min for electrospinning, and placing the PVDF nanofilm obtained by spinning in an oven for drying;
[0036] (3) The obtained polyvinylidene fluoride submicron fiber membrane is uniaxially stretched at a temperature of 40° C. and a speed of 0.001 cm / sec, thereby obtaining a polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method.
[0037] After testing, in the polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method, the proportion of 0-50nm is 0.67%, the proportion of 50-100nm is 35%, the proportion of 100-150nm is 30%, the proportion of 150-200nm is 16.67%, the proportion of 200-250nm is 15%, and the proportion of 250-300nm is 2.67%.
[0038] Example 3
[0039] (1) PVDF, SiC and GO were dissolved in DMF, heated to 70 °C and stirred for 6 h, then THF was added and stirred at room temperature for 18 h (DMF:THF=1:1), and a 6 wt% PVDF solution was obtained by sufficient stirring, wherein the mass concentrations of the components were: PVDF 6 wt%, SiC 0.5 wt%, GO 0.1 wt%;
[0040] (2) placing the prepared PVDF solution into a disposable syringe, and then placing it on an electrospinning machine for electrospinning, using a voltage of 20 kV, a propulsion rate of 1 mL / h, a receiving distance of 11 cm, and a drum speed of 80 r / min for electrospinning, and placing the PVDF nanofilm obtained by spinning in an oven for drying;
[0041] (3) The obtained polyvinylidene fluoride submicron fiber membrane is uniaxially stretched at a temperature of 40° C. and a speed of 0.001 cm / sec, thereby obtaining a polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method.
[0042] According to tests, in the polyvinylidene fluoride submicron fine fiber membrane prepared by the heating stretching method, the proportion of 0-50nm is 1%, the proportion of 50-100nm is 38%, the proportion of 100-150nm is 30%, the proportion of 150-200nm is 23.67%, the proportion of 200-250nm is 5.43%, and the proportion of 250-300nm is 2%.
[0043] The above is only a specific implementation of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. A polyvinylidene fluoride submicron fine fiber membrane prepared by a heating stretching method, characterized in that: The steps include: (1) Dissolve PVDF, SiC and GO in DMF, heat to 70°C and stir for 6-8h, then add THF and stir at room temperature for 18-20h to obtain a PVDF solution; (2) placing the PVDF solution obtained in step (1) into a needle tube, and then placing it on an electrospinning machine for electrospinning, receiving the sprayed PVDF nanomembrane by a receiving roller, and drying the PVDF nanomembrane in an oven to obtain a polyvinylidene fluoride submicron fiber membrane; (3) The polyvinylidene fluoride submicron fiber membrane obtained in step (2) is heated and stretched at a speed of 0.001-0.02 cm / sec and a temperature of 20°C-60°C, thereby obtaining a polyvinylidene fluoride submicron fine fiber membrane prepared by the heating and stretching method.
2. The polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method according to claim 1, characterized in that: Step (1) In the PVDF solution, the concentration of PVDF is 6wt%-8wt%, the concentration of SiC is 0.5wt%-0.7wt%, and the concentration of GO is 0.1wt%-0.3wt%.
3. The polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method according to claim 1, characterized in that: Step (1) The mass of DMF in the PVDF solution: the mass of THF = 1:
1.
4. The polyvinylidene fluoride submicron thin fiber membrane prepared by the heating stretching method according to claim 1, characterized in that: During electrospinning, the spinning voltage was 20 kV, the needle tube advancement speed was 1 mL / h, the receiving distance was 11 cm, and the receiving roller speed was 80 r / min.
Citation Information
Patent Citations
Hollow fiber membrane stretching device
CN103055708A
Wet spinning radiation refrigeration fiber as well as preparation method and application thereof
CN112853522A