A glue-free optical patterning method for colloidal nanocrystals in green solvents
By introducing bifunctional photosensitive ligands on the surface of nanocrystals, direct photolithography in green solvents is achieved, which solves the problem of commercial photoresist residue and the inability of nanocrystals to be patterned in green solvents, and improves the charge transport of nanocrystals. efficiency and fluorescence properties, suitable for industrial production.
Patent Information
- Application Number
- CN202211052499.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-08-31
AI Technical Summary
In existing nanocrystal optical patterning methods, the residue of commercial photoresist affects the charge transport and optical properties of nanocrystals, and they cannot be patterned directly in green solvents, which limits industrial production applications.
Bifunctional photosensitive ligands are used to dissolve the similar structures on the surface of nanocrystals and perform coupling polymerization under specific wavelength light to achieve direct photolithography patterning of nanocrystals in green solvents, avoiding the residue of photoresist. The fluorescent properties of the nanocrystals are retained and the distance between the nanocrystals is shortened.
The nanocrystals were successfully dispersed in a green solvent and achieved direct photolithography, retaining approximately 90% of the fluorescence quantum yield, simplifying the process, reducing costs, and improving the charge transfer efficiency of the nanocrystals.
Smart Images

Figure CN115308997B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials and optical etching, and particularly relates to a non-glue optical patterning method of colloidal nanocrystals in a green solvent. Background Art
[0002] At present, the optical patterning methods for nanocrystals (NCs) are mainly based on two methods: (1) photoresist-based lithography. This method mainly uses relatively mature commercial photoresists, which can be divided into two different methods: (i) first directly lithography the commercial photoresist and use the developer to peel off part of the photoresist, then fill the nanocrystals into the photoresist template, and finally peel off the photoresist to obtain patterned nanocrystals ( Figure 1 a). (ii) directly mixing the nanocrystals with commercial photoresist, then directly photolithography the mixture, embedding the nanocrystals into the photoresist and partially stripping off the photoresist and nanocrystals in a developer ( Figure 1 b). (2) Glue-free direct photolithography. Introducing photoacid generators (PAGs) or bifunctional surface ligands (such as Figure 2 ). Under a specific wavelength, the introduced photosensitive substance decomposes, causing changes in the surface environment of the nanocrystal, thereby affecting its stability in some solvents and selecting the corresponding solvent to elute the nanocrystal to remove the unexposed part ( Figure 1 c). This type of ligand has a wide range of photosensitivity, from deep ultraviolet (DUV, 254nm) to visible light (450nm), and can be used to photolithography nanocrystals containing specific photosensitive groups.
[0003] The nanocrystal patterning method using photoresist will inevitably introduce photoresist, but commercial photoresist cannot effectively remove the photoresist completely during the development process. The remaining residual photoresist will have a great impact on the charge transfer, heat transfer and other properties of the nanocrystals. At the same time, the cost of the photoresist itself is relatively high, which will increase the cost of the nanocrystal patterning process.
[0004] In the non-resist lithography technology, although the problems caused by the introduction of commercial photoresists are avoided, nanocrystals cannot be directly dispersed in green solvents such as propylene glycol methyl ether acetate (PGMEA), diethylene glycol ethyl ether acetate (DGMEA), octane, etc. The patterning process can only be carried out in industrially unacceptable solvents such as toluene and N, N-dimethylformamide (DMF), which greatly limits the current application of nanocrystal patterning technology in actual industrial production. In addition, the introduced functional ligands will change the composition of the nanocrystal surface and damage the nanocrystal surface, further affecting the optical properties of the nanocrystal. Therefore, after the patterning is completed, the nanocrystal needs to be post-processed to repair the surface of the nanocrystal to restore some of the performance. Summary of the invention
[0005] The present invention solves the above-mentioned technical problems existing in the prior art, proposes a photoinduced crosslink lithography (PICL) technology, and designs a class of bifunctional ligands. On the one hand, these ligands are partially similar in structure to green solvents. After being connected to the surface of nanocrystals with carboxylate, amino or thiol groups, they assist the nanocrystals to be dispersed in green solvents such as PGMEA, DGMEA, octane, etc. according to the principle of "like dissolves like"; on the other hand, these ligands have photosensitive methacryloyl groups or benzophenone groups. Due to the photosensitive nature of the groups, they can be coupled and polymerized under light of a specific wavelength, thereby realizing direct photolithographic patterning of nanocrystals. This method retains the advantages of easy operation of non-glue photolithography technology, and will not damage the surface of nanocrystals. While completing patterning, it can also retain the fluorescence properties of nanocrystals and shorten the distance between nanocrystals, effectively improving the efficiency of charge transfer between nanocrystals.
[0006] The technical solution of the present invention is as follows:
[0007] A green photosensitive nanocrystal coating comprises nanocrystals and photosensitive ligands; the selected photosensitive ligands all contain groups coordinated with the nanocrystals, such as carboxylate, amino or mercapto, and methacryloyl or benzophenone photosensitive groups.
[0008] Preferably, the photosensitive ligand is 2-(3-mercaptopropionyloxy)ethyl methacrylate, 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid, (2E)-3-(3-methoxy-4-{2-[(2-methylprop-2-enoyl)oxy]ethoxy}phenyl)prop-2-enoic acid, 4-(4-(methacryloyloxy)phenoxy)-4-oxobutyric acid, mono-2-(methacryloyloxy)ethyl succinate, (E)-6-(4-(methacryloyloxy)phenyl)-4-oxohex-5-enoic acid, ( Any one of (E)-6-(4-(methacryloyloxy)-3-methoxyphenyl)-4-oxohex-5-enoic acid, (E)-6-(4-(methacryloyloxy)-3,5-dimethoxyphenyl)-4-oxohex-5-enoic acid, 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid, phenyl-[4-(10-mercaptodecyloxy)phenyl]methanone, phenyl-[4-(10-mercaptodecylthio)phenyl]methanone, and 4-pyrrolidinyl-phenyl-[4-(10-mercaptodecylthio)phenyl]methanone.
[0009] Preferably, the nanocrystal contains an original organic ligand, and the original organic ligand is any one or a combination of carboxylic acid, phosphonic acid, and amine with a fatty chain greater than 8 carbons. More preferably, the original organic ligand is any one or a combination of oleic acid, stearic acid, palmitic acid, oleylamine, octadecylamine, and octadecylphosphonic acid.
[0010] Preferably, the nanocrystals include CdS, CdSe, CdSe / ZnS, CdSeS / ZnS, CdSe / CdZnSeS / ZnS, CdZnS / ZnS, CdZnSe / ZnS, ZnSe / ZnS, CdSe / CdS, CdSeS / CdS, InP, InP / ZnS, InP / ZnSe / ZnS, InGaP / ZnSe / ZnS, CdTe, PbS, PbSe, PbS / CdS, Fe2O3, Fe3O4, TiO2, ITO, In2O3, CsPbBr3, MAPbBr3 and the like, but are not limited to inorganic nanocrystals.
[0011] The green photosensitive nanocrystal coating is prepared by the following method: ligand exchange between nanocrystals with organic ligands on the surface and photosensitive ligands. Specifically, photosensitive ligands are added to a nanocrystal solution with organic ligands on the surface, and the resulting mixture is vigorously stirred or shaken to obtain a precipitate, which is the product.
[0012] Preferably, the nanocrystal solution with organic ligands on the surface is mixed with the photosensitive ligand in a mass ratio of 10:1, and the resulting mixture is vigorously stirred or shaken until a precipitate is formed as the product. Preferably, the concentration of the photosensitive ligand is greater than or equal to 50 mg / mL.
[0013] Preferably, the ligand exchange is performed under an inert atmosphere.
[0014] The preparation method of green photosensitive nanocrystal ink is: dispersing the green photosensitive nanocrystal coating in a green solvent, wherein the green solvent is propylene glycol methyl ether acetate (PGMEA), ethylene glycol methyl ether acetate (EGMEA), diethylene glycol ethyl ether acetate (DGMEA) or propylene glycol methyl ether (PGME), octane.
[0015] Preferably, the green photosensitive nanocrystalline coating is dispersed in a green solvent to form a stable colloidal solution, and the concentration of the green photosensitive nanocrystalline coating is 10 to 25 mg / mL.
[0016] A method for non-glue optical patterning of colloidal nanocrystals in a green solvent comprises the following steps: using the green photosensitive nanocrystal ink to prepare a continuous, dense and thickness-controllable nanocrystal film on a substrate; pressing a mask plate engraved with a specific pattern on the film, exposing it to an ultraviolet light source, and developing it in a developer.
[0017] Preferably, the substrate is a silicon wafer, a quartz wafer or a glass wafer.
[0018] Preferably, the developer is propylene glycol methyl ether acetate (PGMEA), ethylene glycol methyl ether acetate (EGMEA), diethylene glycol ethyl ether acetate (DGMEA) or propylene glycol methyl ether (PGME), octane.
[0019] Compared with the prior art, the advantages of the present invention are as follows:
[0020] The present invention successfully disperses the nanocrystals in the green solvent by introducing a photosensitive ligand having a structure similar to that of the green solvent, and can perform direct photolithography on the nanocrystals.
[0021] The photosensitive nanocrystals obtained by ligand exchange in the present invention can be effectively dispersed in green solvents and their absorption and emission spectra, morphology and size remain unchanged, while the fluorescence quantum yield (PLQY) can be retained at about 90%. Through the exploration of the mechanism, it is clear that the process is due to the free radical polymerization of acryloyl in the photosensitive ligand structure under ultraviolet light, thereby shortening the distance between nanocrystals, thereby greatly reducing their solubility in solvents such as toluene and propylene glycol methyl ether acetate.
[0022] The invention solves the problem that nanocrystals cannot be directly photolithographically processed in green solvents. The process is expected to be applied in the commercialization of nanocrystals in the field of electroluminescent and photoluminescent quantum dot displays. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 a is a photoresist-based optical etching technology 1; Figure 1 b is a photoresist-based optical etching technology 2; Figure 1 c is photoresist-free lithography technology; Figure 1 d is the optical patterning method of the present invention, which has no damage to the fluorescence performance;
[0024] Figure 2 It is a photoacid generator (PAG) or bifunctional surface ligand introduced into the colloidal nanocrystal system to achieve photoresist-free lithography.
[0025] Figure 3 It is a schematic diagram of the method for surface treatment of nanocrystals in the present invention.
[0026] Figure 4 It is a schematic diagram of the photolithography process of the present invention.
[0027] Figure 5 This is a comparison of the transmission electron micrographs of the nanocrystals before (left) and after (right) ligand exchange.
[0028] Figure 6Comparison of the luminescence properties of nanocrystals before (black line) and after (gray line) treatment with photosensitizing ligands.
[0029] Figure 7 It is a photolithographic pattern with 2-(3-mercaptopropionyloxy)ethyl methacrylate as a ligand.
[0030] Figure 8 It is a photolithographic pattern with 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid as a ligand.
[0031] Fig. 9 It is a photolithographic pattern with 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid as a ligand. DETAILED DESCRIPTION
[0032] Embodiment 1:
[0033] Direct photolithography of nanocrystals (quantum dots) in green solvents using deep ultraviolet light as the light source and 2-(3-mercaptopropionyloxy)ethyl methacrylate as the ligand
[0034] All ligand exchanges were performed in a nitrogen-filled glove box (O2 and H2O less than 0.01 ppm) using anhydrous solvents. The photosensitive ligand used was 2-(3-mercaptopropionyloxy)ethyl methacrylate.
[0035] Red fluorescent nanocrystalline CdSe / ZnS quantum dots with oleic acid on the surface are dispersed in n-hexane, and 2-(3-mercaptopropionyloxy)ethyl methacrylate is a pure substance. First, a ligand exchange treatment is performed. 200μL NCs solution (25mg / mL) is added with 20μL 2-(3-mercaptopropionyloxy)ethyl methacrylate. The resulting mixture is vigorously stirred or shaken until NCs precipitation is observed. After centrifugation, the precipitate is redispersed in 200μL PGMEA and precipitated with 1mL n-hexane to remove excess 2-(3-mercaptopropionyloxy)ethyl methacrylate ligands. After centrifugation, the precipitate is dispersed in PGMEA to form a stable colloidal solution (10-25mg / mL). The transmission electron microscope (TEM) photo of the material is shown in FIG. Figure 5 As shown. 10μL NCs PGMEA solution was dropped on the surface of the silicon wafer and spun on a coating machine to form a uniform film. A mask with a specific pattern was pressed on the film, exposed to a 254nm ultraviolet light source, and developed in PGMEA developer. The resulting pattern is shown in Figure 7 shown.
[0036] Embodiment 2:
[0037] Direct photolithography of nanocrystals (quantum dots) in green solvents using 365 nm as light source and 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid as ligand
[0038] All ligand exchanges were performed in a nitrogen-filled glove box (O2 and H2O less than 0.01 ppm) using anhydrous solvents. The photosensitive ligand used was 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid.
[0039] Green fluorescent nanocrystalline CdSe / CdZnSeS quantum dots with oleic acid as surface ligand are dispersed in n-hexane, and 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid is prepared into a solution in n-hexane. First, a ligand exchange treatment was performed. 200 μL of NCs solution (25 mg / mL) was added with 20 μL of 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid n-hexane solution (50 mg / mL). The resulting mixture was vigorously stirred or shaken until NCs precipitation was observed. After centrifugation, the precipitate was redispersed in 200 μL PGMEA and precipitated with 1 mL of n-hexane to remove excess 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid ligand. After centrifugation, the precipitate was dispersed in PGMEA to form a stable colloidal solution (10-25 mg / mL). The absorption and fluorescence spectra before and after treatment are compared. Figure 6 10 μL NCs PGMEA solution was dropped on the surface of the silicon wafer and spin-coated into a uniform film on a coating machine. A mask with a specific pattern was pressed on the film, exposed to a 365 nm ultraviolet light source, and developed in PGMEA developer. The resulting pattern is as follows Figure 8 To fully demonstrate the universality of this method, we photolithography CdSeS / ZnS quantum dots that emit red fluorescence and CdZnS / ZnS quantum dots that emit blue fluorescence, and both obtained nanocrystal patterns that retain fluorescence.
[0040] Embodiment 3:
[0041] Direct photolithography of nanocrystals (quantum dots) in green solvents using 405 nm as light source and 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid as ligand
[0042] All ligand exchanges were performed in a nitrogen-filled glove box (O2 and H2O less than 0.01 ppm) using anhydrous solvents. The photosensitive ligand used was 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid.
[0043] Green fluorescent nanocrystalline CdSe / CdZnSeS quantum dots with oleic acid on the surface are dispersed in n-hexane, and 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid is prepared as a solution in n-hexane. First, ligand exchange treatment was performed. 200 μL of NCs solution (25 mg / mL) was added with 20 μL of 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid in n-hexane (50 mg / mL). The resulting mixture was vigorously stirred or shaken until NCs precipitation was observed. After centrifugation, the precipitate was redispersed in 200 μL of PGMEA and precipitated with 1 mL of n-hexane to remove excess 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid ligand. After centrifugation, the precipitate was dispersed in PGMEA to form a stable colloidal solution (10-25 mg / mL). 10 μL of NCs in PGMEA solution was dropped on the surface of the silicon wafer and spin-coated into a uniform film on a spin coater. The mask with a specific pattern is pressed on the film, exposed to a 365nm ultraviolet light source, and developed in PGMEA developer. The resulting pattern is as follows Fig. 9 shown.
[0044] Embodiment 4:
[0045] The same experimental method as in Example 3 can achieve the same technical effect by using the following photosensitizing ligand instead of 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid.
[0046] (2E)-3-(3-Methoxy-4-{2-[(2-methylprop-2-enoyl)oxy]ethoxy}phenyl)prop-2-enoic acid
[0047] 4-(4-(Methacryloyloxy)phenoxy)-4-oxobutanoic acid
[0048] Mono-2-(methacryloyloxy)ethyl succinate
[0049] (E)-6-(4-(Methacryloyloxy)phenyl)-4-oxohex-5-enoic acid
[0050] (E)-6-(4-(Methacryloyloxy)-3-methoxyphenyl)-4-oxohex-5-enoic acid
[0051] (E)-6-(4-(Methacryloyloxy)-3,5-dimethoxyphenyl)-4-oxohex-5-enoic acid
[0052] Phenyl-[4-(10-mercaptodecyloxy)phenyl]methanone, Phenyl-[4-(10-mercaptodecylthio)phenyl]methanone
[0053] 4-Pyrrolidinyl-phenyl-[4-(10-mercaptodecylthio)phenyl]methanone
[0054] Embodiment 5:
[0055] The same experimental method as in Example 3 is used, but CdS, CdSe, CdSe / ZnS, CdSeS / ZnS, CdSe / CdZnSeS / ZnS, CdZnS / ZnS, CdZnSe / ZnS, ZnSe / ZnS, CdSe / CdS, CdSeS / CdS, InP, InP / ZnS, InP / Zn Se / ZnS, InGaP / ZnSe / ZnS, CdTe, PbS, PbSe, PbS / CdS, Fe2O3, Fe3O4, TiO2, ITO, In2O3, CsPbBr3, and MAPbBr3 nanocrystals are used instead of CdSe / CdZnSeS quantum dots, and the same technical effects can be achieved.
[0056] Embodiment 6:
[0057] The same experimental method as in Example 3 can achieve the same technical effect by using octane, ethylene glycol methyl ether acetate (EGMEA), diethylene glycol ethyl ether acetate (DGMEA) or propylene glycol methyl ether (PGME) instead of propylene glycol methyl ether acetate (PGMEA).
[0058] It should be noted that the above embodiments are merely preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Equivalent replacements or substitutions made on the basis of the above embodiments all fall within the protection scope of the present invention.
Claims
1. A green photosensitive nanocrystal coating, characterized in that: The invention comprises a nanocrystal and a photosensitive ligand; the photosensitive ligand comprises a group coordinated with the nanocrystal and a methacryloyl or benzophenone photosensitive group; The photosensitive ligand is 2-(3-mercaptopropionyloxy)ethyl methacrylate, 5-[3-methoxy-4-(2-methylprop-2-enoyloxy)phenyl]pent-4-enoic acid, (2E)-3-(3-methoxy-4-{2-[(2-methylprop-2-enoyl)oxy]ethoxy}phenyl)prop-2-enoic acid, 4-(4-(methacryloyloxy)phenoxy)-4-oxobutyric acid, mono-2-(methacryloyloxy)ethyl succinate, (E)-6-(4-(methacryloyloxy)phenyl)-4-oxohex-5-enoic acid, (E)-6-(4-(methacryloyloxy)-3-methoxyphenyl)-4-oxohex-5-enoic acid, (E)-6-(4-(methacryloyloxy)-3,5-dimethoxyphenyl)-4-oxohex-5-enoic acid, Any one of 2-(6-(2-(methacryloyloxy)ethoxy)-2-oxo-2H-chromen-3-yl)acetic acid, phenyl-[4-(10-mercaptodecyloxy)phenyl]methanone, phenyl-[4-(10-mercaptodecylthio)phenyl]methanone and 4-pyrrolidinyl-phenyl-[4-(10-mercaptodecylthio)phenyl]methanone.
2. The green photosensitive nanocrystal coating according to claim 1, characterized in that: The group coordinated with the nanocrystal is any one or more of carboxylate, amino and thiol.
3. The green photosensitive nanocrystal coating according to claim 1, characterized in that: The nanocrystals are any one of CdS, CdSe, CdSe / ZnS, CdSeS / ZnS, CdSe / CdZnSeS, CdSe / CdZnSeS / ZnS, CdZnS / ZnS, CdZnSe / ZnS, ZnSe / ZnS, CdSe / CdS, CdSeS / CdS, InP, InP / ZnS, InP / ZnSe / ZnS, InGaP / ZnSe / ZnS, CdTe, PbS, PbSe, PbS / CdS, Fe2O3, Fe3O4, TiO2, ITO, In2O3, CsPbBr3, and MAPbBr3, and the nanocrystals contain original organic ligands, and the original organic ligands are any one of or a combination of carboxylic acids, phosphonic acids, and amines having a fatty chain greater than 8 carbon atoms.
4. The method for preparing the green photosensitive nanocrystalline coating according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: adding a photosensitive ligand into a nanocrystal solution with an organic ligand on the surface, and vigorously stirring or shaking the obtained mixture to obtain a precipitate, which is the product.
5. The preparation method according to claim 4, characterized in that: Under an inert atmosphere, a 25 mg / mL solution of nanocrystals with organic ligands on the surface is mixed with a photosensitive ligand at a volume ratio of 10:1, and the resulting mixture is vigorously stirred or shaken until a precipitate is generated, which is the product.
6. A method for preparing green photosensitive nanocrystal ink, characterized in that: The green photosensitive nano-crystal coating according to any one of claims 1 to 4 is dispersed in a green solvent, wherein the green solvent is propylene glycol methyl ether acetate, ethylene glycol methyl ether acetate, octane, diethylene glycol ethyl ether acetate or propylene glycol methyl ether.
7. The preparation method according to claim 6, characterized in that: The green photosensitive nano-crystal coating is dispersed in a green solvent to form a stable colloidal solution, and the concentration of the green photosensitive nano-crystal coating is 10-25 mg / mL.
8. A method for non-adhesive optical patterning of colloidal nanocrystals in a green solvent, characterized in that: The method comprises the following steps: using the green photosensitive nanocrystal ink as described in claim 6 to prepare a continuous, dense and thickness-controllable nanocrystal film on a substrate; pressing a mask plate engraved with a specific pattern on the film, exposing it to an ultraviolet light source, and developing it in a developer.
9. The method according to claim 8, characterized in that The substrate is a silicon wafer, a quartz wafer or a glass wafer; the developer is propylene glycol methyl ether acetate, ethylene glycol methyl ether acetate, octane, diethylene glycol ethyl ether acetate or propylene glycol methyl ether.