A method for improving polymer melt strength and toughness

By mixing reactive polymer B and polymer A and combining with functional additives, the problem of insufficient polymer melt strength and toughness is solved, and high melt strength and toughness are improved while maintaining the material's durability. Degradability and processing properties.

CN115322546BActive Publication Date: 2024-10-01JIANGNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211128937.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-10-01
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

It is difficult to effectively improve the melt strength and toughness of polyglycolic acid, glycolic acid-based copolymers, polylactic acid, lactic acid-based copolymers, and polyethylene terephthalate with the existing technology, and the improvement methods often damage their degradability or Liquidity.

Method used

Mix reactive polymer B and polymer A through melt blending or extrusion. Reactive polymer B contains flexible polyester backbone and reactive groups. The ratio is polymer A: reactive polymer B = 90 -99: 1-30, add functional additives to form a composition with high melt strength and toughness.

Benefits of technology

Significantly improves the melt strength and toughness of the polymer, forms a long-chain branched structure, enhances molecular chain entanglement, maintains complete degradability and good processing performance of the system, and is suitable for compression molding, foaming, blow molding and other processes .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115322546B_ABST
    Figure CN115322546B_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the melt strength and toughness of a polymer, and belongs to the technical field of polymer processing and modification. The invention is to melt and blend 90 to 99 parts by weight of polymer A, 1 to 30 parts by weight of reactive polymer B and 0.1 to 3 parts by weight of functional additives as main raw materials at a certain temperature to obtain a high melt strength and high toughness composition. The composition provided by the invention not only has high melt strength but also has excellent toughness, and can be directly used for compression molding, foaming, blow molding, and secondary molding to prepare thermoplastic plastic products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for improving polymer melt strength and toughness, belonging to the technical field of polymer processing and modification. Background Art

[0002] With the rapid development of polymer materials industry, the application of polymer materials has penetrated into various fields of industry, agriculture and people's daily life. However, most polymer materials are currently derived from petroleum-based materials, which are not easy to achieve natural degradation and difficult to recycle. Polyglycolic acid, glycolic acid-based copolymers, polylactic acid, lactic acid-based copolymers, and polyethylene terephthalate are all biodegradable polymer materials with excellent degradation performance, non-toxicity and good biocompatibility, but they have the disadvantage of low melt strength in processing, so they need to be modified.

[0003] Existing methods for improving melt strength, such as CN103626982A, provide a method for improving the melt strength of polyester resins. Although the intermediates with active functional groups prepared by the method get rid of the limitations of small molecules, they destroy the degradability of the polyester system. In addition, during the melt processing of ester polymers, the coupling copolymer intermediates change the polymer molecular chain structure and thus improve the melt strength. This method easily produces a cross-linked structure, which deteriorates the fluidity of the system and even loses its melt processability.

[0004] In addition, the current methods for improving the melt strength of polyglycolic acid, glycolic acid-based copolymers, polylactic acid, lactic acid-based copolymers, and polyethylene terephthalate have failed to effectively improve the defect of polyester brittleness. Therefore, it is extremely necessary to invent a new method for preparing a polymer composition with high melt strength and excellent toughness. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides a method for simultaneously improving the strength and toughness of a polymer melt.

[0006] The object of the present invention is to provide a method for improving the melt strength and toughness of a polymer, wherein the method comprises mixing a reactive polymer B with a polymer A, melt blending or melt extruding;

[0007] The reactive polymer B comprises a flexible polyester main chain and a side chain having an active group; the active group comprises at least one of anhydride, epoxy group and isocyanate;

[0008] The polymer A is at least one of polyglycolic acid, glycolic acid-based copolymers, polylactic acid, lactic acid-based copolymers, and polyethylene terephthalate.

[0009] In one embodiment of the present invention, the weight ratio is 85-99 parts of polymer A and 1-30 parts of reactive polymer B. More preferably, the weight ratio is 90-99 parts of polymer A and 10-30 parts of reactive polymer B.

[0010] In one embodiment of the present invention, the mass ratio of polymer A to reactive polymer B is (90-99):(1-30). It may be preferably (90-99):(3-30); or preferably (90-99):(5-30); or preferably (90-99):(10-30); or preferably (90-99):(20-30); or preferably (95-99):(10-30).

[0011] In one embodiment of the present invention, the method further comprises adding 0.1 to 3 parts by weight of a functional aid.

[0012] In one embodiment of the present invention, the method is to prepare a high melt strength and high toughness composition using 90 to 99 parts by weight of polymer A, 1 to 15 parts by weight of reactive polymer B and 0.1 to 3 parts by weight of functional additives as main raw materials.

[0013] In one embodiment of the present invention, the functional additive includes at least one of an antistatic agent, an antioxidant, an antioxidant, an anti-hydrolysis agent and a filler.

[0014] In one embodiment of the present invention, the flexible polyester main chain of the reactive polymer B is polymerized from at least one monomer selected from the group consisting of caprolactone, lactide, glycolide, adipic acid, terephthalic acid, succinic acid and butanediol.

[0015] In one embodiment of the present invention, the mass fraction of active groups in the reactive polymer B is 0.1 to 30%, preferably 5 to 25%, and more preferably 15 to 25%.

[0016] In one embodiment of the present invention, the reactive polymer B is prepared by melt grafting a flexible polyester with a monomer C under the action of a free radical initiator; the monomer C contains both a -C=C- double bond and an active group.

[0017] In one embodiment of the present invention, monomer C can be specifically selected from at least one of glycidyl methacrylate, glycidyl acrylate, methyl methacrylate, styrene, styrene-based monomers, maleic anhydride, epoxidized unsaturated vegetable oils and fats, epoxidized cardanol, epoxidized eugenol, and isocyanates containing unsaturated double bonds.

[0018] In one embodiment of the present invention, the mass ratio of the flexible polyester to the monomer C is 50:(1-50); preferably 50:(5-50); further preferably 50:(15-30).

[0019] In one embodiment of the present invention, the free radical initiator is at least one of dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, di(tert-butylperoxy)butane, tert-butyl peroxide, tert-butyl peroxypivalate, tert-butyl peracetate, methyl ethyl ketone peroxide, tert-butyl perbenzoate and diisopropyl peroxydicarbonate.

[0020] In one embodiment of the present invention, the functional additive is specifically selected from: Irganox 1330, polycarbodiimide, JL-5P, JL-WT, antioxidant 4010, and antioxidant RD.

[0021] In one embodiment of the present invention, the melting temperature is 110-180°C; for example, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc.

[0022] The present invention also provides a composition with high melt strength and toughness, which comprises, by weight: 90 to 99 parts of polymer A, 1 to 15 parts of reactive polymer B, and 0.1 to 3 parts of functional additives; wherein the reactive polymer B comprises a flexible polyester main chain and a side chain having an active group; the active group comprises at least one of anhydride, epoxy group, and isocyanate;

[0023] The polymer A is at least one of polyglycolic acid, glycolic acid-based copolymers, polylactic acid, lactic acid-based copolymers, and polyethylene terephthalate.

[0024] In one embodiment of the present invention, the preparation method of the above composition specifically comprises:

[0025] Method 1: Premix polymer A, reactive polymer B and functional additives at room temperature according to weight ratio, add them into internal mixer for melt blending, and obtain a high melt strength and high toughness composition;

[0026] Or method 2, polymer A, reactive polymer B and functional additives are premixed uniformly at room temperature according to weight ratio, added into the conveying section of a twin-screw extruder, and subjected to continuous melt extrusion to obtain a high melt strength and high toughness composition.

[0027] In one embodiment of the present invention, in method 1, the melt blending time is 1 to 15 minutes.

[0028] In one embodiment of the present invention, in method 1, the temperature of melt blending is 1-50°C above the melting point of polymer A; the rotor speed is 30-200 rpm. The blending temperature can be appropriately adjusted according to the melting temperature of polymer A, and the speed can be adjusted according to the melt viscosity of the composition. The temperature of melt blending can be specifically selected from 5°C, 10°C, 20°C, 30°C, 40°C, and 50°C above the melting point.

[0029] In one embodiment of the present invention, in method 2, the temperature of the screw extrusion is 1-50°C above the melting point of polymer A, and the screw speed is 50-300 rpm. The screw extrusion temperature can be appropriately adjusted according to the melting temperature of polymer A, and the screw speed can be adjusted according to the melt viscosity of the composition. The extrusion temperature can be specifically selected from 5°C, 10°C, 20°C, 30°C, 40°C, and 50°C above the melting point.

[0030] The present invention also provides the use of the high melt strength and high toughness composition for compression molding, foaming, blow molding, and secondary molding to prepare thermoplastic plastic products.

[0031] The beneficial effects of the present invention are:

[0032] (1) The method of improving the melt strength and toughness of a polymer of the present invention comprises melt blending 90 to 99 parts by weight of a polymer A, 1 to 10 parts by weight of a reactive polymer B and 0.1 to 3 parts by weight of a functional additive as main raw materials at a certain temperature to obtain a high melt strength and high toughness composition.

[0033] (2) In the present invention, the reactive polymer B reacts with the polymer A in situ during melt processing to form a long-chain branched structure, which significantly enhances the entanglement between the molecular chains, thereby improving the melt strength of the polymer; at the same time, the main chain of the reactive polymer B is selected as a degradable flexible polyester, which, on the one hand, makes the system completely degradable, and on the other hand, the flexible polyester and polymer A are combined through chemical bonds to greatly improve the toughness of polymer A.

[0034] (3) In the present invention, when the ratio of polymer A to reactive polymer B is in the preferred range of (90-99): (20-30), the polymer melt strength can be greatly improved. This is because the molecular chains in the system are entangled with each other in addition to the entanglement between straight chain molecules and the entanglement between long branches. This makes the entire system into a huge entangled network, and the melt strength is greatly improved.

[0035] (4) In addition, the functional additives used will not substantially affect the performance of the high melt strength and high toughness composition. The present invention is easy to implement on conventional polymer material processing equipment and can be directly used for compression molding, foaming, blow molding, and secondary molding to prepare thermoplastic plastic products. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 1-2 is a torque diagram of Example 1-2 and Comparative Example 1-2;

[0037] Figure 2 It is the stress-strain curve diagram of Example 1-2 and Comparative Example 1-2. DETAILED DESCRIPTION

[0038] The embodiments disclosed herein are examples of the present invention, which can be embodied in different forms. Therefore, the disclosed details including specific structural and functional details are not intended to limit the present invention, but are merely the basis of the claims. It should be understood that the detailed description of the present invention is not intended to limit but to cover all possible modifications, equivalents and alternatives falling within the scope of the present invention as defined by the appended claims. The application uses the word "may" in an allowed sense rather than a mandatory sense throughout the text. Similarly, unless otherwise indicated, the words "include", "comprise" and "consist of" mean "including but not limited to". The words "one" or "a" mean "at least one", and the word "multiple" means more than one. When using abbreviations or technical terms, these terms represent the generally accepted meanings known in the technical field.

[0039] The purification involved in the present invention refers to: completely dissolving the solid sample obtained after grafting with chloroform, and precipitating it in methanol (the volume ratio of chloroform to methanol is 1:5).

[0040] The mass fraction A of the active epoxy group in the reactive polymer B of the present invention is the peak area ratio of the characteristic groups of the nuclear magnetic hydrogen spectrum of the purified sample according to the formula A=M 1 I 1 / M 2 I 2 Calculated, where I 1 is the characteristic peak area of ​​any hydrogen on the active group (epoxy group), M 1 is the relative molecular mass of the active group, I 2 is the characteristic peak area of ​​hydrogen on the α-carbon (ortho position of ester group) in flexible polyester, M 2 is the relative molecular mass of the flexible polyester monomer unit; the mass fraction of the active anhydride and isocyanate groups in the reactive polymer B involved is A is the peak area ratio of the characteristic groups of the NMR carbon spectrum of the purified sample according to the formula A=M' 1 I' 1 / M' 2 I' 2 Calculated, where I' 1 M' is the NMR characteristic peak area of ​​the carbonyl characteristic carbon in the active group (isocyanate / anhydride), 1 is the relative molecular mass of the active group, I' 2M' is the NMR characteristic peak area of ​​the carbon on the α-carbon (ortho to the ester group) in the flexible polyester. 2 is the relative molecular mass of the flexible polyester monomer unit.

[0041] Example 1

[0042] (1) Preparation of reactive polymer B

[0043] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0044] (2) Preparation of high melt strength and high toughness composition

[0045] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0046] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0047] Example 2

[0048] (1) Preparation of reactive polymer B

[0049] The glycidyl methacrylate in Example 1 was replaced with cardanol glycidyl ether, and a reactive polymer B (mass fraction of epoxy groups was 10%) was prepared by the same method, which was recorded as SEPCL.

[0050] (2) Preparation of high melt strength and high toughness composition

[0051] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SEPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0052] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0053] Example 3

[0054] (1) Preparation of reactive polymer B

[0055] The glycidyl methacrylate in Example 1 was replaced by maleic anhydride, and a reactive polymer B (the mass fraction of anhydride groups was 10%) was prepared by the same method, which was recorded as SMPCL.

[0056] (2) Preparation of high melt strength and high toughness composition

[0057] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SCPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0058] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0059] Example 4

[0060] (1) Preparation of reactive polymer B

[0061] The glycidyl methacrylate in Example 1 was replaced by 3-isopropyl-dimethylbenzyl isocyanate, and a reactive polymer B (with a mass fraction of isocyanate groups of 10%) was prepared by the same method, which was recorded as STPCL.

[0062] (2) Preparation of high melt strength and high toughness composition

[0063] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SCPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0064] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0065] Example 5

[0066] (1) Preparation of reactive polymer B

[0067] 50 g of polycaprolactone (Mn=70000), 15 g of glycidyl methacrylate, 5 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 15%) was obtained, which was recorded as SGPCL.

[0068] (2) Preparation of high melt strength and high toughness composition

[0069] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0070] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0071] Example 6

[0072] (1) Preparation of reactive polymer B

[0073] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0074] (2) Preparation of high melt strength and high toughness composition

[0075] 90 g of polylactic acid (Mn=130000) was melt-blended with 15 g of SGPCL and 3 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0076] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0077] Example 7

[0078] (1) Preparation of reactive polymer B

[0079] 50 g of a copolymer of butylene adipate and butylene terephthalate (BSF C1200), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of diisopropylbenzene peroxide were melt-grafted at 170° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (the mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPBAT.

[0080] (2) Preparation of high melt strength and high toughness composition

[0081] 90 g of polylactic acid (Mn=130000), 10 g of SGPBAT and 1 g of a functional additive (antioxidant Irganox1330) were premixed uniformly at room temperature, added to the conveying section of a twin-screw extruder and continuously melt-extruded at 220° C. (50° C. above the melting point) to obtain a high melt strength and high toughness composition.

[0082] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat-plate vulcanizer for tensile testing.

[0083] Example 8

[0084] (1) Preparation of reactive polymer B

[0085] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0086] (2) Preparation of high melt strength and high toughness composition

[0087] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0088] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0089] Example 9

[0090] (1) Preparation of reactive polymer B

[0091] The glycidyl methacrylate in Example 1 was replaced with cardanol glycidyl ether, and a reactive polymer B (mass fraction of epoxy groups was 10%) was prepared by the same method, which was recorded as SEPCL.

[0092] (2) Preparation of high melt strength and high toughness composition

[0093] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0094] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0095] Example 10

[0096] (1) Preparation of reactive polymer B

[0097] The glycidyl methacrylate in Example 1 was replaced by maleic anhydride, and a reactive polymer B (the mass fraction of anhydride groups was 10%) was prepared by the same method, which was recorded as SMPCL.

[0098] (2) Preparation of high melt strength and high toughness composition

[0099] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0100] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0101] Embodiment 11

[0102] (1) Preparation of reactive polymer B

[0103] The glycidyl methacrylate in Example 1 was replaced by 3-isopropyl-dimethylbenzyl isocyanate, and a reactive polymer B (with a mass fraction of isocyanate groups of 10%) was prepared by the same method, which was recorded as STPCL.

[0104] (2) Preparation of high melt strength and high toughness composition

[0105] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0106] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0107] Example 12

[0108] (1) Preparation of reactive polymer B

[0109] 50 g of polycaprolactone (Mn=70000), 15 g of glycidyl methacrylate, 5 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 15%) was obtained, which was recorded as SGPCL.

[0110] (2) Preparation of high melt strength and high toughness composition

[0111] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0112] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0113] Embodiment 13

[0114] (1) Preparation of reactive polymer B

[0115] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0116] (2) Preparation of high melt strength and high toughness composition

[0117] 99 g of polyglycolic acid (Mn=150000) was melt-blended with 5 g of SGPCL and 1 g of a functional aid (antioxidant Irganox 1330) at 240° C. (10° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0118] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0119] Embodiment 14

[0120] (1) Preparation of reactive polymer B

[0121] 50 g of a copolymer of butylene adipate and butylene terephthalate (BSF C1200), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of diisopropylbenzene peroxide were melt-grafted at 170° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (the mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPBAT.

[0122] (2) Preparation of high melt strength and high toughness composition

[0123] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 270° C. (40° C. above the melting point) for 5 minutes to obtain a high melt strength and high toughness composition.

[0124] The extruded composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat-plate vulcanizer for tensile testing.

[0125] Embodiment 15

[0126] (1) Preparation of reactive polymer B

[0127] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0128] (2) Preparation of high melt strength and high toughness composition

[0129] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0130] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0131] Example 16

[0132] (1) Preparation of reactive polymer B

[0133] The glycidyl methacrylate in Example 1 was replaced with cardanol glycidyl ether, and a reactive polymer B (mass fraction of epoxy groups was 10%) was prepared by the same method, which was recorded as SEPCL.

[0134] (2) Preparation of high melt strength and high toughness composition

[0135] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0136] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0137] Embodiment 17

[0138] (1) Preparation of reactive polymer B

[0139] The glycidyl methacrylate in Example 1 was replaced by maleic anhydride, and a reactive polymer B (the mass fraction of anhydride groups was 10%) was prepared by the same method, which was recorded as SMPCL.

[0140] (2) Preparation of high melt strength and high toughness composition

[0141] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0142] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0143] Embodiment 18

[0144] (1) Preparation of reactive polymer B

[0145] The glycidyl methacrylate in Example 1 was replaced by 3-isopropyl-dimethylbenzyl isocyanate, and a reactive polymer B (with a mass fraction of isocyanate groups of 10%) was prepared by the same method, which was recorded as STPCL.

[0146] (2) Preparation of high melt strength and high toughness composition

[0147] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0148] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0149] Embodiment 19

[0150] (1) Preparation of reactive polymer B

[0151] 50 g of polycaprolactone, 15 g of glycidyl methacrylate, 5 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 15%) was obtained, which was recorded as SGPCL.

[0152] (2) Preparation of high melt strength and high toughness composition

[0153] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0154] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0155] Embodiment 20

[0156] (1) Preparation of reactive polymer B

[0157] 50 g of polycaprolactone (Mn=150000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPCL.

[0158] (2) Preparation of high melt strength and high toughness composition

[0159] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 3 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. (5° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0160] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0161] Embodiment 21

[0162] (1) Preparation of reactive polymer B

[0163] 50 g of a copolymer of butylene adipate and butylene terephthalate (BSF C1200), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of diisopropylbenzene peroxide were melt-grafted at 170° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B (the mass fraction of epoxy groups is 10%) was obtained, which was recorded as SGPBAT.

[0164] (2) Preparation of high melt strength and high toughness composition

[0165] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPBAT and 2 g of a functional aid (antioxidant Irganox 1330) at 270° C. (30° C. above the melting point) for 15 minutes to obtain a high melt strength and high toughness composition.

[0166] The above blended composition is fully dried and then subjected to a melt flow test using a melt flow tester, and is hot-pressed by a flat vulcanizer for tensile testing.

[0167] Comparative Example 1

[0168] 100 g of polylactic acid (Mn=130000) and 1 g of a functional aid (antioxidant Irganox 1330) were melt-blended at 190° C. for 10 minutes to obtain a composition.

[0169] Comparative Example 2

[0170] 95 g of polylactic acid (Mn=130000) was melt-blended with 7.13 g of polycaprolactone, 1.43 g of glycidyl methacrylate, 1.43 g of styrene, 0.03 g of benzoyl peroxide and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. for 10 minutes in one step to obtain a composition.

[0171] Comparative Example 3

[0172] (1) Preparation of polymer B

[0173] 50 g of polycaprolactone (Mn=70000), 0.05 g of glycidyl methacrylate, 10 g of styrene, and 0.1 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a polymer B (mass fraction of epoxy group is 0.05%) was obtained, which was recorded as SGPCL.

[0174] (2) Preparation of composition

[0175] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. for 10 minutes to obtain a composition.

[0176] Comparative Example 4

[0177] 100 g of polyglycolic acid (Mn=150000) and 1 g of a functional aid (antioxidant Irganox 1330) were melt-blended at 240° C. for 10 minutes to obtain a composition.

[0178] Comparative Example 5

[0179] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 7.13 g of polycaprolactone, 1.43 g of glycidyl methacrylate, 1.43 g of styrene, 0.03 g of benzoyl peroxide and 1 g of a functional aid (antioxidant Irganox 1330) at 240° C. for 10 minutes in one step to obtain a composition.

[0180] Comparative Example 6

[0181] (1) Preparation of polymer B

[0182] 50 g of polycaprolactone (Mn=70000), 0.05 g of glycidyl methacrylate, 10 g of styrene, and 0.1 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a polymer B (mass fraction of epoxy group is 0.05%) was obtained, which was recorded as SGPCL.

[0183] (2) Preparation of composition

[0184] 95 g of polyglycolic acid (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 240° C. for 10 minutes to obtain a composition.

[0185] Comparative Example 7

[0186] 100 g of polyethylene terephthalate (Mn=150000) and 1 g of a functional aid (antioxidant Irganox 1330) were melt-blended at 255° C. for 10 minutes to obtain a composition.

[0187] Comparative Example 8

[0188] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 7.13 g of polycaprolactone, 1.43 g of glycidyl methacrylate, 1.43 g of styrene, 0.03 g of benzoyl peroxide and 1 g of a functional aid (antioxidant Irganox 1330) at 255° C. for 10 minutes in one step to obtain a composition.

[0189] Comparative Example 9

[0190] (1) Preparation of polymer B

[0191] 50 g of polycaprolactone (Mn=70000), 0.05 g of glycidyl methacrylate, 10 g of styrene, and 0.1 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a polymer B (mass fraction of epoxy group is 0.05%) was obtained, which was recorded as SGPCL.

[0192] (2) Preparation of composition

[0193] 95 g of polyethylene terephthalate (Mn=150000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 255° C. for 10 minutes to obtain a composition.

[0194] It should be noted that the polyesters used in the above various examples and comparative examples were vacuum dried at 60° C. for 12 hours before use. The mass fraction of the acid anhydride, epoxy group and isocyanate in the reactive polymer B prepared in the example is 0.1 to 30%.

[0195] The polylactic acid compositions in Examples 1-7 and Comparative Examples 1-3 were subjected to a melt flow rate test using a melt flow rate tester, kept at 190° C. for 5 minutes, and then the melt flow rate was measured under the conditions of 190° C. and 2.16 kg.

[0196] The polyglycolic acid compositions in Examples 8-14 and Comparative Examples 4-6 were subjected to melt flow rate testing using a melt flow rate tester. The compositions were kept at 230° C. for 5 minutes, and the melt flow rates were then measured at 230° C. and 2.16 kg.

[0197] The polyethylene terephthalate compositions in Examples 15-21 and Comparative Examples 7-9 were subjected to melt flow rate testing using a melt flow rate tester. The compositions were kept at 260° C. for 5 minutes, and the melt flow rates were then measured at 260° C. and 2.16 kg.

[0198] The melt strength (MS) of the compositions obtained in Examples 1-21 and Comparative Examples 1-9 was calculated by formula (1):

[0199]

[0200] Where: ΔL—the length when the melt extrusion diameter is reduced to half;

[0201] r 0 —The radius of the initial extrusion from the extruder die;

[0202] MFR—melt flow rate, g / 10min.

[0203] The compositions obtained in Examples 1-21 and Comparative Examples 1-9 were tested for tensile strength and elongation at break using a universal testing machine according to GB / T 1040.1-2018 at a tensile rate of 10 mm / min.

[0204] The melt flow rate, melt strength, tensile strength and elongation at break of the tested embodiments and comparative examples are shown in Table 1.

[0205] Table 1 Melt flow rate, melt strength, tensile strength and elongation at break of each embodiment and comparative example

[0206]

[0207]

[0208] From Examples 1-7 and Comparative Examples 1-3, it can be seen that the method of using glycidyl methacrylate, cardanol glycidyl ether, maleic anhydride, 3-isopropyl-dimethylbenzyl isocyanate as active monomers to modify polycaprolactone or butylene adipate and butylene terephthalate and then melt blending with polylactic acid can increase the viscosity of the system, reduce the melt index from 21 to about 7, but still maintain good melt fluidity (i.e., melt processing performance); at the same time, improve the melt strength of polylactic acid, increase the melt strength from 233Pa·s to more than 4000Pa·s, an increase of nearly 20 times; have no significant effect on tensile strength, but significantly increase the elongation at break by more than 30 times. There are similar final effects at different processing temperatures.

[0209] It can be seen from Examples 8-14 and Comparative Examples 4-6 that the method of using glycidyl methacrylate, cardanol glycidyl ether, maleic anhydride, 3-isopropyl-dimethylbenzyl isocyanate as active monomers to modify polycaprolactone or butylene adipate and butylene terephthalate and then melt blending with polyglycolic acid can increase the viscosity of the system, reducing the melt index from 12.8 to about 5, but still maintaining good melt fluidity; at the same time, the melt strength of polyglycolic acid is increased from 145Pa·s to more than 7000Pa·s, which is nearly 50 times higher; it has no significant effect on tensile strength, but significantly increases the elongation at break by more than 20 times. And there are similar final effects at different processing temperatures.

[0210] It can be seen from Examples 9 and 10 and Comparative Example 3 that the method of using glycidyl methacrylate, cardanol glycidyl ether, maleic anhydride, and 3-isopropyl-dimethylbenzyl isocyanate as active monomers to modify polycaprolactone or butylene adipate and butylene terephthalate and then melt blending with polyethylene terephthalate can increase the viscosity of the system, reduce the melt index from 15.3 to about 6, but still maintain good melt fluidity; at the same time, improve the melt strength of polyethylene terephthalate, increase the melt strength from 879Pa·s to about 10000Pa·s, which is nearly 11 times; have no significant effect on tensile strength, but significantly increase the elongation at break by more than 5 times. And there are similar final effects at different processing temperatures.

[0211] Embodiment 22

[0212] (1) Preparation of polymer B

[0213] 50 g of polycaprolactone (as shown in Table 2) was melt-grafted with different amounts of glycidyl methacrylate, 10 g of styrene, and 0.1 g of benzoyl peroxide at 130° C. to obtain solid samples. After the solid samples were purified, a polymer B was obtained, which was recorded as SGPCL.

[0214] (2) Preparation of composition

[0215] 95 g of polylactic acid (Mn=130000) was melt-blended with 10 g of SGPCL and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. for 10 minutes to obtain a composition.

[0216] The melt flow rate, melt strength, tensile strength and elongation at break of the test compositions are shown in Table 2. Table 2 Melt flow rate, melt strength, tensile strength and elongation at break of compositions obtained with different amounts of glycidyl methacrylate

[0217]

[0218] When the amount of epoxy monomer used is too high, the grafting rate in the system is reduced, gel is easily generated (ie, cross-linking), which reduces the processing performance and makes it difficult to carry out purification and subsequent steps.

[0219] Embodiment 23

[0220] (1) Preparation of reactive polymer B

[0221] 50 g of polycaprolactone (Mn=70000), 10 g of glycidyl methacrylate, 10 g of styrene, and 0.2 g of benzoyl peroxide were melt-grafted at 130° C. to obtain a solid sample. After purifying the solid sample, a reactive polymer B was obtained, which was recorded as SGPCL.

[0222] (2) Preparation of high melt strength and high toughness composition

[0223] 95 g of polylactic acid (Mn=130000) was melt blended with a certain amount of SGPCL (shown in Table 3) and 2 g of a functional aid (antioxidant Irganox 1330) at 190° C. (20° C. above the melting point) for 10 minutes to obtain a high melt strength and high toughness composition.

[0224] The above blended composition was fully dried and then subjected to a melt flow test using a melt flow tester, and was hot-pressed by a flat vulcanizer for tensile testing. The results are shown in Table 2.

[0225] Table 3 Melt flow rate, melt strength, tensile strength and elongation at break of the compositions obtained with different amounts of SGPCL

[0226]

[0227] The above examples demonstrate that the present invention can obtain a composition with high melt strength, high toughness and good processing performance. The composition provided by the present invention not only has high melt strength but also has excellent toughness, and can be directly used for compression molding, foaming, blow molding, and secondary molding to prepare thermoplastic plastic products.

[0228] Those skilled in the art should understand that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the melt strength and toughness of a polymer, the method comprising mixing a reactive polymer B with a polymer A, melt blending or melt extruding; wherein: The reactive polymer B contains both a flexible polyester main chain and a side chain with an active group; the active group includes at least one of an epoxy group and an isocyanate; the polymer A is at least one of polyglycolic acid, a glycolic acid-based copolymer, polylactic acid, a lactic acid-based copolymer, and polyethylene terephthalate; The flexible polyester main chain of the reactive polymer B is polymerized from at least one monomer selected from the group consisting of caprolactone, glycolide, adipic acid, terephthalic acid, succinic acid and butanediol; The reactive polymer B is prepared by melt grafting a flexible polyester with a monomer C under the action of a free radical initiator; the monomer C contains a -C=C- double bond and an active group, which is selected from at least one of cardanol glycidyl ether and 3-isopropyl-dimethylbenzyl isocyanate; The mass fraction of active groups in the reactive polymer B is 5%-25%.

2. The method according to claim 1, characterized in that According to the weight ratio, polymer A is 85-99 parts and reactive polymer B is 1-30 parts.

3. The method according to claim 1, characterized in that The method further comprises adding 0.1 to 3 parts by weight of a functional additive; the functional additive comprises at least one of an antistatic agent, an antioxidant, an anti-aging agent, an anti-hydrolysis agent and a filler.

4. A composition with high melt strength and toughness, characterized in that: The invention comprises, by weight: 85-99 parts of polymer A, 1-30 parts of reactive polymer B, and 0.1-3 parts of functional additives; wherein the reactive polymer B comprises a flexible polyester main chain and a side chain having an active group; the active group comprises at least one of an epoxy group and an isocyanate; the polymer A is at least one of polyglycolic acid, a glycolic acid-based copolymer, polylactic acid, a lactic acid-based copolymer, and polyethylene terephthalate; The flexible polyester main chain of the reactive polymer B is polymerized from at least one monomer selected from the group consisting of caprolactone, glycolide, adipic acid, terephthalic acid, succinic acid and butanediol; The reactive polymer B is prepared by melt grafting a flexible polyester with a monomer C under the action of a free radical initiator; the monomer C contains a -C=C- double bond and an active group, and is selected from at least one of cardanol glycidyl ether and 3-isopropyl-dimethylbenzyl isocyanate; The mass fraction of active groups in the reactive polymer B is 5%-25%.

5. The composition according to claim 4, characterized in that The preparation method of the composition comprises: Method 1: Premix polymer A, reactive polymer B and functional additives at room temperature according to weight ratio, add them into internal mixer for melt blending, and obtain a high melt strength and high toughness composition; Or method 2, polymer A, reactive polymer B and functional additives are premixed uniformly at room temperature according to weight ratio, added into the conveying section of a twin-screw extruder, and subjected to continuous melt extrusion to obtain a high melt strength and high toughness composition.

6. Use of the composition according to claim 4 or 5 in compression molding, foaming, blow molding, and secondary molding to prepare thermoplastic plastic products.