A production process of LiF thermoluminescent material detector
By adding barium and BaF2 to the LiF:Mg, Cu, P detector, the problem of low response in the low energy range is solved, meeting the new requirements reported by the ICRU, and the dose closer to tissue equivalence is achieved The characteristics are suitable for any LiF thermal light detector manufacturer.
Patent Information
- Application Number
- CN202210897945.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-28
AI Technical Summary
The existing LiF: Mg and Ti detectors are not proportional to the thermal emission yield when the radiation volume changes, resulting in abnormally low response within the low energy range and failing to meet the personal dose equivalent H (10) and surrounding doses proposed by the ICRU report. The new requirement of equivalent H*(10), and due to the addition of copper impurities, the radiation energy received by the detector in practical applications is not accurate.
By adding trace amounts of barium to the LiF:Mg, Cu, P detector, adjusting its atomic number to approach tissue equivalence, and using BaF2 as a dopant to maintain the thermal light-emitting sensitivity of the original material unchanged, satisfying New dosage properties requirements.
Realizes the flat response and uplift response of LiF:Mg, Cu, P detectors in the low energy segment, meets the new requirements reported by ICRU, and the addition of barium elements does not require changes to the existing production process, and is suitable for any LiF thermal light detection , the manufacturer provides dosage properties closer to tissue equivalence.
Smart Images

Figure CN115308786B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radiation protection dosimetry, and in particular to a production process of a LiF thermoluminescent material detector. Background Art
[0002] With the expansion of application fields and the improvement of measurement accuracy requirements, the sensitivity of LiF:Mg, Ti detectors cannot meet the new demands of the application market.
[0003] In order to improve the accuracy of LiF detectors in dose measurement, Japan has successively developed LiF:Mg, Cu and LiF:Mg, Cu, P detectors, with the sensitivity increased from five times to nearly thirty times that of LiF:Mg, Ti. However, in the use of these two detectors and the study of their dosimetric characteristics, it was found that due to the incorporation of copper (Cu) impurities, when they detect rays of the same radiation amount but different photon energies, the thermoluminescence yield (sensitivity intensity) released by the two detectors is not in direct or inverse proportion to the positive or negative changes in the radiation amount, but shows an abnormally low phenomenon in the photon range of 80KeV energy, which is called "under-response" in this academic field. This does not conform to the two new physical practical quantities proposed in ICRU (International Commission on Radiation Units and Measurements) Reports 39 and 43, namely: the new requirements for personal dose equivalent H(10) and ambient dose equivalent H*(10); personal dose equivalent H(10) is the dose equivalent received by soft tissue at a depth of 10mm below a specified point on the human body; H*(10) is the dose equivalent received in a radioactive environment, such as around a nuclear reactor and other radioactive devices. The two reports require that in free air, after being properly filtered when worn on a human model or on the chest of a human body, the detector can basically meet the traditional low-energy photon energy response curve Hp(10) being flat (basically close to the new requirement of the energy response curve of lithium borate (Li2B4O7)), and can also meet the new requirement of H*(10) protrusion proposed in ICRU Report No. 39. This requires that the detector with LiF as the matrix material must meet the requirement of Hp(10) being flat in the energy range below 1250KeV and the new requirement of H*(10) protrusion in the low energy range when used for monitoring the two quantities.
[0004] In order to meet the new requirements of the above two physical quantities, the current application field is to encapsulate the sheet-shaped thermoluminescent detector with LiF as the matrix material in a plastic box called a dose box with an effective atomic number Zff close to the body tissue, and then add a metal (copper, tin, lead) sheet called a filter on the radiation incident direction of the sheet to perform the so-called "energy response modification"; this combination of the dose box, metal filter and detector is called a dosimeter. It is not difficult to see from the structure of the dosimeter that in actual application of the dosimeter, the radiation received by the thermoluminescent detector is filtered by the filter, and when the dosimeter is worn on the human body, the radiation received by the human body in the radiation field is not filtered; therefore, it is inaccurate to use the radiation energy received by the detector to evaluate the radiation energy received by human tissue.
[0005] In order to improve the dosimetric characteristics of the above-mentioned detectors with LiF as the matrix material and make them meet the new requirements of personal dose equivalent H(10) and ambient dose equivalent H*(10) proposed in ICRU Report No. 39, it is necessary to seek the incorporation of a new functional impurity element so that the new detectors can not only meet the new requirements of the above two physical quantities of detectors with LiF as the matrix material represented by LiF:Mg,Cu,P, but also maintain their original high thermoluminescence sensitivity unchanged and be closer to tissue equivalence.
[0006] In view of this, a production process of LiF thermoluminescent material detector is proposed. Summary of the invention
[0007] In order to solve the above disadvantages of the prior art, the present invention provides a production process of a LiF thermoluminescent material detector. The present invention is implemented through the following technical solutions.
[0008] A production process of a LiF thermoluminescent material detector comprises the following steps:
[0009] S1: Ingredients
[0010] 1.1: The raw material component ratio of the experimental sample is: 20 grams of prepared LiF:Mg, Cu, P, Ba powder to be pressed into tablets, the amount of raw material components of LiF:Mg, Cu, P, Ba powder to be pressed into tablets per 1g of lithium fluoride is: phosphoric acid is 0.031190496ml, magnesium oxide is 0.0031087g, copper fluoride is 0.000607g, barium fluoride for personal dose detector is 0.00805g, barium fluoride for environmental dose monitoring detector is 0.01345g, lithium fluoride is 1g;
[0011] S2: Firing polycrystalline
[0012] 2.1: Turn on the power of the commercial tubular sintering furnace, set the constant temperature of the control program to 950℃, and heat it up. At the same time, connect the tubular furnace and the nitrogen cylinder through a pressure reducing table with a flow meter. After the temperature is constant at 950℃, proceed to the next step;
[0013] 2.2: Take 20g of the powder prepared in S1 and put it in a 50ml platinum crucible, cover it tightly and place it on the crucible bracket, then move it into a constant temperature tube furnace and push it into the center of the tube furnace, connect the exhaust pipe cover at the inlet, unscrew the valve of the nitrogen cylinder in time, adjust the flow rate to 2L / min, and start timing when the temperature rises back to 950℃;
[0014] 2.3: When the timing reaches 30 minutes, turn on the power of the cooling fan, remove the exhaust pipe at the inlet of the tube furnace, pull the crucible bracket out to the furnace tube mouth, use a large long-handled tweezers or long flat-nosed pliers to move the bracket to the side of the fan, and then use crucible tongs to move the crucible under the fan to cool it quickly, and close the nitrogen bottle valve and the power button;
[0015] 2.4: After the crucible is cooled under the fan for 6-10 minutes, the multi-crystal blocks in the crucible will automatically separate from the crucible. The crucible should be removed in time to allow the crystal blocks to directly receive the cold air from the fan, which will cool them down faster. After they reach room temperature, they can be crushed.
[0016] S3: Crushing polycrystalline
[0017] 3.1: Place the LiF:Mg, Cu, P, Ba polycrystalline block in a porcelain mortar, hit it into small pieces with appropriate force, further grind it into powder, and immediately use a 60-mesh standard sieve to sieve out the powder with less than 60 mesh for tableting;
[0018] S4: Pressing
[0019] 4.1: Use a single-punch tablet press for the pharmaceutical industry, equipped with a Φ4.5mm die, to punch out round tablets with a thickness of 0.8mm. Different specifications of dies can be selected as needed to press round tablets of different diameters and thicknesses;
[0020] S5: High temperature sintering
[0021] 5.1: The purpose of high temperature sintering is to make the pressed tablets have sufficient mechanical strength in application. Take 15 pressed tablets and place them in a platinum box;
[0022] 5.2: According to the method in 2.1 of process S2, set the temperature control program of the tubular sintering furnace to 660℃, turn on the power to heat it up, replace the nitrogen cylinder with an oxygen cylinder, and after the furnace temperature stabilizes, put the platinum box containing 15 tablets, according to the operation procedure in 2.2 of S2, unscrew the valve of the oxygen cylinder, adjust the flow rate to 3-5 liters / minute, and start timing when the temperature rises back to 660℃;
[0023] 5.3: When the timing reaches 30 minutes, the subsequent procedure is the same as the method in 2.3 of S2. After the platinum box is cooled to room temperature, the detector is taken out;
[0024] S6: Performance Testing
[0025] 6.1: Low temperature annealing: Take a few newly prepared LiF:Mg, Cu, P, Ba detectors at random, place them in the annealing tray and put them in the center of the annealing furnace, close the furnace door, turn on the annealing furnace power switch, and strictly anneal according to the 240℃ / 10 minute annealing program;
[0026] 6.2: Irradiation: After annealing, the detector is irradiated with an experimental dose of an americium radiation source with an energy of about 50 KeV;
[0027] 6.3: Reading: Obtain the luminescence curve and relative thermoluminescence sensitivity using a RGD-3 TL reader.
[0028] Furthermore, in S4, the powder is pressed into large blocks through hot pressing technology, and then cut into square and strip detectors of different specifications as needed.
[0029] Beneficial effects of the present invention:
[0030] 1. The irreplaceable advantage of the present invention is that the atomic number of barium is much smaller than that of lead, which determines that by adding only a trace amount of barium (Ba) element to the LiF:Mg, Cu, (P, Si, Ag)Ba detector, a new dosimetric characteristic close to tissue equivalence can be given, so that it can meet the new requirements of the relevant ICRU report, and the mass component ratio and other dosimetric characteristics of the thermoluminescent detector with LiF, Mg and Cu as raw materials remain unchanged;
[0031] 2. The addition of barium (Ba) element completely continues the original production process of LiF: Mg, Cu, P detectors, without making new changes or adding any equipment; therefore, any manufacturer of LiF thermoluminescent detectors at home and abroad can produce new LiF: Mg, Cu, (P, Si, Ag, etc.) Ba thermoluminescent detectors that need to improve low-energy response;
[0032] 3. The present invention adopts the measure of new additive BaF2 to endow LiF:Mg, Cu, (P, Si, Ag)Ba detector with new dosimetric characteristics. This is carried out under the condition that it is known that barium (Ba) element has a specific function for low-energy radiation. This is completely different from the impurity elements doped into all early detectors, which are known through a large number of experiments. Therefore, it has certain guiding significance for the research and development of detectors in the future;
[0033] 4. Among the alkaline earth elements in the periodic table, except for radium (Ra), all are members of the thermoluminescent detector family, and barium (Ba) and beryllium (Be) have specific functions for low-energy radiation, that is, barium (Ba) has the specific function of absorbing low-energy radiation, and beryllium (Be) has the specific function of transmitting low-energy radiation. The specific functions of the two may have theoretical and practical guiding significance for the adjustment of the energy dependence of solid dose detectors in the future.
[0034] 5. Since the new thermoluminescent detectors of LiF:Mg, Cu, P, Ba can be cut into 1×1×1mm or punched into ¢1×1mm scale, they can be placed in any desired position in the body through minimally invasive technology. Their application in in vivo diagnosis and treatment in radiation medicine cannot be replaced by other electronic dose monitoring instruments. Therefore, their application in this field will show incomparable superiority. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a process flow chart of the present invention;
[0036] Figure 2 Comparison of photon energy dependence of LiF:Mg, Cu, P, and Ba detectors with different barium doping amounts;
[0037] Figure 3 The photon energy dependence curve of the barium doping amount that meets the Hp(10) and H*(10) requirements. DETAILED DESCRIPTION
[0038] The scheme of the present invention is described in more detail and completely below.
[0039] Specific embodiment 1, a production process of a LiF thermoluminescent material detector, comprises the following steps:
[0040] S1: Ingredients
[0041] 1.1: The raw material component ratio of the experimental sample is: 20 grams of prepared LiF: Mg, Cu, P, Ba powder to be pressed into tablets. In S1, the amount of the raw material components of LiF: Mg, Cu, P, Ba powder to be pressed into tablets per 1g of lithium fluoride is shown in Table 1:
[0042] Table 1: Raw material composition ratio of LiF:Mg, Cu, P, Ba detector
[0043]
[0044] Note: During the production process, the amount of barium fluoride added to the detector used for personal dose is based on the amount of H(10), and the amount of barium fluoride added to the detector used for environmental dose monitoring is based on the amount of H*(10). The product name of the LiF:Mg, Cu, P thermoluminescent detector in actual application is named GR-200; for ease of application, the new LiF:Mg, Cu, P, Ba detector used for personal dose monitoring of H(10) is named GR-400H, and the one used for environmental dose monitoring of H*(10) is named GR-400H*.
[0045] S2: Firing polycrystalline
[0046] 2.1: Turn on the power of the commercial tubular sintering furnace, set the constant temperature of the control program to 950℃, and heat it up. At the same time, connect the tubular furnace and the nitrogen cylinder through a pressure reducing table with a flow meter. After the temperature is constant at 950℃, proceed to the next step;
[0047] 2.2: Take 20g of the powder prepared in S1 and put it in a 50ml platinum crucible, cover it tightly and place it on the crucible bracket, then move it into a constant temperature tube furnace and push it into the center of the tube furnace, connect the exhaust pipe cover at the inlet, unscrew the valve of the nitrogen cylinder in time, adjust the flow rate to 2L / min, and start timing when the temperature rises back to 950℃;
[0048] 2.3: When the timing reaches 30 minutes, turn on the power of the cooling fan, remove the exhaust pipe at the inlet of the tube furnace, pull the crucible bracket out to the furnace tube mouth, use a large long-handled tweezers or long flat-nosed pliers to move the bracket to the side of the fan, and then use crucible tongs to move the crucible under the fan to cool it quickly, and close the nitrogen bottle valve and the power button;
[0049] 2.4: After the crucible is cooled under the fan for 6-10 minutes, the multi-crystal blocks in the crucible will automatically separate from the crucible. Move the crucible away in time to allow the crystal blocks to directly receive the cold air from the fan, which can cool down faster. After it reaches room temperature, it can be crushed;
[0050] S3: Crushing polycrystalline
[0051] 3.1: Place the LiF:Mg, Cu, P, Ba polycrystalline block in a porcelain mortar, hit it into small pieces with appropriate force, further grind it into powder, and immediately use a 60-mesh standard sieve to sieve out the powder with less than 60 mesh for tableting;
[0052] S4: Pressing
[0053] 4.1: Use a single-punch tablet press for the pharmaceutical industry, usually equipped with a Φ4.5mm die, to punch out round tablets with a thickness of 0.8mm. Different specifications of dies can be selected as needed to press round tablets of different diameters and thicknesses;
[0054] Description: The powder can be pressed into large blocks by hot pressing technology, and then cut into detectors of different specifications such as square and strip shapes according to needs;
[0055] S5: High temperature sintering
[0056] 5.1: The purpose of high temperature sintering is to make the pressed tablets have sufficient mechanical strength in application. Take 15 pressed tablets and place them in a platinum box;
[0057] 5.2: According to the method in 2.1 of process S2, set the temperature control program of the tubular sintering furnace to 660℃, turn on the power to heat it up, replace the nitrogen cylinder with an oxygen cylinder, and after the furnace temperature stabilizes, put the platinum box containing 15 tablets, according to the operation procedure in 2.2 of S2, unscrew the valve of the oxygen cylinder, adjust the flow rate to 3-5 liters / minute, and start timing when the temperature rises back to 660℃;
[0058] 5.3: When the timing reaches 30 minutes, the subsequent procedure is the same as the method in 2.3 of S2. After the platinum box is cooled to room temperature, the detector is taken out;
[0059] S6: Performance Testing
[0060] 6.1: Low temperature annealing: Take a few newly prepared LiF:Mg, Cu, P, Ba detectors at random, place them in the annealing tray and put them in the center of the annealing furnace, close the furnace door, turn on the annealing furnace power switch, and strictly anneal according to the 240℃ / 10 minute annealing program;
[0061] 6.2: Irradiation: After annealing, the detector is irradiated with an experimental dose of americium (241Am) radiation source with an energy of about 50Kev;
[0062] 6.3: Reading: Obtain the luminescence curve and relative thermoluminescence sensitivity using a RGD-3 TL reader.
[0063] Experiment 1:
[0064] TL sensitivity of TL detectors prepared from different barium compounds + LiF:Mg, Cu, P raw materials
[0065] Using the same process as the previous experiment, different barium compounds BaCO3, BaS04, BaF2 (single crystal) and Ba3(PO4)2 were used in this experiment. The amount of these compounds contained the same barium content. Four TL detectors were prepared. Their relative thermoluminescence sensitivities obtained under the same annealing, irradiation and readout conditions as the LiF:Mg, Cu, P detectors are shown in Table 2:
[0066] Table 2: Relative thermoluminescence sensitivity of four LiFTL detectors
[0067] Sample No. 1 2 3 4 5 Ba compounds <![CDATA[;BaC03]]> <![CDATA[BaS04]]> <![CDATA[BaF2]]> <![CDATA[Ba3(P04)2]]> LiF:Mg,Cu,P Addition amount (Wt%) 50% 54.2% 47% 50.4% 0.0% TL Strength 21.012uGy 12.36uGy 22.608mGy 6.402mGy 4.5368mGy Relative TL strength 0.0046 0.0027 4.98 1.411 1.00
[0068] Note: The dosages of the four barium compounds contain equal amounts of the element barium.
[0069] The results shown in Table 2 indicate that BaF2 is the best dopant for the preparation of LiF:Mg,Cu,P,Ba.
[0070] Experiment 2:
[0071] Dependence of TL intensity of LiF:Mg, Cu, P, Ba detectors on the amount of barium (Ba) doping
[0072] The amount of barium doped will not only affect the TL sensitivity of the LiF:Mg, Cu, P, Ba detector, but also the effective atomic number Zff of the LiF:Mg, Cu, P, Ba detector, and may eventually cause the LiF:Mg, Cu, P, Ba detector to deviate from tissue equivalence, which mainly depends on the amount of barium doped. Therefore, a suitable amount of barium doping must be obtained from experiments. The less this amount contributes to the Zff of the LiF:Mg, Cu, P, Ba detector, the closer it is to the Zff of muscle tissue.
[0073] As shown in Table 3, the dependence of TL intensity of LiF:Mg, Cu, P, and Ba detectors on the amount of barium doping is listed.
[0074] Table 3: Dependence of TL intensity of LiF:Mg, Cu, P, Ba detectors on barium doping amount
[0075]
[0076] The results in Table 3 show that the TL intensity of LiF:Mg, Cu, P, Ba detectors for 241Am low-energy rays increases with the increase of BaF2 doping within a wide range. At the same time, the data in the TL / BaWt% row also show that the less the barium doping, the greater the contribution of the unit mass of barium to the low-energy thermoluminescence yield. This provides a prerequisite for using a smaller amount of barium doping to meet the new requirements of H(10) and H*(10) and make the Zff of LiF:Mg, Cu, P, Ba detectors closer to tissue equivalence. Photon energy dependence experiments were conducted on samples with two BaF2 doping levels, and the results are Figure 2 Shown in.
[0077] from Figure 2 The results show that, in the range of 80 KeV below the 60Co γ-ray energy, the TL intensity of LiF:Mg, Cu, P, and Ba detectors decreases with the decrease of the barium doping amount.
[0078] From the above experiments, it can be seen that the TL intensity of LiF:Mg, Cu, P, and Ba detectors can be freely adjusted with the amount of barium doped. From this result, it can be known that by adjusting the amount of barium doped, the barium doping amount that meets the new requirements of personal dose equivalent Hp(10) and ambient dose equivalent H*(10) proposed in ICRU Reports 39 and 43 can be obtained. Through multiple experiments, better results were obtained than those doped with lead, as shown in Table 4:
[0079] Table 4: New requirements for barium doping levels corresponding to lead for the two practical quantities H(10) and H*(10) proposed in ICRU Reports 39 and 43
[0080]
[0081]
[0082] Notes on Table 4: The data provided in the table only indicate that the barium reagent used in the experiment is of "chemically pure" grade. Please note that the purity may vary from place to place.
[0083] The samples of LiF:Mg, Cu, P, Ba detectors with two barium doping amounts in Table 4 were subjected to photon energy dependence experiments, and the results are shown in Table 5.
[0084] Table 5: Photon energy dependence of barium incorporation to meet Hp(10) and H*(10) requirements
[0085]
[0086] From the data in Table 4 and Table 5, it can be seen that the mass of the newly added barium element in satisfying the two physical quantities Hp(10) and H*(10) is less than that of the lead element, and the atomic number Z of the barium element is much smaller than that of the lead element. Therefore, the LiF:Mg,Cu,P,Ba detector has better tissue equivalence than the LiF:Mg,Cu,P,Pb detector. Therefore, the LiF:Mg,Cu,P,Ba detector is the latest LiF thermoluminescent material detector that is close to tissue equivalence. According to the data in Table 5, a graph can be drawn showing Figure 3 Photon energy dependence curves of the two barium incorporation levels.
[0087] Depend on Figure 3 It can be seen that the energy dependence curve of Hp(10) is slightly convex, because when the detector is placed in a dose box of organic material in personal dose monitoring, the detector is inadvertently shielded slightly, and the energy dependence curve is completely flat. When monitoring deep doses in the body, the barium doping amount required for energy dependence can be adjusted to any required level according to actual needs, and the curve can also become completely flat or convex; while the energy dependence curve of H*(10) is completely convex in the low energy range.
[0088] The ultimate goal of the development of radiation protection dosimetry is to quantitatively determine the degree of damage caused by radioactive radiation of different energies in the human body, so as to take effective measures to prevent the occurrence of injury accidents. The key point of this invention is that the thermoluminescent detector with LiF:Mg, Cu as the matrix material, such as: LiF:Mg, Cu; LiF:Mg, Cu, Si; LiF:Mg, Cu, P, etc., after quantitatively adding an impurity element Ba, these new detectors LiF:Mg,Cu,Ba; LiF:Mg,Cu,Si,Ba; LiF:Mg,Cu,P,Ba, etc. are used to measure personal dose monitoring and diagnostic doses in radiomedicine and control of therapeutic doses, which can ensure that the health of people exposed to radioactive radiation will not be damaged, and the technical indicators of the dosimetric performance of the LiF detector with Ba added elements will meet the two new requirements of practical quantities proposed in ICRU Reports 39 and 43, which are not available in all previous thermoluminescent detectors.
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the present invention.
Claims
1. A production process of a LiF thermoluminescent material detector, characterized in that: The steps include: S1: Ingredients 1.1: The raw material component ratio of the experimental sample is: 20 grams of prepared LiF:Mg, Cu, P, Ba powder to be pressed into tablets, the amount of raw material components of LiF:Mg, Cu, P, Ba powder to be pressed into tablets per 1g of lithium fluoride is: phosphoric acid is 0.031190496ml, magnesium oxide is 0.0031087g, copper fluoride is 0.000607g, barium fluoride for personal dose detector is 0.00805g, barium fluoride for environmental dose monitoring detector is 0.01345g, lithium fluoride is 1g; S2: Firing polycrystalline 2.1: Turn on the power of the commercial tubular sintering furnace, set the constant temperature of the control program to 950℃, and heat it up. At the same time, connect the tubular furnace and the nitrogen cylinder through a pressure reducing table with a flow meter. After the temperature is constant at 950℃, proceed to the next step; 2.2: Take 20g of the powder prepared in S1 and put it in a 50ml platinum crucible, cover it tightly and place it on the crucible bracket, then move it into a constant temperature tube furnace and push it into the center of the tube furnace, connect the exhaust pipe cover at the inlet, unscrew the valve of the nitrogen cylinder in time, adjust the flow rate to 2L / min, and start timing when the temperature rises back to 950℃; 2.3: When the timing reaches 30 minutes, turn on the power of the cooling fan, remove the exhaust pipe at the inlet of the tube furnace, pull the crucible bracket out to the furnace tube mouth, use a large long-handled tweezers or long flat-nosed pliers to move the bracket to the side of the fan, and then use crucible tongs to move the crucible under the fan to cool it quickly, and close the nitrogen bottle valve and the power button; 2.4: After the crucible is cooled under the fan for 6-10 minutes, the multi-crystal blocks in the crucible will automatically separate from the crucible. The crucible should be removed in time to allow the crystal blocks to directly receive the cold air from the fan, which will cool them down faster. After they reach room temperature, they can be crushed. S3: Crushing polycrystalline 3.1: Place the LiF:Mg, Cu, P, Ba polycrystalline block in a porcelain mortar, hit it into small pieces with appropriate force, further grind it into powder, and immediately use a 60-mesh standard sieve to sieve out the powder with less than 60 mesh for tableting; S4: Pressing 4.1: Use a single-punch tablet press for the pharmaceutical industry, equipped with a Φ4.5mm die, to punch out round tablets with a thickness of 0.8mm. Different specifications of dies can be selected as needed to press round tablets of different diameters and thicknesses; S5: High temperature sintering 5.1: The purpose of high temperature sintering is to make the pressed tablets have sufficient mechanical strength in application. Take 15 pressed tablets and place them in a platinum box; 5.2: According to the method in 2.1 of process S2, set the temperature control program of the tubular sintering furnace to 660℃, turn on the power to heat it up, replace the nitrogen cylinder with an oxygen cylinder, and after the furnace temperature stabilizes, put the platinum box containing 15 tablets, according to the operation procedure in 2.2 of S2, unscrew the valve of the oxygen cylinder, adjust the flow rate to 3-5 liters / minute, and start timing when the temperature rises back to 660℃; 5.3: When the timing reaches 30 minutes, the subsequent procedure is the same as the method in 2.3 of S2. After the platinum box is cooled to room temperature, the detector is taken out; S6: Performance Testing 6.1: Low temperature annealing: Take a few newly prepared LiF:Mg, Cu, P, Ba detectors at random, place them in the annealing tray and put them in the center of the annealing furnace, close the furnace door, turn on the annealing furnace power switch, and strictly anneal according to the 240℃ / 10 minute annealing program; 6.2: Irradiation: After annealing, the detector is irradiated with an experimental dose of an americium radiation source with an energy of about 50 KeV; 6.3: Reading: Obtain the luminescence curve and relative thermoluminescence sensitivity using a RGD-3 TL reader.
2. The production process of a LiF thermoluminescent material detector according to claim 1, characterized in that: In S4, the powder is pressed into large blocks through hot pressing technology, and then cut into square and strip-shaped detectors of different specifications as needed.